A thermosensitive sensing material and a wide-temperature-range Fe-doped manganese-based thermosensitive sensor and a preparation method thereof
By fabricating an Fe-doped manganese-based thermistor, the problem of insufficient accuracy of existing sensors in a wide temperature range was solved, achieving high-precision and low-energy-consumption temperature monitoring.
Patent Information
- Application Number
- CN202411812618.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-10
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-12-10
AI Technical Summary
Existing thermistors have insufficient accuracy and poor linearity in a wide temperature range of -20℃ to 60℃, which cannot meet the temperature monitoring requirements of high-precision equipment.
A high-precision, wide-temperature-range Fe-doped manganese-based thermistor sensor was fabricated by mixing Fe, Ni, Co, and Mn oxides in a specific ratio, combined with ball milling, sintering, mixing, and pressing processes.
It achieves high-precision temperature monitoring within the range of -20℃ to 60℃, has a high thermistor constant B value, low room temperature resistance, low energy consumption, good adaptability, and a simple and low-cost preparation process.
Smart Images

Figure CN119613098B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to manganese-based thermistor materials, specifically to a thermistor material and a wide-temperature-range Fe-doped manganese-based thermistor sensor and its preparation method. Background Technology
[0002] The large diurnal temperature range in high-altitude regions makes it easy for equipment to experience performance degradation and abnormal protective system operation due to abnormal storage microenvironment temperatures during long-term operation. Therefore, temperature monitoring of the equipment storage microenvironment is crucial for ensuring stable and reliable equipment performance, especially for precision electronic instruments, which have stringent requirements for storage microenvironment conditions. For example, the transport packaging of a certain type of product has specific requirements for microenvironment temperature; when the external ambient temperature is between -15℃ and +50℃, real-time and accurate monitoring of the microenvironment temperature is necessary.
[0003] Currently, traditional thermistors often fail to meet the demand for accurate temperature monitoring in a wide temperature range of -20℃ to 60℃. Most existing manganese-based thermistors have a temperature measurement range above room temperature. Therefore, the development of high-precision, wide-temperature-range thermistors is crucial. Traditional thermistors in this wide temperature range often suffer from large accuracy fluctuations, poor linearity, or poor long-term stability. For example, a commonly used thermistor experiences a significant decrease in sensitivity at low temperatures, leading to increased measurement errors; while some sensors are prone to performance drift near high-temperature boundaries, failing to meet the requirements for long-term accurate monitoring. Therefore, developing a thermistor specifically designed for this temperature range (-20℃ to 60℃) and possessing high-precision characteristics is essential. Summary of the Invention
[0004] This invention provides a thermistor material and a wide-temperature-range Fe-doped manganese-based thermistor sensor and its preparation method, aiming to solve the problems of insufficient accuracy and poor temperature range adaptability of existing thermistors in a specific low-temperature range (-20℃~60℃), and to provide reliable sensing technology support for many devices that require accurate temperature monitoring in this temperature range.
[0005] The present invention adopts the following technical solution.
[0006] A thermal sensing material with the chemical formula Fe x Ni 0.3 Co 0.9 Mn 1.8-x O4, x = 0.5~0.8. Preferably, the chemical formula of the thermal sensing material is Fe. 0.6 Ni 0.3 Co 0.9 Mn 1.2 O4.
[0007] A method for fabricating a wide-temperature-range Fe-doped manganese-based thermistor, comprising the following steps: Step 1: Weigh the raw materials MnCO3, NiO, Co3O4, and Fe3O4, and then ball-mill, vacuum filter, and dry them to obtain powder. Step 2: Sinter the obtained powder material, and then ball mill the sintered material a second time to obtain the active powder for the thermal sensor. Step 3: Mix the obtained thermistor active powder with polyvinyl alcohol aqueous solution, dry the mixture after it is evenly mixed, grind and sieve it to obtain the mixed thermistor active powder; then compress the obtained thermistor active powder into a tablet to obtain the thermistor preform. Step 4: The obtained thermistor blank is sintered a second time, and then a silver electrode is coated to obtain a wide-temperature-range Fe-doped manganese-based thermistor.
[0008] Preferably, the raw materials are weighed according to the amount of each element, and the weighed raw materials satisfy the condition "Fe x Ni 0.3 Co 0.9 Mn 1.8-x04 The required doping ratio is "(x=0.5~0.7)".
[0009] Preferably, the raw materials are weighed according to the amount of each element, and the weighed raw materials satisfy the condition "Fe x Ni 0.3 Co 0.9 Mn 1.8-x04 The doping ratio requirement is "(x=0.6)".
[0010] Preferably, in step 1, ultrapure water is used as a dispersant, and the ball-to-material ratio is controlled to be 2:1.
[0011] Preferably, the sintering method in step 2 is as follows: first, heat the temperature to 200°C at a rate of 5°C / min and hold it for one hour, then heat the temperature to 900°C at a rate of 5°C / min, sinter for 3 hours, and then cool it to room temperature.
[0012] Preferably, the tablet compression in step 3 requires holding the pressure for at least 90 seconds.
[0013] Preferably, the secondary sintering method in step 4 is as follows: first, the temperature is raised to 600°C at a rate of 2°C / min and held for 2 hours, then the temperature is raised to 1150°C at a rate of 5°C / min, sintered for 3 hours, and then cooled to room temperature.
[0014] In this invention, during the sintering process in step 2, the active material crystal of the thermal sensor is formed.
[0015] Beneficial effects: The thermal sensing material and wide-temperature-range Fe-doped manganese-based thermal sensor provided by this invention have the advantages of high precision when used in a specific medium and low temperature range (-20℃~60℃), and good temperature range adaptability. Its thermistor constant B value, a key indicator of reaction sensitivity, reaches as high as 3839.59. It also has the advantages of low room temperature resistance and low energy consumption. Attached Figure Description
[0016] Figure 1 The resistance-temperature test results are for the wide-temperature-range Fe-doped manganese-based thermistor in Example 1. Figure 2 The room temperature resistance r25 of the wide-temperature-range Fe-doped manganese-based thermistor in Example 1 is measured. Figure 3 The material constant B value of the wide-temperature-range Fe-doped manganese-based thermistor in Example 1 is the test result. Detailed Implementation
[0017] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1
[0018] A Fe-doped manganese-based thermistor, with the chemical formula Fe 0.6 Ni 0.3 Co 0.9 Mn 1.2 The preparation method of O4, a wide-temperature-range Fe-doped manganese-based thermistor, includes the following steps: Step 1: Weigh the raw materials MnCO3, NiO, Co3O4, and Fe3O4 (weighed according to the amount of each element; the masses of MnCO3, NiO, Co3O4, and Fe3O4 are 9.55g, 1.55g, 5g, and 3.21g, respectively). After drying the weighed raw materials in a vacuum drying oven, perform high-energy ball milling using a planetary ball mill. During the ball milling process, use ultrapure water as a dispersant and control the ball-to-material ratio of zirconia balls to raw materials in the ball mill to be 2:1. After ball milling, use a sieve to filter out the grinding beads, and use vacuum filtration to filter out the finely ground powder and dry it. Step 2: Sinter the obtained powder material, and then ball mill the sintered material a second time to obtain the active powder for the thermal sensor; specifically: first, heat the material to 200°C at a rate of 5°C / min and hold it for one hour, then heat it to 900°C at a rate of 5°C / min, sinter for 3 hours, and then cool it to room temperature. During this process, the active material crystals of the thermal sensor are formed. After sintering, a second ball mill is performed (the second ball milling method is the same as the ball milling method in Step 1) to obtain fine active powder for the thermal sensor. Step 3: Mix the obtained thermistor active powder with 6wt% polyvinyl alcohol aqueous solution. The mixing amount is 2ml of polyvinyl alcohol aqueous solution for every 3g of active powder. After mixing evenly, dry, grind and sieve to obtain the mixed thermistor active powder. Then, compress the obtained thermistor active powder into tablets (control the pressure of the tablet press to 15Mpa and the holding time to two minutes) to obtain the thermistor preform. Step 4: The obtained thermistor blank is subjected to secondary sintering (first, the temperature is raised to 600℃ at a rate of 2℃ / min and held for 2 hours, then the temperature is raised to 1150℃ at a rate of 5℃ / min and sintered for 3 hours before being cooled to room temperature). After the sintering is completed, a silver electrode is coated and wires are led out to obtain a wide-temperature-range Fe-doped manganese-based thermistor. Example 2
[0019] A Fe-doped manganese-based thermistor, with the chemical formula Fe 0.5 Ni 0.3 Co 0.9 Mn 1.3 The preparation method of this wide-temperature-range Fe-doped manganese-based thermistor is the same as in Example 1. Example 3
[0020] A Fe-doped manganese-based thermistor, with the chemical formula Fe 0.7 Ni 0.3 Co 0.9 Mn 1.1 The preparation method of this wide-temperature-range Fe-doped manganese-based thermistor is the same as in Example 1. Example 4
[0021] A Fe-doped manganese-based thermistor, with the chemical formula Fe 0.8 Ni 0.3 Co 0.9 The preparation method of this wide-temperature-range Fe-doped manganese-based thermistor is the same as in Example 1.
[0022] The performance of the Fe-doped manganese-based thermistors obtained in each embodiment was tested. A total of 4 groups of samples (two samples in each group) were selected. The sensor samples prepared in Example 1 were numbered A2-1 and A2-2, the sensor samples prepared in Example 2 were numbered A1-1 and A1-2, the sensor samples prepared in Example 3 were numbered A3-1 and A3-2, and the sensor samples prepared in Example 4 were numbered A4-1 and A4-2.
[0023] Four sets of prepared samples were tested using a temperature and humidity chamber and a resistance meter, with a test temperature range of -20℃ to 60℃. The resistance-temperature test results are shown below. Figure 1 The room temperature resistance R25 test results are shown in [link to test results]. Figure 2 The test results for the material constant B value are shown in [link to test results]. Figure 3 .
[0024] After analyzing the performance test results of the four groups of samples, it was found that the A2 group of samples (i.e. the Fe-doped manganese-based thermistor prepared in Example 1) had the most ideal comprehensive performance. The test results of the two samples in the A2 group had a high degree of fit and reached a high value of 3839.59 in the thermistor constant B, a key indicator of reaction sensitivity. It also had a low room temperature resistance and low energy consumption.
[0025] This invention utilizes four groups of active materials with specific Fe doping ratios and a specific preparation process to produce a thermistor and a wide-temperature-range Fe-doped manganese-based thermistor. These materials offer high precision in a specific low-temperature range (-20℃ to 60℃), good temperature adaptability, and advantages such as simple preparation process, good controllability, and low manufacturing cost.
Claims
1. A thermal sensing material, characterized in that: Its chemical formula is Fe 0.6 Ni 0.3 Co 0.9 Mn 1.2 O4.
2. A method for fabricating a wide-temperature-range Fe-doped manganese-based thermistor, characterized in that the steps include... include: Step 1: Weigh the raw materials MnCO3, NiO, Co3O4, and Fe3O4. Ball mill, vacuum filter, and dry the raw materials to obtain powder. Weigh the raw materials according to the molar amounts of each element, ensuring that the weighed raw materials satisfy the condition "Fe...". 0.6 Ni 0.3 Co 0.9 Mn 1.2 The required doping ratio is "O4"; Step 2: Sinter the obtained powder material, and then ball mill the sintered material a second time to obtain the active powder for the thermal sensor. Step 3: Mix the obtained thermistor active powder with polyvinyl alcohol aqueous solution, dry the mixture after it is evenly mixed, grind and sieve it to obtain the mixed thermistor active powder; then compress the obtained thermistor active powder into a tablet to obtain the thermistor preform. Step 4: The obtained thermistor blank is sintered a second time, and then a silver electrode is coated to obtain a wide-temperature-range Fe-doped manganese-based thermistor.
3. The preparation method according to claim 2, characterized in that: In step 1, ultrapure water is used as a dispersant, and the ball-to-material ratio of zirconia pellets to raw materials in the ball mill is controlled to be 2:
1.
4. The preparation method according to claim 2, characterized in that, The sintering method in step 2 is as follows: first, heat the temperature to 200℃ at a rate of 5℃ / min and hold it for one hour, then heat the temperature to 900℃ at a rate of 5℃ / min, sinter for 3 hours, and then cool it to room temperature.
5. The preparation method according to claim 2, characterized in that, In step 3, the tablets need to be compressed for at least 90 seconds.
6. The preparation method according to claim 2, characterized in that, The secondary sintering method in step 4 is as follows: first, heat the temperature to 600℃ at a rate of 2℃ / min and hold for 2 hours, then heat the temperature to 1150℃ at a rate of 5℃ / min, sinter for 3 hours, and then cool to room temperature.
7. The preparation method according to any one of claims 2-6, characterized in that: During the sintering process in step 2, the active material crystals of the thermistor are formed.