A silicon-containing coating and a method for preparing the same, and a modified nylon material and a method for preparing and using the same

By coating nylon fibers with a silicon-containing coating to form a modified nylon material, the problem of difficult removal of release cloth is solved, achieving good release effect and improved production efficiency, while reducing energy consumption and costs.

CN119614078BActive Publication Date: 2026-11-24JIANGSU AIHE COMPOSITE MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411823841.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-11
Publication Date
2026-11-24
Estimated Expiration
2044-12-11

AI Technical Summary

Technical Problem

Existing release fabrics are difficult to remove easily from the surface of composite products while ensuring release effect, and high polarity materials can easily cause fiber cloth to break or remain, affecting production efficiency.

Method used

Modified nylon materials using silicon-containing coatings are formed by combining hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, methylphenylvinylpolysiloxane, anchoring agents, platinum catalysts, and inhibitors to form a coating, which is then applied to nylon fibers to form modified nylon materials with good demolding effect and easy removal.

Benefits of technology

Modified nylon materials are cured and molded at low temperatures, reducing energy consumption, avoiding high-temperature thermal shrinkage, providing good demolding effect, preserving fiber texture, improving production efficiency, and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119614078B_ABST
    Figure CN119614078B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of composite material molding technology, specifically relating to a silicon-containing coating and its preparation method, as well as a modified nylon material, its preparation method, and its application. This invention uses a low-molecular-weight polysiloxane, enabling the product to be cured at low temperatures, reducing energy consumption during production and avoiding the thermal shrinkage of nylon fibers under high-temperature processes. The silicon-containing coating provided by this invention not only cures at low temperatures but also withstands higher temperatures, with readily available raw materials and controllable costs. The modified nylon material provided by this invention utilizes the silicon-containing coating to improve the surface polarity of nylon fibers. The resulting modified nylon material not only has good thermal stability and does not exhibit silicon migration but is also easy to remove from the surface of composite material products after use, leaving a fiber cloth texture on the product surface, reducing post-processing time and improving the production efficiency of composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite material molding technology, specifically relating to a silicon-containing coating and its preparation method, as well as a modified nylon material, its preparation method, and its application. Background Technology

[0002] Currently, the molding of resin-based composite materials mainly utilizes vacuum flow technology, drying tunnel technology, and autoclave molding technology. In the implementation of these processes, a release cloth is required to separate the resin from other auxiliary materials. After the resin has cured and formed, the release cloth is removed to obtain the composite material product.

[0003] In terms of material, release fabrics can be categorized into polyester release fabrics, nylon release fabrics, and PTFE release fabrics. While PTFE release fabrics offer good release performance, their smooth surface necessitates grinding and other treatments before subsequent processing. Polyester and nylon release fabrics, although leaving fiber textures on the composite material surface and reducing post-processing time, suffer from high surface polarity, making them difficult to release. If the resin content is high and the oxidizing properties are strong, forced peeling can easily lead to fiber breakage, leaving a large amount of residue on the resin surface that is difficult to clean.

[0004] In summary, existing release fabrics cannot guarantee effective release while making them easy to remove from the surface of composite material products. Summary of the Invention

[0005] The purpose of this invention is to provide a silicon-containing coating and its preparation method, as well as a modified nylon material and its preparation method and application. The modified nylon material modified by the silicon-containing coating provided by this invention has good demolding effect and is easy to remove from the surface of composite material products after use.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] This invention provides a silicone-containing coating, comprising the following raw materials in parts by weight: 5-20 parts of hexamethylcyclotrisiloxane, 5-20 parts of octamethylcyclotetrasiloxane, 5-15 parts of methylphenylvinyl polysiloxane, 0.5-5 parts of anchoring agent, 0.5-5 parts of platinum catalyst, 0.1-0.5 parts of inhibitor, and 100-500 parts of toluene; wherein the methylphenylvinyl polysiloxane has a viscosity of 10,000-50,000 mPa·s at 25°C.

[0008] Preferably, the vinyl chain ratio of the methylphenyl vinyl polysiloxane is 0.4%, and the phenyl chain ratio is 10-30%.

[0009] Preferably, the anchoring agent is a silane-based anchoring agent; the silane-based anchoring agent includes one or more of γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0010] Preferably, the inhibitor is a hydroxyl-containing inhibitor.

[0011] The present invention also provides a method for preparing the silicon-containing coating described above, comprising the following steps:

[0012] A premixed solution was prepared by premixing hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, methylphenylvinylpolysiloxane, anchoring agent, inhibitor and toluene; the premixed solution was then mixed with a platinum catalyst to obtain the silicon-containing coating.

[0013] The present invention also provides a modified nylon material, comprising nylon fibers and a silicon-containing coating covering the surface of the nylon fibers; the silicon-containing coating is formed by the silicon-containing coating described in the above-described scheme or the silicon-containing coating obtained by the preparation method described in the above-described scheme.

[0014] Preferably, the weight ratio of the silicon-containing coating to the nylon fiber is 1:10 to 150.

[0015] The present invention also provides a method for preparing the modified nylon material described above, comprising the following steps:

[0016] The modified nylon material is obtained by coating the surface of nylon fibers with a silicon-containing coating, drying and curing it.

[0017] Preferably, the curing temperature is 90–150°C, and the curing time is 30–120 seconds.

[0018] The present invention also provides the application of the modified nylon material described in the above-described scheme or the modified nylon material obtained by the preparation method described in the above-described scheme as a release fabric.

[0019] This invention provides a silicon-containing coating. The silicon-containing coating provided by this invention is used to prepare modified nylon materials, improving the surface polarity of nylon fibers. The resulting modified nylon material not only has good thermal stability and no silicon migration, but also good demolding effect. Furthermore, it is easy to remove from the surface of composite material products after use, leaving the fiber cloth texture on the product surface, reducing post-processing time and improving the production efficiency of composite materials.

[0020] Furthermore, this invention utilizes polysiloxanes with relatively low molecular weight, enabling the product to be cured and molded at low temperatures. This reduces energy consumption during production and avoids the thermal shrinkage of nylon fibers during high-temperature processes. The silicone-containing coating provided by this invention not only cures at low temperatures but can also withstand higher temperatures, with readily available raw materials and controllable costs.

[0021] This invention also provides a method for preparing the silicon-containing coating described above. The preparation method provided by this invention is simple in steps, convenient in operation, and low in cost.

[0022] This invention also provides a modified nylon material. The modified nylon material provided by this invention utilizes a silicon-containing coating to improve the surface polarity of the nylon fibers. The resulting modified nylon material not only exhibits good thermal stability and no silicon migration, but also has good demolding performance. Furthermore, it is easy to remove from the surface of composite material products after use, leaving the fiber cloth texture on the product surface, reducing post-processing time and improving the production efficiency of composite materials.

[0023] This invention also provides a method for preparing the modified nylon material described above. The preparation method provided by this invention can adjust the silicon-containing coating content of the nylon fibers by controlling the dipping time, ensuring that the modified nylon material is easily removed from the surface of the composite material product after use, and leaving the texture of the nylon fiber cloth on the product surface, thus reducing the time required for post-processing.

[0024] This invention also provides the application of the modified nylon material described in the above-described scheme or the modified nylon material obtained by the preparation method described in the above-described scheme as a release cloth. The modified nylon material provided by this invention has good release effect and leaves the fiber cloth texture on the surface of the product, making it suitable for use as a release cloth in fields such as composite material molding. Attached Figure Description

[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 Scanning electron microscope images of nylon fiber cloth and the modified nylon materials of Examples 3 and 5;

[0027] Figure 2 Water droplet contact angle diagrams for nylon fiber cloth, modified nylon materials of Examples 1 and 3-6;

[0028] Figure 3 Photoelectron spectra of nylon fiber cloth and the modified nylon materials of Examples 1, 3 and 5;

[0029] Figure 4 The images show the actual application of the modified nylon material autoclaves in Examples 1 and 3-6. Detailed Implementation

[0030] This invention provides a silicon-containing coating, which is made from the following raw materials in parts by weight: 5-20 parts of hexamethylcyclotrisiloxane, 5-20 parts of octamethylcyclotetrasiloxane, 5-15 parts of methylphenylvinylpolysiloxane, 0.5-5 parts of anchoring agent, 0.5-5 parts of platinum catalyst, 0.1-0.5 parts of inhibitor, and 100-500 parts of toluene.

[0031] The raw materials for the silicon-containing coating provided by this invention include 5 to 20 parts of hexamethylcyclotrisiloxane (D3), specifically 7, 9, 11, 13, 15, 17, or 19 parts. This invention uses hexamethylcyclotrisiloxane as one of the main raw materials for the reaction.

[0032] The raw materials for the silicon-containing coating provided by this invention include 5 to 20 parts of octamethylcyclotetrasiloxane (D4), specifically 7, 9, 11, 13, 15, 17, or 19 parts. This invention uses octamethylcyclotetrasiloxane as one of the main raw materials for the reaction.

[0033] The raw materials for the silicone-containing coating provided by this invention include 5 to 15 parts of methylphenylvinyl polysiloxane, specifically 7, 9, 11, or 13 parts. This invention uses methylphenylvinyl polysiloxane as one of the main raw materials for the reaction.

[0034] In this invention, the viscosity of the methylphenyl vinyl polysiloxane at 25°C is 10,000 to 50,000 mPa·s, specifically 15,000 mPa·s, 20,000 mPa·s, 25,000 mPa·s, 30,000 mPa·s, 35,000 mPa·s, 40,000 mPa·s, or 45,000 mPa·s. The vinyl chain ratio is preferably 0.4%, and the phenyl chain ratio is preferably 10 to 30%, specifically 15%, 20%, or 25%.

[0035] The raw materials for the silicone-containing coating provided by this invention include 0.5 to 5 parts of an anchoring agent, specifically 0.7, 0.9, 1.2, 1.5, 1.8, 2, 2.5, 3, 3.5, 4, or 4.5 parts. This invention improves the adhesion between the silicone-containing coating and the nylon fiber cloth through an adhesion promoter.

[0036] In this invention, the anchoring agent is preferably a silane-based anchoring agent; the silane-based anchoring agent preferably includes one or more of γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0037] The raw materials for the silicon-containing coating provided by the present invention include 0.5 to 5 parts of platinum catalyst, specifically 0.7 parts, 0.9 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts or 4.8 parts.

[0038] In this invention, the platinum catalyst is preferably a platinum / olefin siloxane coordination compound; the effective content of the platinum catalyst is preferably 10,000 ppm.

[0039] The raw materials for the silicon-containing coating provided by this invention include 0.1 to 0.5 parts of an inhibitor, specifically 0.2, 0.3, or 0.4 parts. This invention uses the inhibitor primarily to slow down the reaction rate and prevent explosive polymerization.

[0040] In this invention, the inhibitor is preferably a hydroxyl-containing inhibitor; the hydroxyl-containing inhibitor is preferably an unsaturated alcohol; and the unsaturated alcohol is preferably 2-methyl-3-butyn-2-ol.

[0041] The raw materials for the silicone-containing coating provided by this invention include 100 to 500 parts of toluene, specifically 120 parts, 150 parts, 170 parts, 200 parts, 240 parts, 270 parts, 300 parts, 350 parts, 400 parts, or 450 parts. This invention uses toluene as a solvent to dilute the coating, thereby adjusting the application amount of the silicone-containing coating.

[0042] The present invention also provides a method for preparing the silicon-containing coating described above, comprising the following steps:

[0043] A premix was prepared by premixing hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, methylphenylvinylpolysiloxane, anchoring agent, inhibitor and toluene.

[0044] The premixed liquid and platinum catalyst are mixed to obtain the silicon-containing coating.

[0045] This invention involves premixing hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, methylphenylvinylpolysiloxane, an anchoring agent, an inhibitor, and toluene to obtain a premixed solution. In this invention, the premixing is preferably performed by stirring; the premixing time is preferably 10–30 min, specifically 10 min, 15 min, 20 min, 25 min, or 30 min.

[0046] After obtaining the premixed liquid, the present invention mixes the premixed liquid with a platinum catalyst to obtain the silicon-containing coating. In the present invention, the mixing is preferably performed by stirring; the mixing time is preferably 5 minutes.

[0047] The present invention also provides a modified nylon material, comprising nylon fibers and a silicon-containing coating covering the surface of the nylon fibers; the silicon-containing coating is formed by the silicon-containing coating described in the above-described scheme or the silicon-containing coating obtained by the preparation method described in the above-described scheme.

[0048] The modified nylon material provided by the present invention includes nylon fibers; the preferred warp and weft density of the nylon fibers is 158*158 fibers / dm, 315*244 fibers / dm, or 409*343 fibers / dm.

[0049] The modified nylon material provided by the present invention includes a silicon-containing coating on the surface of the nylon fiber; the weight ratio of the silicon-containing coating to the nylon fiber is preferably 1:10 to 150, specifically 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, 1:110, 1:120, 1:130, 1:140 or 1:150.

[0050] The present invention also provides a method for preparing the modified nylon material described above, comprising the following steps:

[0051] The modified nylon material is obtained by coating the surface of nylon fibers with a silicon-containing coating, drying and curing it.

[0052] In this invention, the coating is preferably dip coating; the dip coating is preferably applied once; the dip coating time is preferably 5 to 15 seconds, specifically 7 seconds, 9 seconds, 11 seconds or 13 seconds.

[0053] In this invention, the drying is preferably oven drying; the drying temperature is preferably 50-70°C, specifically 55°C, 60°C or 65°C, and the heat preservation drying time is preferably 1-3 minutes, specifically 2 minutes.

[0054] In this invention, the curing temperature is preferably 90–150°C, specifically 100°C, 110°C, 120°C, 130°C, or 140°C, and the curing time is preferably 30–120 seconds, specifically 40 seconds, 60 seconds, 80 seconds, or 100 seconds. During the curing process, under the action of a platinum catalyst, the diene bonds, silane-hydrogen bonds, or hydroxyl groups in the organosiloxanes (hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, and methylphenylvinylpolysiloxane) undergo addition or condensation reactions, crosslinking to form a 3D network structure. An anchoring agent increases the bonding force between the coating and the nylon fibers, thereby achieving a modified nylon material with a release effect.

[0055] In this invention, the curing process preferably includes cooling the product and then winding it up.

[0056] The present invention also provides the application of the modified nylon material described in the above-described scheme or the modified nylon material obtained by the preparation method described in the above-described scheme as a release fabric.

[0057] The modified nylon material provided by this invention has good demolding effect and leaves the fiber cloth texture on the surface of the product, making it suitable for use as a demolding cloth in fields such as composite material molding.

[0058] To further illustrate the present invention, the following detailed description of the invention's solutions, in conjunction with the accompanying drawings and embodiments, is provided, but should not be construed as limiting the scope of protection of the present invention.

[0059] Example 1

[0060] Ten parts of hexamethylcyclotrisiloxane (D3), ten parts of octamethylcyclotetrasiloxane (D4), five parts of methylphenylvinyl polysiloxane (vinyl chain ratio of 0.4%, phenyl chain ratio of 10%), 0.5 parts of anchoring agent (γ-aminopropyltriethoxysilane), 0.1 parts of inhibitor (2-methyl-3-butyn-2-ol), and 300 parts of toluene were added to a container and stirred evenly for 15 min. Then, 1.2 parts of platinum catalyst (platinum / olefin siloxane coordination compound, effective content of 10000 ppm) were added and stirred for 5 min to obtain a silicon-containing coating.

[0061] The silicone-containing coating is poured into the glue tank. A nylon fiber cloth with a warp and weft density of 158*158 threads / decimeter is selected. The nylon fiber cloth is immersed in the glue tank for 5 seconds, then transferred to the drying section of the drying tunnel at 60℃ to dry for 1 minute, and then transferred to the curing section of the curing tunnel at 120℃ to cure for 60 seconds. The cloth is then rolled up to obtain the modified nylon material.

[0062] Example 2

[0063] Five parts of hexamethylcyclotrisiloxane (D3), five parts of octamethylcyclotetrasiloxane (D4), 15 parts of methylphenylvinyl polysiloxane (vinyl chain ratio of 0.4%, phenyl chain ratio of 20%), 0.5 parts of anchoring agent (γ-aminopropyltriethoxysilane), 0.1 parts of inhibitor (2-methyl-3-butyn-2-ol), and 300 parts of toluene were added to a container and stirred evenly for 15 min. Then, 1.2 parts of platinum catalyst (platinum / olefin siloxane coordination compound, effective content of 10000 ppm) were added and stirred for 5 min to obtain a silicon-containing coating.

[0064] The silicone-containing coating is poured into the glue tank. A nylon fiber cloth with a warp and weft density of 409*343 threads / decimeter is selected. The nylon fiber cloth is immersed in the glue tank for 5 seconds, then transferred to the drying section of the drying tunnel at 60℃ to dry for 1 minute, and then transferred to the curing section of the curing tunnel at 120℃ to cure for 60 seconds. The cloth is then rolled up to obtain the modified nylon material.

[0065] Example 3

[0066] Five parts of hexamethylcyclotrisiloxane (D3), five parts of octamethylcyclotetrasiloxane (D4), 15 parts of methylphenylvinyl polysiloxane (vinyl chain ratio of 0.4%, phenyl chain ratio of 20%), 0.5 parts of anchoring agent (γ-aminopropyltriethoxysilane), 0.1 parts of inhibitor (2-methyl-3-butyn-2-ol), and 300 parts of toluene were added to a container and stirred evenly for 15 min. Then, 1.2 parts of platinum catalyst (platinum / olefin siloxane coordination compound, effective content of 10000 ppm) were added and stirred for 5 min to obtain a silicon-containing coating.

[0067] The silicone-containing coating is poured into the glue tank. A nylon fiber cloth with a warp and weft density of 409*343 threads / decimeter is selected. The nylon fiber cloth is immersed in the glue tank for 5 seconds, then transferred to the drying section of the drying tunnel at 60℃ to dry for 1 minute, and then transferred to the curing section of the curing tunnel at 150℃ to cure for 30 seconds. The cloth is then rolled up to obtain the modified nylon material.

[0068] Example 4

[0069] Ten parts of hexamethylcyclotrisiloxane (D3), eight parts of octamethylcyclotetrasiloxane (D4), seven parts of methylphenylvinyl polysiloxane (vinyl chain ratio of 0.4%, phenyl chain ratio of 10%), 0.5 parts of anchoring agent (γ-glycidoxypropyltrimethoxysilane), 0.1 parts of inhibitor (2-methyl-3-butyn-2-ol), and 300 parts of toluene were added to a container and stirred evenly for 15 min. Then, 1.2 parts of platinum catalyst (platinum / olefin siloxane coordination compound, effective content of 10000 ppm) were added and stirred for 5 min to obtain a silicone-containing coating.

[0070] The silicone-containing coating is poured into the glue tank. A nylon fiber cloth with a warp and weft density of 409*343 threads / decimeter is selected. The nylon fiber cloth is immersed in the glue tank for 10 seconds, then transferred to the drying section of the drying tunnel at 60℃ for 2 minutes, and then transferred to the curing section of the curing tunnel at 120℃ for 60 seconds. Finally, it is rolled up to obtain the modified nylon material.

[0071] Example 5

[0072] Ten parts of hexamethylcyclotrisiloxane (D3), eight parts of octamethylcyclotetrasiloxane (D4), seven parts of methylphenylvinyl polysiloxane (vinyl chain ratio of 0.4%, phenyl chain ratio of 10%), 0.5 parts of anchoring agent (γ-glycidoxypropyltrimethoxysilane), 0.1 parts of inhibitor (2-methyl-3-butyn-2-ol), and 300 parts of toluene were added to a container and stirred evenly for 15 minutes. Then, 1.2 parts of platinum catalyst (platinum / olefin siloxane coordination compound, effective content of 10000 ppm) were added and stirred for 5 minutes to obtain a silicone-containing coating.

[0073] The silicone-containing coating is poured into the glue tank. A nylon fiber cloth with a warp and weft density of 409*343 threads / decimeter is selected. The nylon fiber cloth is immersed in the glue tank for 15 seconds, then transferred to the drying section of the drying tunnel at 60℃ for 3 minutes, and then transferred to the curing section of the curing tunnel at 120℃ for 60 seconds. The cloth is then rolled up to obtain the modified nylon material.

[0074] Example 6

[0075] Ten parts of hexamethylcyclotrisiloxane (D3), eight parts of octamethylcyclotetrasiloxane (D4), seven parts of methylphenylvinyl polysiloxane (vinyl chain ratio of 0.4%, phenyl chain ratio of 10%), 0.5 parts of anchoring agent (γ-glycidoxypropyltrimethoxysilane), 0.1 parts of inhibitor (2-methyl-3-butyn-2-ol), and 300 parts of toluene were added to a container and stirred evenly for 15 minutes. Then, 1.2 parts of platinum catalyst (platinum / olefin siloxane coordination compound, effective content of 10000 ppm) were added and stirred for 5 minutes to obtain a silicone-containing coating.

[0076] The silicone-containing coating is poured into the glue tank. A nylon fiber cloth with a warp and weft density of 409*343 threads / decimeter is selected. The nylon fiber cloth is immersed in the glue tank for 10 seconds, then transferred to the drying section of the drying tunnel at 60℃ to dry for 2 minutes, and then transferred to the curing section of the curing tunnel at 90℃ to cure for 120 seconds. The cloth is then rolled up to obtain the modified nylon material.

[0077] Table 1. Formulations and process parameters for Examples 1-6

[0078]

[0079]

[0080] Test Example 1

[0081] The modified nylon materials prepared in Examples 1-6 were tested for coating amount, release force, residual rate, and 180° peel force against glass fiber epoxy resin prepreg. The release force test method was as follows: tesa TM 7475 tape was applied to the release surface of the modified nylon material to be tested. After rolling it back and forth three times with a 2kg pressure roller, a 25mm×130mm strip was cut. The strip was left at room temperature for 20 minutes and then applied to a steel plate with adhesive. The 7475 tape was peeled off at a peeling speed of 300mm / min at a 180° angle using a tensile testing machine. The reading of the tensile testing machine is the release force after 20 minutes.

[0082] The residual rate test method is as follows: standard NITTO tape TM31B tape was applied to the release surface of the modified nylon material to be tested, and rolled back and forth three times with a 2kg roller. A 25mm x 300mm strip was then cut and placed horizontally between two glass plates. The glass plates were placed at 70℃, 50% RH, and under a 2kg pressure for 20 hours; after cooling at room temperature for 4 hours, the strip was removed. The 31B standard tape on the strip was slowly peeled off from the release film and then applied to a steel plate. A 2kg electric roller was used to roll back and forth twice at a speed of 300mm / min under its own weight. After 20 minutes, the tape was peeled off on a tensile testing machine at a speed of 300mm / min. The average peel force reading from the tensile testing machine was recorded as L1.

[0083] Apply the new 31B standard tape (from the same roll used for the stencil) directly to the steel plate. Roll it back and forth twice at 300 mm / min under its own weight. Let it rest for 20 minutes. Then, peel the tape off at 300 mm / min using a tensile testing machine. Record the average peel force reading from the tensile testing machine as L0. The residual rate is calculated as: L1 / L0 × 100%. A higher residual rate indicates better performance of the modified nylon material and less impact on the adhesion of any adhesive substances applied to its surface.

[0084] The 180° peel test method is based on GB / T 2792-2014, and the results are shown in Table 2.

[0085] Table 2. Performance test results of modified nylon materials in Examples 1-6

[0086]

[0087]

[0088] As shown in Tables 1 and 2, although methylphenylvinyl polysiloxane has a relatively large molecular weight, which helps improve the temperature resistance of organosilicon, its reactivity is low, requiring a higher temperature for curing. Furthermore, due to the presence of active amide groups within the nylon fiber cloth, prolonged exposure to high temperatures can cause yellowing or shrinkage, making a high proportion of methylphenylvinyl polysiloxane unsuitable. With prolonged impregnation time, the surface coating of the nylon fiber cloth increases, making it easier to peel off from the resin prepreg surface. Because this invention uses low molecular weight polysiloxane, it has minimal steric hindrance and high reactivity, enabling reaction at low temperatures. The product obtained by reacting at 90°C for 2 minutes is essentially identical to the product obtained by reacting at 120°C for 1 minute, reducing energy consumption and protecting the nylon fiber cloth.

[0089] Test Example 2

[0090] Scanning electron microscopy analysis was performed on the nylon fiber cloth and the modified nylon materials of Examples 3 and 5. The results are as follows: Figure 1 As shown. According to Figure 1 It is evident that the nylon fiber cloth has a relatively loose structure with large gaps between the fibers; however, after applying the silicon-containing coating to the nylon fibers, the fiber surface undergoes significant changes, as shown in the scanning electron microscope image of Example 3; with the increase of coating amount, the degree of coating coverage on the fibers gradually increases, with the coating amount in Example 5 being 6.6 g / m². 2 The coating amount in Example 3 was 1.5 g / m³. 2 .

[0091] Water droplet contact angle tests were conducted on nylon fiber cloth, the modified nylon materials of Examples 1 and 3-6, and the results are as follows: Figure 2 As shown. According to Figure 2 It can be seen that since the nylon fiber cloth has no coating on its surface, water droplets are in a wetting state on it. The silicon coating content of Example 5 is the highest, so its water droplet contact angle is the largest. This is followed by Example 4 and Example 1. As the content of the silicon coating decreases, the water droplet contact angle also decreases. Example 2 has a small water droplet contact angle because of its high molecular weight organosilicon content, low low-temperature reactivity, and incomplete reaction. Furthermore, high molecular weight organosilicon is prone to shrinkage of nylon fiber cloth when reacting at high temperatures. Therefore, the content of high molecular weight organosilicon should not be too high.

[0092] Photoelectron spectroscopy analysis was performed on the nylon fiber cloth and the modified nylon materials of Examples 1, 3, and 5. The results are as follows: Figure 3 As shown. According to Figure 3 It can be seen that as the basis weight of the silicon-containing coating gradually increases, the content of Si element also increases significantly, resulting in a good adhesion effect on the surface of nylon fiber.

[0093] The modified nylon materials from Examples 1 and 3-6 were tested in autoclaves, and the results are as follows: Figure 4 As shown. According to Figure 4 It can be seen that without a silicon-containing coating or with a low silicon-containing coating content, it is difficult to peel off from the surface of the prepreg after use. As the silicon-containing coating content increases, the release property of the surface is significantly improved, and the nylon fiber cloth can be completely peeled off from the surface of the prepreg, thus playing the role of a release cloth. In Example 3, due to the high production temperature, the nylon fiber cloth was deformed, and the effect after use was not good. From the comparison of the use of Examples 5 and 6, it can be seen that the low reaction temperature can allow the silicon-containing coating to adhere to the nylon fiber, achieving the same effect as the high temperature reaction. This not only reduces energy consumption but also reduces the impact of high temperature on the nylon fiber cloth.

[0094] As can be seen from the above embodiments, the modified nylon material with silicon-containing coating provided by the present invention has good demolding effect, good temperature resistance, and leaves fiber cloth texture on the surface of the product.

[0095] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A silicon-containing coating, characterized in that, It is prepared from the following raw materials in parts by weight: 10 parts hexamethylcyclotrisiloxane, 8 parts octamethylcyclotetrasiloxane, 7 parts methylphenylvinylpolysiloxane, 0.5 parts anchoring agent, 1.2 parts platinum catalyst, 0.1 parts inhibitor, and 300 parts toluene; the methylphenylvinylpolysiloxane has a viscosity of 10,000~50,000 mPa·s at 25 °C, the anchoring agent is γ-glycidyl etheroxypropyltrimethoxysilane, the inhibitor is 2-methyl-3-butyn-2-ol, and the methylphenylvinylpolysiloxane has a vinyl chain ratio of 0.4% and a phenyl chain ratio of 10%.

2. The method for preparing the silicon-containing coating according to claim 1, characterized in that, Includes the following steps: A premix was prepared by premixing hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, methylphenylvinylpolysiloxane, anchoring agent, inhibitor and toluene. The premixed liquid and platinum catalyst are mixed to obtain the silicon-containing coating.

3. A modified nylon material, characterized in that, It includes nylon fibers and a silicon-containing coating covering the surface of the nylon fibers; the silicon-containing coating is formed by the silicon-containing coating of claim 1 or the silicon-containing coating obtained by the preparation method of claim 2.

4. The modified nylon material according to claim 3, characterized in that, The weight ratio of the silicon-containing coating to the nylon fiber is 1:10~150.

5. A method for preparing the modified nylon material according to any one of claims 3 to 4, characterized in that, Includes the following steps: The modified nylon material is obtained by coating the surface of nylon fibers with a silicon-containing coating, drying and curing it.

6. The preparation method according to claim 5, characterized in that, The curing temperature is 90~150 ℃, and the curing time is 30~120 s.

7. The use of the modified nylon material according to any one of claims 3 to 4 or the modified nylon material obtained by the preparation method according to any one of claims 5 to 6 as a release fabric.

Citation Information

Patent Citations

  • High-temperature-resistant low-transfer organosilicone release agent and preparation method thereof

    CN109880523A

  • Strippable cloth for composite material forming and preparation method and application thereof

    CN117779460A