A magnesium-based hydrogen storage material, a preparation method and application thereof
By using a ternary magnesium alloy system composed of Ni and Er, the problems of high temperature and low rate of magnesium-based hydrogen storage materials have been solved, achieving high-efficiency hydrogen storage performance below 350℃, which is suitable for fuel cells, hydride hydrogen storage devices and hydrogen separation and recovery devices.
Patent Information
- Application Number
- CN202411809493.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-10
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-10
AI Technical Summary
Magnesium-based hydrogen storage materials suffer from high hydrogen absorption and desorption temperatures and slow reaction rates, which limit their widespread application in the hydrogen energy industry chain.
A ternary magnesium alloy system composed of Ni and Er was used to prepare Mg-Ni-Er alloy powder by vacuum melting and ball milling, forming Mg₂Ni phase and Er solid solution, providing more active sites and diffusion channels, and improving thermodynamic and kinetic properties.
At temperatures of 350℃ and below, magnesium-based hydrogen storage materials exhibit excellent hydrogen absorption and desorption performance, with fast hydrogen desorption rate and significantly increased hydrogen absorption capacity, meeting the requirements of industrial applications.
Smart Images

Figure CN119614901B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydrogen storage materials technology, specifically relating to a magnesium-based hydrogen storage material, its preparation method, and its application. Background Technology
[0002] Hydrogen energy boasts abundant resources, is carbon-free, has high energy density (120 MJ / kg), and diverse applications, demonstrating immense potential in mitigating environmental pollution and driving energy transition. Currently, safe and efficient hydrogen storage and transportation technologies are one of the main bottlenecks restricting the development of the hydrogen energy industry chain.
[0003] Compared with traditional hydrogen storage technologies, magnesium-based solid-state hydrogen storage technology has advantages such as low cost, high hydrogen storage density (7.6 wt.% and 110 g H2 / L), safety, high efficiency, and good reversibility, which opens up greater possibilities for the large-scale utilization of hydrogen energy. However, inherent thermodynamic and kinetic challenges related to magnesium-based hydrogen storage still exist, which directly lead to its disadvantages of high hydrogen absorption and desorption temperatures (>350℃) and slow reaction rates. Therefore, solving these problems remains the main scientific challenge for the widespread application of magnesium-based solid-state hydrogen storage technology.
[0004] Alloying is a simple and efficient way to improve the hydrogen storage performance of MgH2, which is conducive to achieving industrialization goals. Existing research has found that alloys based on ternary magnesium alloy systems composed of transition metals and rare earth metals can effectively form long-period phases. The nanocrystals formed by the decomposition of these long-period phases after initial activation provide more active sites for the reaction, offering more active sites and diffusion channels for hydrogen dissociation and transfer. This results in good hydrogen charging and decharging performance at temperatures up to 350℃, enabling better hydrogen storage. Therefore, developing an alloy based on a ternary magnesium alloy system composed of transition metals and rare earth metals as a hydrogen storage material has great potential. Summary of the Invention
[0005] This invention develops a ternary magnesium alloy system based on Ni (transition metal) and Er (rare earth metal) as a hydrogen storage material. It has excellent hydrogen absorption and desorption performance at 350℃ and below, and its performance is better than that of other ternary magnesium alloys composed of rare earth metals, such as Gd.
[0006] To achieve the above objectives, the present invention can adopt the following technical solutions:
[0007] In one aspect, the present invention provides a magnesium-based hydrogen storage material, which, by mass percentage, comprises Er 2%-12%, Ni 2%-12%, unavoidable impurities, and the balance Mg.
[0008] Preferably, in the above-mentioned magnesium-based hydrogen storage material, the mass percentage of Mg is ≥90%, and the mass fraction of Ni is ≥Er.
[0009] Preferably, in the above-mentioned magnesium-based hydrogen storage material, the mass percentage of Mg is ≥90%, and the mass fraction of Ni is ≥Er, with the mass fraction of Ni being 5%-7.8%.
[0010] Preferably, the above-mentioned magnesium-based hydrogen storage material is selected from any one of the following materials: (a) magnesium-based hydrogen storage material comprising, by mass percentage, 7.8% Ni, 2.2% Er, unavoidable impurities, and the balance Mg; (b) magnesium-based hydrogen storage material comprising, by mass percentage, 2.2% Ni, 7.8% Er, unavoidable impurities, and the balance Mg; (c) magnesium-based hydrogen storage material comprising, by mass percentage, 6.5% Ni, 3.5% Er, unavoidable impurities, and the balance Mg; (d) magnesium-based hydrogen storage material comprising, by mass percentage, 5% Ni, 5% Er, unavoidable impurities, and the balance Mg; (e) magnesium-based... The hydrogen storage materials, by mass percentage, include 2% Ni, 12% Er, unavoidable impurities, and the balance Mg; (f) the magnesium-based hydrogen storage materials, by mass percentage, include 12% Ni, 2% Er, unavoidable impurities, and the balance Mg; (g) the magnesium-based hydrogen storage materials, by mass percentage, include 7% Ni, 5% Er, unavoidable impurities, and the balance Mg; (h) the magnesium-based hydrogen storage materials, by mass percentage, include 6% Ni, 6% Er, unavoidable impurities, and the balance Mg; (i) the magnesium-based hydrogen storage materials, by mass percentage, include 5% Ni, 3% Er, unavoidable impurities, and the balance Mg.
[0011] Another aspect of the present invention provides a method for preparing the magnesium-based hydrogen storage material of the present invention, comprising: (1) mixing magnesium ingots, Mg-Ni master alloy and Mg-Er master alloy and then melting them, and casting them to obtain Mg-Ni-Er alloy; (2) preparing Mg-Ni-Er alloy into Mg-Ni-Er alloy powder, thereby obtaining the magnesium-based hydrogen storage material.
[0012] Preferably, the above preparation method satisfies one or more of the following conditions: (a) in step (1), the purity of the magnesium ingot is ≥99%; (b) in step (1), the smelting includes: smelting in a vacuum smelting furnace in two stages, the power of the first stage is ≥15kW and the power of the second stage is ≥35kW; the smelting time of the first stage and the second stage is ≥5min each; (c) in step (2), preparing Mg-Ni-Er alloy into Mg-Ni-Er alloy powder includes: pulverizing Mg-Ni-Er alloy and ball milling to obtain Mg-Ni-Er alloy powder; (d) the diameter of Mg-Ni-Er alloy powder is ≤15um.
[0013] Preferably, the ball milling described above satisfies one or more of the following conditions: 1) ball milling is carried out in an inert gas environment; 2) mechanical wet ball milling is selected.
[0014] Preferably, the above-mentioned mechanical wet ball milling satisfies one or more of the following conditions: (i) the solvent for ball milling is selected from one or more of n-heptane, ethanol, isopropanol or ethyl acetate; (ii) the ball-to-material ratio is (20-40):1; (iii) the ball milling speed is 250 rpm-350 rpm; (iv) the diameter of the grinding balls is 8 mm and 6 mm.
[0015] In another aspect, the present invention provides a hydrogen storage device, which is made of the magnesium-based hydrogen storage material of the present invention.
[0016] Another aspect of the present invention provides an application of the magnesium-based hydrogen storage material of the present invention in solid-state hydrogen storage.
[0017] The beneficial effects of this invention include at least the following:
[0018] (1) The magnesium-based hydrogen storage material provided by the present invention has excellent hydrogen absorption and desorption capacity. At 350℃ (4MPa), the hydrogen desorption capacity can reach 6.16wt.% in 5 minutes; at 300℃ (4MPa), the hydrogen absorption capacity can reach 5.77wt.% in 10 minutes; and at 250℃ (4MPa), the hydrogen absorption capacity can reach 5.7wt.% in 20 minutes.
[0019] (2) The magnesium-based hydrogen storage material provided by the present invention has an excellent hydrogen release rate. After hydrogenation at 300℃ (4MPa), it only takes 2 minutes to release 6.3wt.% of hydrogen; and at 350℃ (4MPa), the hydrogen absorption can reach 6.44wt.% within 60 minutes.
[0020] (3) Compared with the magnesium-based hydrogen storage material based on Gd, the magnesium-based hydrogen storage material provided by the present invention can improve the hydrogen release rate by about 6% in 5 minutes at 350℃ (4MPa); the hydrogen absorption rate in 10 minutes at 300℃ (4MPa) can improve the hydrogen absorption rate by about 20%; and the hydrogen absorption rate in 20 minutes at 250℃ (4MPa) can improve the hydrogen absorption rate by about 24%.
[0021] (4) Among the magnesium-based hydrogen storage materials provided by the present invention, the hydrogen absorption and desorption performance of hydrogen storage materials with Mg ≥ 90% and Ni mass fraction ≥ Er mass fraction is much better than that of hydrogen storage materials with Mg < 90% and Ni mass fraction ≥ Er mass fraction; for example, the performance of Mg-5wt.%Ni-5wt.%Er alloy is much better than that of Mg-6wt.%Ni-6wt.%Er alloy; and for another example, the performance of Mg-7.8wt.%Ni-2.2wt.%Er alloy is much better than that of Mg-12wt.%Ni-2wt.%Er alloy.
[0022] (5) The preparation method of magnesium-based hydrogen storage material provided by the present invention can be obtained by vacuum melting and ball milling. The preparation method is simple and meets the requirements of industrial application of magnesium-based hydrogen storage material. Attached Figure Description
[0023] Figure 1 The image shows a SEM image of the Mg-Ni-Er alloy prepared in Example 1.
[0024] Figure 2 SEM image of the ball-milled Mg-Ni-Er alloy prepared in Example 1;
[0025] Figure 3 The XRD pattern of the Mg-Ni-Er alloy prepared in Example 1 is shown below.
[0026] Figure 4 Isothermal hydrogen desorption curves of the magnesium-based hydrogen storage material prepared in Example 1 at different temperatures;
[0027] Figure 5 Isothermal hydrogen absorption curves of the magnesium-based hydrogen storage material prepared in Example 1 at different temperatures;
[0028] Figure 6 The hydrogen absorption and desorption curves of the magnesium-based hydrogen storage material prepared in Example 1 after 40 cycles at 300°C are shown. Detailed Implementation
[0029] The embodiments described are provided to better illustrate the present invention, but are not intended to limit the scope of the invention to the embodiments described. Therefore, non-essential improvements and adjustments made to the embodiments by those skilled in the art based on the above description are still within the scope of protection of the present invention.
[0030] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit this disclosure. Singular expressions include plural expressions unless they have a distinct meaning in the context. As used herein, it should be understood that terms such as “comprising,” “having,” “including,” are intended to indicate the presence of a feature, number, operation, material, or combination thereof. The terminology of the invention is disclosed in the specification and is not intended to exclude the possibility that one or more other features, numbers, operations, materials, or combinations thereof may be present or added. As used herein, “ / ” may be interpreted as “and” or “or,” depending on the context.
[0031] This invention provides a magnesium-based hydrogen storage material, which, by mass percentage, comprises 2%-12% Er, 2%-12% Ni, unavoidable impurities, and the balance Mg.
[0032] It should be noted that the magnesium-based hydrogen storage material in this invention is a Mg-Ni-Er alloy. On the one hand, the Mg2Ni phase formed can promote H2 dissociation and effectively act as a "hydrogen pump". After ball milling, the Mg2Ni phase becomes finer, providing a large number of active sites for hydrogen dissociation and diffusion, thus promoting the stable and efficient hydrogen storage kinetics of MgH2. On the other hand, Er is dissolved in the Mg matrix, causing lattice distortion, which effectively promotes Mg-H dissociation and greatly improves the thermodynamic stability of MgH2, showing good application prospects in solid-state hydrogen storage.
[0033] It should also be noted that the magnesium-based hydrogen storage material in this invention, by mass percentage, includes Er 2%-12%, Ni 2%-12%, unavoidable impurities, and the balance Mg; wherein Er can be 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or 11%, etc.; in addition, unavoidable impurities refer to small amounts of non-metallic elements, metallic elements, or compounds that cannot be completely removed from the metal during the metal smelting and processing due to limitations of raw materials, process conditions, etc.
[0034] In some specific examples, the above-mentioned magnesium-based hydrogen storage materials have a Mg mass percentage ≥ 90% and a Ni mass fraction ≥ Er mass fraction.
[0035] It should be noted that, in this invention, the magnesium-based hydrogen storage material preferably has a Mg mass percentage ≥ 90% and a Ni mass fraction ≥ Er mass fraction; for example, the Mg mass percentage can be 91%, 92%, 93%, 94%, or 95%, etc., and the Ni and Er mass fractions can be adaptively adjusted according to the Mg mass percentage; when the Mg mass percentage is < 90% and the Ni mass fraction is ≥ Er mass fraction, the hydrogen absorption and desorption performance of the magnesium-based hydrogen storage material is not as good as that of the magnesium-based hydrogen storage material with a Mg mass percentage ≥ 90% and a Ni mass fraction ≥ Er mass fraction; for example, the performance of the Mg-5wt.%Ni-5wt.%Er alloy is much better than that of the Mg-6wt.%Ni-6wt.%Er alloy; and the performance of the Mg-7.8wt.%Ni-2.2wt.%Er alloy is much better than that of the Mg-12wt.%Ni-2wt.%Er alloy.
[0036] In some specific examples, in the above-mentioned magnesium-based hydrogen storage materials, the mass percentage of Mg is ≥90%, and the mass fraction of Ni is ≥Er, with the mass fraction of Ni being 5%-7.8%.
[0037] It should be noted that, in the magnesium-based hydrogen storage material of the present invention, the mass percentage of Mg is ≥90% and the mass fraction of Ni is ≥Er, and the preferred mass fraction of Ni is 5%-7.8%, such as 5.3%, 5.5%, 5.8%, 6%, 6.2%, 6.4%, 6.8%, 7%, 7.3%, 7.5% or 7.7%.
[0038] In some specific examples, the magnesium-based hydrogen storage materials mentioned above are selected from any one of the following materials:
[0039] (a) The magnesium-based hydrogen storage material, by mass percentage, includes 7.8% Ni, 2.2% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 6.16 wt.% at 350 °C (4 MPa) for 5 min; a hydrogen absorption of 5.77 wt.% at 300 °C (4 MPa) for 10 min; and a hydrogen absorption of 5.7 wt.% at 250 °C (4 MPa) for 20 min.
[0040] (b) The magnesium-based hydrogen storage material, by mass percentage, includes 2.2% Ni, 7.8% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 5.19 wt.% at 350°C (4 MPa) for 5 minutes; a hydrogen absorption of 5.18 wt.% at 300°C (4 MPa) for 10 minutes; and a hydrogen absorption of 3.7 wt.% at 250°C (4 MPa) for 20 minutes.
[0041] (c) The magnesium-based hydrogen storage material, by mass percentage, includes 6.5% Ni, 3.5% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 5.86 wt.% at 350℃ (4MPa) for 5 minutes; a hydrogen absorption of 5.6 wt.% at 300℃ (4MPa) for 10 minutes; and a hydrogen absorption of 5.3 wt.% at 250℃ (4MPa) for 20 minutes.
[0042] (d) The magnesium-based hydrogen storage material, by mass percentage, includes 5% Ni, 5% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 5.8 wt.% at 350℃ (4MPa) for 5 minutes; a hydrogen absorption of 5.54 wt.% at 300℃ (4MPa) for 10 minutes; and a hydrogen absorption of 5.0 wt.% at 250℃ (4MPa) for 20 minutes.
[0043] (e) The magnesium-based hydrogen storage material, by mass percentage, includes 2% Ni, 12% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 5.7 wt.% at 350°C (4 MPa) for 5 min; a hydrogen absorption of 4.3 wt.% at 300°C (4 MPa) for 10 min; and a hydrogen absorption of 3.9 wt.% at 250°C (4 MPa) for 20 min.
[0044] (f) The magnesium-based hydrogen storage material, by mass percentage, includes 12% Ni, 2% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 5.5 wt.% at 350℃ (4MPa) for 5 minutes; a hydrogen absorption of 5.2 wt.% at 300℃ (4MPa) for 10 minutes; and a hydrogen absorption of 4.9 wt.% at 250℃ (4MPa) for 20 minutes.
[0045] (g) The magnesium-based hydrogen storage material, by mass percentage, includes 7% Ni, 5% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 5.6 wt.% at 350℃ (4MPa) for 5 minutes; a hydrogen absorption of 5.3 wt.% at 300℃ (4MPa) for 10 minutes; and a hydrogen absorption of 4.8 wt.% at 250℃ (4MPa) for 20 minutes.
[0046] (h) The magnesium-based hydrogen storage material, by mass percentage, includes 6% Ni, 6% Er, unavoidable impurities, and the balance Mg; the proportion of this magnesium-based hydrogen storage material can achieve a hydrogen release of 5.4 wt.% at 350℃ (4MPa) for 5 minutes; a hydrogen absorption of 5.1 wt.% at 300℃ (4MPa) for 10 minutes; and a hydrogen absorption of 4.6 wt.% at 250℃ (4MPa) for 20 minutes.
[0047] (i) The magnesium-based hydrogen storage material, by mass percentage, includes 5% Ni, 3% Er, unavoidable impurities, and the balance Mg; the magnesium-based hydrogen storage material of this proportion can achieve a hydrogen release of 5.5 wt.% at 350 °C (4 MPa) for 5 min; a hydrogen absorption of 5.2 wt.% at 300 °C (4 MPa) for 10 min; and a hydrogen absorption of 4.9 wt.% at 250 °C (4 MPa) for 20 min.
[0048] This invention also provides a method for preparing the magnesium-based hydrogen storage material of the present invention, comprising: (1) mixing magnesium ingots, Mg-Ni master alloy and Mg-Er master alloy and then melting them, and casting them to obtain Mg-Ni-Er alloy; (2) preparing Mg-Ni-Er alloy into Mg-Ni-Er alloy powder, thereby obtaining the magnesium-based hydrogen storage material.
[0049] It should be noted that the operations such as "melting" and "casting" in this invention are conventional operations in the field and have no specific meaning. The specific operation method of the above operations can be selected according to the specific preparation environment.
[0050] In some specific examples, the above preparation method satisfies one or more combinations of the following conditions:
[0051] (a) In step (1), the purity of the magnesium ingot is ≥99%;
[0052] (b) In step (1), the smelting includes: smelting in a vacuum smelting furnace in two stages, with the power of the first stage being ≥15kW and the power of the second stage being ≥35kW; the smelting time of the first stage and the second stage is ≥5min each.
[0053] (c) In step (2), preparing Mg-Ni-Er alloy into Mg-Ni-Er alloy powder includes: crushing Mg-Ni-Er alloy and ball milling to obtain Mg-Ni-Er alloy powder;
[0054] (d) The diameter of Mg-Ni-Er alloy powder is ≤15um; specifically, the diameter of Mg-Ni-Er alloy powder can be ≤13um, ≤12um or ≤10um, etc., and different particle sizes are obtained according to different processes; the general particle size can be 5um-15um.
[0055] It should be noted that the operations such as "pulverizing" and "ball milling" in this invention are conventional operations in the field and have no specific meaning. The specific operation method of the above operations can be selected according to the specific preparation environment; for example, "pulverizing" in this invention can be performed by abrasion.
[0056] It should also be noted that the above preparation method satisfies any one of the conditions (a) to (c) above, and preferably satisfies all of the above conditions simultaneously.
[0057] In some specific examples, the above-mentioned ball mill satisfies one or more combinations of the following conditions:
[0058] 1) Ball milling is performed in an inert gas environment; specifically, the inert gas is a gas environment known in the art, such as argon, nitrogen or helium; in addition, the purpose of ball milling in an inert gas environment is to reduce the oxidation of the sample and the corrosion of the ball milling equipment.
[0059] 2) Mechanical wet ball milling is selected; specifically, any ball milling method known in the art can be selected in this invention, with mechanical wet ball milling being preferred, as the ball milling effect is better than other ball milling methods.
[0060] It should also be noted that the ball mill described above can satisfy any one of the conditions 1) to 2), and preferably all of the above conditions are satisfied at the same time.
[0061] In some specific examples, the above-described mechanical wet ball milling satisfies one or more of the following conditions:
[0062] (i) The solvent for ball milling is selected from one or more combinations of n-heptane, ethanol, isopropanol or ethyl acetate; specifically, n-heptane is preferred as the solvent for ball milling, as it is more effective than other solvents.
[0063] (ii) The ball-to-material ratio is (20-40):1; specifically, the ball-to-material ratio is the mass ratio of grinding balls to Mg-Ni-Er alloy, which can be 24:1, 27:1, 30:1, 33:1, 35:1 or 38:1, etc.
[0064] (iii) The ball mill speed is 250rpm-350rpm, such as 280rpm, 300rpm or 320rpm, etc.;
[0065] (iv) The diameter of the grinding balls is 8 mm and 6 mm; specifically, the diameter of the grinding balls can be arbitrarily selected, but a mixture of grinding balls with diameters of 8 mm and 6 mm is preferred.
[0066] It should be noted that the above-mentioned mechanical wet ball milling can satisfy any one of the above conditions (i) to (iv), and preferably all of the above conditions are satisfied at the same time.
[0067] This invention also provides a hydrogen storage device, which is made from the magnesium-based hydrogen storage material of this invention.
[0068] It should be noted that the magnesium-based hydrogen storage material in this invention has excellent hydrogen absorption and desorption properties, and can be used to prepare different hydrogen storage devices, such as fuel cells, hydride hydrogen storage devices, heat storage and heat transfer devices, and hydrogen separation and recovery devices.
[0069] This invention also provides an application of the magnesium-based hydrogen storage material of this invention in solid-state hydrogen storage.
[0070] It should be noted that, as described above, the magnesium-based hydrogen storage material of this invention has excellent hydrogen absorption and desorption properties and excellent potential for solid-state hydrogen storage.
[0071] To better understand the present invention, specific examples are provided below to further illustrate the content of the present invention, but the content of the present invention is not limited to the examples below.
[0072] I. Preparation and Characterization of Magnesium-Based Hydrogen Storage Materials
[0073] In the following examples, "Mg-30wt.%Ni" refers to a Ni-Mg alloy containing 30% Ni by mass and the remainder being Mg, and other expressions of this kind have the same meaning; "Mg-7.8wt.%Ni-2.2wt.%Er" refers to a Ni-Er-Mg alloy containing both 7.8% Ni and 2.2% Er by mass and the remainder being Mg, and other expressions of this kind have the same meaning.
[0074] Example 1
[0075] (1) Preparation of Mg-Ni-Er alloy: Weigh 3400g of pure Mg, 1326g of Mg-30wt.%Ni and 374g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 20kW for 10 minutes, then melt at 40kW for 10 minutes and cast to obtain Mg-Ni-Er alloy;
[0076] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 280rpm, milling jar of 250mL stainless steel, milling balls of 8mm and 6mm diameter stainless steel, 2 milling balls of 8mm diameter and the rest of 6mm milling balls) for 10h to prepare magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 7.8wt.%Ni, 2.2wt.%Er and unavoidable impurities and balance of Mg (can also be marked as Mg-7.8wt.%Ni-2.2wt.%Er, the same below).
[0077] The SEM image of the Mg-Ni-Er alloy prepared in step (1) is shown below. Figure 1 As shown, it can be seen that there is a large amount of Mg2Ni phase aggregate at the grain boundaries of the Mg-Ni-Er alloy obtained after melting.
[0078] The SEM image of the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy prepared in step (2) is shown below. Figure 2 As shown, the particle size of magnesium-based hydrogen storage materials based on Mg-Ni-Er alloy is approximately 5µm-15µm.
[0079] The XRD pattern of the Mg-Ni-Er alloy prepared in step (1) is shown below. Figure 3 As shown, the Mg-Ni-Er alloy is mainly composed of the α-Mg phase and the Mg2Ni phase.
[0080] Example 2
[0081] The difference between Example 2 and Example 1 is that the amount of raw materials added is different. The amount of raw materials added in Example 2 is: 3400g of pure Mg, 374g of Mg-30wt.%Ni, and 1326g of Mg-30wt.%Er. Other steps are the same as in Example 1. The magnesium-based hydrogen storage material based on Mg-Ni-Er alloy prepared includes 2.2wt.%Ni, 7.8wt.%Er, and unavoidable impurities and the balance of Mg.
[0082] Example 3
[0083] (1) Preparation of Mg-Ni-Er alloy: Weigh 3400g of pure Mg, 850g of Mg-30wt.%Ni and 850g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 15kW for 5min, then melt at 35kW for 5min and cast to obtain Mg-Ni-Er alloy;
[0084] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 250rpm, milling jar of 500mL stainless steel, and stainless steel milling balls with diameters of 8mm and 6mm, the number of milling balls is the same as in Example 1) for 10h to prepare magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 5wt.%Ni, 5wt.%Er and unavoidable impurities and the balance of Mg.
[0085] Example 4
[0086] (1) Preparation of Mg-Ni-Er alloy: Weigh 3400g of pure Mg, 1105g of Mg-30wt.%Ni and 595g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 15kW for 5min, then melt at 35kW for 5min and cast to obtain Mg-Ni-Er alloy;
[0087] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 250rpm, milling jar of 500mL stainless steel, and grinding balls of 8mm and 6mm diameter stainless steel, the number of grinding balls is the same as in Example 1) for 10h to obtain magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 6.5wt.%Ni, 3.5wt.%Er and unavoidable impurities and the balance of Mg.
[0088] Example 5
[0089] (1) Preparation of Mg-Ni-Er alloy: Weigh 2720g of pure Mg, 340g of Mg-30wt.%Ni and 2040g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 15kW for 5min, then melt at 35kW for 5min and cast to obtain Mg-Ni-Er alloy;
[0090] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 250rpm, milling jar of 500mL stainless steel, and grinding balls of 8mm and 6mm diameter stainless steel, the number of grinding balls is the same as in Example 1) for 10h to obtain magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 2wt.%Ni, 12wt.%Er and unavoidable impurities and the balance of Mg.
[0091] Example 6
[0092] (1) Preparation of Mg-Ni-Er alloy: Weigh 2720g of pure Mg, 2040g of Mg-30wt.%Ni and 340g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 15kW for 5min, then melt at 35kW for 5min and cast to obtain Mg-Ni-Er alloy;
[0093] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 250rpm, milling jar of 500mL stainless steel, and grinding balls of 8mm and 6mm diameter stainless steel, the number of grinding balls is the same as in Example 1) for 10h to obtain magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 12wt.%Ni, 2wt.%Er and unavoidable impurities and the balance of Mg.
[0094] Example 7
[0095] (1) Preparation of Mg-Ni-Er alloy: Weigh 3060g of pure Mg, 1190g of Mg-30wt.%Ni and 850g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 15kW for 5min, then melt at 35kW for 5min and cast to obtain Mg-Ni-Er alloy;
[0096] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 250rpm, milling jar of 500mL stainless steel, and grinding balls of 8mm and 6mm diameter stainless steel, the number of grinding balls is the same as in Example 1) for 10h to obtain magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 7wt.%Ni, 5wt.%Er and unavoidable impurities and the balance of Mg.
[0097] Example 8
[0098] (1) Preparation of Mg-Ni-Er alloy: Weigh 2720g of pure Mg, 1020g of Mg-30wt.%Ni and 1020g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 15kW for 5min, then melt at 35kW for 5min and cast to obtain Mg-Ni-Er alloy;
[0099] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 250rpm, milling jar of 500mL stainless steel, and stainless steel milling balls with diameters of 8mm and 6mm, the number of milling balls is the same as in Example 1) for 10h to obtain magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 6wt.%Ni, 6wt.%Er and unavoidable impurities and the balance of Mg.
[0100] Example 9
[0101] (1) Preparation of Mg-Ni-Er alloy: Weigh 3740g of pure Mg, 850g of Mg-30wt.%Ni and 510g of Mg-30wt.%Er respectively, place them in a vacuum melting furnace, melt and stir at 15kW for 5min, then melt at 35kW for 5min and cast to obtain Mg-Ni-Er alloy;
[0102] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Er alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 5g was mechanically wet-milled under argon atmosphere (n-heptane as solvent, ball-to-material ratio of 30:1, milling speed of 250rpm, milling jar of 500mL stainless steel, and stainless steel milling balls with diameters of 8mm and 6mm, the number of milling balls is the same as in Example 1) for 10h to obtain magnesium-based hydrogen storage material based on Mg-Ni-Er alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy includes 5wt.%Ni, 3wt.%Er and unavoidable impurities and the balance of Mg.
[0103] Comparative Example 1
[0104] The difference between Comparative Example 1 and Example 1 is that the amount of raw materials added is different. The amount of raw materials added in Comparative Example 1 is 3400g of pure Mg and 1700g of Mg-30wt.%Ni. Other steps are the same as in Example 1. The magnesium-based hydrogen storage material based on Mg-Ni alloy prepared includes 10wt.%Ni and unavoidable impurities and the balance of Mg.
[0105] Comparative Example 2
[0106] The difference between Comparative Example 2 and Example 1 is that the amount of raw materials added is different; the amount of raw materials added in Comparative Example 2 is: 3400g of pure Mg and 1700g of Mg-30wt.%Er; other steps are the same as in Example 1; the magnesium-based hydrogen storage material based on Mg-Er alloy prepared includes 10wt.%Er and unavoidable impurities and the balance of Mg.
[0107] Comparative Example 3
[0108] (1) Preparation of Mg-Ni-Gd alloy: Weigh 3400g of pure Mg, 1326g of Mg-30wt.%Ni and 374g of Mg-30wt.%Gd respectively, place them in a vacuum melting furnace, melt and stir at 20kW for 10 minutes, then melt at 40kW for 10 minutes and cast to obtain Mg-Ni-Gd alloy;
[0109] (2) Preparation of magnesium-based hydrogen storage material based on Mg-Ni-Gd alloy: The Mg-Ni-Er alloy prepared above was pulverized into powder, and 15g was mechanically wet-milled under an argon atmosphere (n-heptane as solvent, ball-to-material ratio of 20:1, milling speed of 280rpm, milling jar of 500mL stainless steel, and stainless steel milling balls with diameters of 8mm and 6mm, the number of milling balls being the same as in Example 1) for 10h to prepare magnesium-based hydrogen storage material based on Mg-Ni-Gd alloy; the magnesium-based hydrogen storage material based on Mg-Ni-Gd alloy includes 7.8wt.%Ni, 2.2wt.%Gd, and unavoidable impurities and the balance of Mg.
[0110] II. Hydrogen absorption and desorption tests of magnesium-based hydrogen storage materials
[0111] 150 mg of the magnesium-based hydrogen storage material (Mg-7.8 wt.% Ni-2.2 wt.% Er alloy powder) prepared in Example 1 was weighed in a glove box. The hydrogen desorption curves of the sample with temperature were tested using a PCTpro high-pressure gas adsorption instrument: isothermal hydrogen desorption curves at 225 °C, 250 °C, 275 °C, 300 °C, 325 °C and 350 °C at an initial hydrogen pressure of 0.01 MPa; isothermal hydrogen adsorption curves at 225 °C, 250 °C, 275 °C, 300 °C, 325 °C and 350 °C at an initial hydrogen pressure of 4 MPa; and hydrogen adsorption and desorption curves after 50 cycles at 300 °C.
[0112] The isothermal hydrogen desorption curves of the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy prepared in Example 1 at different temperatures and initial hydrogen pressures of 0.01 MPa are shown below. Figure 4 As shown, the results indicate that it can release 5.9 wt.% hydrogen at 260°C for 22 minutes; at 300°C, it only takes 2 minutes to release 6.3 wt.% hydrogen. This shows that the magnesium-based hydrogen storage material prepared in Example 1 not only has a lower initial hydrogen release temperature, but also significantly improved hydrogen release kinetics.
[0113] The isothermal hydrogen absorption curves of the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy prepared in Example 1 at different temperatures and initial hydrogen pressures of 4 MPa are shown below. Figure 5 As shown, the results indicate that it can absorb 6.44 wt.% hydrogen within 60 minutes at 350°C; this demonstrates that the hydrogen absorption kinetics of the magnesium-based hydrogen storage material prepared in Example 1 are significantly improved.
[0114] The hydrogen absorption and desorption curves of the magnesium-based hydrogen storage material based on Mg-Ni-Er alloy prepared in Example 1 after 40 cycles at 300°C and an initial hydrogen pressure of 3 MPa are shown below. Figure 6As shown, the results indicate that after 40 cycles of hydrogen absorption and desorption, the cycle capacity of the ball-milled Mg-7.8wt.%Ni-2.2wt.%Er alloy powder remains above 5.7wt.%, demonstrating stable cycle reversibility.
[0115] In addition, using a calibrated PCTpro high-pressure gas adsorption instrument (Setalam Instruments, France), the hydrogen release, hydrogen absorption, and hydrogen absorption of the magnesium-based hydrogen storage materials based on Mg-Ni-Er alloy in Examples 1 to 9 and Comparative Examples 1 to 3 were tested at 350°C and 4MPa initial hydrogen pressure for 5 minutes, 300°C and 4MPa initial hydrogen pressure for 10 minutes, and 250°C and 4MPa initial hydrogen pressure for 20 minutes. The results are shown in Table 1 below.
[0116] Table 1. Hydrogen absorption and desorption of different magnesium-based hydrogen storage materials based on Mg-Ni-Er alloys.
[0117]
[0118]
[0119] As shown in Table 1 above, the magnesium-based hydrogen storage material containing both Ni and Er exhibits excellent hydrogen absorption and desorption performance. At 350℃ (4MPa), the hydrogen desorption capacity reaches 6.16 wt.% in 5 minutes; at 300℃ (4MPa), the hydrogen absorption capacity reaches 5.77 wt.% in 10 minutes; and at 250℃ (4MPa), the hydrogen absorption capacity reaches 5.7 wt.% in 20 minutes (Example 1). All of these (Examples 1 to 9) are significantly superior to the hydrogen absorption and desorption performance of magnesium-based hydrogen storage materials containing only Ni or Er. Furthermore, the hydrogen absorption and desorption performance of the magnesium-based hydrogen storage material containing both Ni and Er is also significantly superior to that of the magnesium-based hydrogen storage material containing both Ni and Gd. The hydrogen absorption and desorption performance of the materials is far superior to that of magnesium-based hydrogen storage materials containing only Ni or Er. For example, at 350℃ (4MPa), the hydrogen desorption capacity in 5 minutes is about 6% higher for magnesium-based hydrogen storage materials containing both Ni and Er than that containing both Ni and Gd. At 300℃ (4MPa), the hydrogen absorption capacity in 10 minutes is about 20% higher for magnesium-based hydrogen storage materials containing both Ni and Er than that containing both Ni and Gd. At 250℃ (4MPa), the hydrogen absorption capacity in 20 minutes is about 24% higher for magnesium-based hydrogen storage materials containing both Ni and Er than that containing both Ni and Gd.
[0120] Furthermore, comparing Examples 1, 3, 4, and 2 reveals that when the mass fraction of Mg is 90%, the hydrogen absorption and desorption performance of hydrogen storage materials with a mass fraction of Ni ≥ Er is better than that of hydrogen storage materials with a mass fraction of Ni < Er. For example, the hydrogen absorption and desorption performance of the hydrogen storage material in Example 1 is better than that of the hydrogen storage material in Example 2.
[0121] Furthermore, by comparing Examples 1 and 9 with Examples 6 and 7, or comparing Examples 3 and 8, it can be seen that when the mass fraction of Ni is greater than or equal to the mass fraction of Er, the hydrogen absorption and desorption performance of hydrogen storage materials with a mass fraction of Mg greater than or equal to 90% is better than that of hydrogen storage materials with a mass fraction of Mg less than 90%. For example, the hydrogen absorption and desorption performance of hydrogen storage materials in Examples 1 and 9 is better than that in Examples 6 and 7, and the hydrogen absorption and desorption performance of hydrogen storage material in Example 3 is better than that in Example 9.
[0122] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A magnesium-based hydrogen storage material, characterized in that, It comprises, by mass percentage, 2%-12% Er, 2%-12% Ni, unavoidable impurities and balance Mg; Mg mass percentage ≥ 90% and Ni mass fraction ≥ Er mass fraction.
2. The magnesium-based hydrogen storage material according to claim 1, characterized in that, The mass fraction of Ni is 5%-7.8%.
3. The magnesium-based hydrogen storage material according to claim 2, characterized in that, Magnesium-based hydrogen storage materials can be selected from any one of the following materials: (a) The magnesium-based hydrogen storage material comprises, by mass percentage, 7.8% Ni, 2.2% Er, unavoidable impurities and the balance Mg; (b) Magnesium-based hydrogen storage materials, by mass percentage, include 6.5% Ni, 3.5% Er, unavoidable impurities, and the balance Mg; (c) Magnesium-based hydrogen storage materials, by mass percentage, include 5% Ni, 5% Er, unavoidable impurities and the balance Mg; (d) Magnesium-based hydrogen storage materials, by mass percentage, include 5% Ni, 3% Er, unavoidable impurities, and the balance Mg.
4. A method for preparing the magnesium-based hydrogen storage material according to any one of claims 1 to 3, characterized in that, include: (1) Mix magnesium ingots, Mg-Ni master alloy and Mg-Er master alloy and then melt them to cast Mg-Ni-Er alloy; (2) Prepare Mg-Ni-Er alloy powder from Mg-Ni-Er alloy to obtain magnesium-based hydrogen storage material.
5. The preparation method according to claim 4, characterized in that, The preparation method satisfies one or more of the following conditions: (a) In step (1), the purity of the magnesium ingot is ≥99%; (b) In step (1), the smelting includes: smelting in a vacuum smelting furnace in two stages, with the power of the first stage being ≥15kW and the power of the second stage being ≥35kW; the smelting time of the first stage and the second stage are each ≥5min. (c) In step (2), preparing Mg-Ni-Er alloy into Mg-Ni-Er alloy powder includes: crushing Mg-Ni-Er alloy and ball milling to obtain Mg-Ni-Er alloy powder; (d) The diameter of Mg-Ni-Er alloy powder is ≤15um.
6. The preparation method according to claim 5, characterized in that, The ball mill satisfies one or more of the following conditions: 1) Ball milling is performed in an inert gas environment; 2) Select mechanical wet ball milling.
7. The preparation method according to claim 6, characterized in that, Mechanical wet ball milling satisfies one or more of the following conditions: (i) The solvent for ball milling is selected from one or more combinations of n-heptane, ethanol, isopropanol or ethyl acetate; (ii) The ball-to-material ratio is (20-40):1; (iii) The ball mill rotation speed is 250 rpm - 350 rpm; (iv) The diameter of the grinding balls is 8 mm and 6 mm.
8. A hydrogen storage device, characterized in that, It is prepared from the magnesium-based hydrogen storage material as described in any one of claims 1 to 3.
9. The application of the magnesium-based hydrogen storage material according to any one of claims 1 to 3 in solid-state hydrogen storage.
Citation Information
Patent Citations
Nickel-containing high-toughness controllable degradation magnesium alloy material as well as preparation method and application thereof
CN109295368A
High-toughness rapidly-degradable Mg-Er-Ni alloy for underground fracturing and preparation method of high-toughness rapidly-degradable Mg-Er-Ni alloy
CN114908280A