Pore filling type anion exchange membrane, preparation method thereof and water electrolysis hydrogen production device
A pore-filled anion exchange membrane was prepared by thermally crosslinking biphenylpiperidone-styrene onto a porous polyethylene membrane. This solved the mechanical and dimensional stability problems of anion exchange membranes under alkaline conditions and achieved high conductivity and good water electrolysis performance.
Patent Information
- Application Number
- CN202411734434.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-11-28
AI Technical Summary
Existing anion exchange membranes have insufficient mechanical properties and dimensional stability under alkaline conditions, which affects the long-term use of electrochemical devices. Furthermore, the difference in hydrophilicity and hydrophobicity between ion polymers and porous substrates leads to unstable wetting and composite processes.
A pore-filled anion exchange membrane was prepared by forming a network structure with a pretreated porous polyethylene membrane and biphenylpiperidone-styrene through a thermal crosslinking reaction, thereby enhancing its stability in the porous polyethylene membrane.
It improves the stability, airtightness, conductivity and alkali resistance of the membrane, exhibiting excellent water electrolysis performance, and is suitable for large-scale industrial production.
Smart Images

Figure SMS_1 
Figure QLYQS_1 
Figure HDA0005161407390000011
Abstract
Description
Technical Field
[0001] This invention relates to the field of ion exchange membrane technology, and in particular to a pore-filled anion exchange membrane, its preparation method, and an electrolytic water hydrogen production device. Background Technology
[0002] With the increasing prominence of environmental protection issues, the development of technologies such as hydrogen production through water electrolysis, flow batteries, fuel cells, electrochemical ammonia synthesis, carbon dioxide reduction, salinity gradient energy conversion, electrodialysis, lithium extraction from salt lakes, and wastewater treatment has attracted much attention. In the development of these technologies, polyelectrolyte membrane materials play a crucial role in separating the positive and negative electrodes while allowing selective ion conduction across the membrane to form a complete current loop. The performance of polyelectrolyte membrane materials directly determines the technical parameters of electrochemical devices and their application processes. Therefore, it is essential to develop polyelectrolyte membrane materials with high ion selectivity, high ionic conductivity, long service life, and good mechanical properties.
[0003] In recent years, researchers have made significant efforts to develop high-performance anion exchange membranes (AEMs) by modulating the polymer backbone. For example, polyolefins, polystyrene, polyethersulfone, and poly(ether ketone) have been developed as polymer backbones for anion exchange membranes; cationic groups, such as pyrazole cations, imidazole cations, and metal-coordinated cations, have also been developed to modulate the polymer backbone. However, these materials exhibit numerous instabilities under alkaline conditions, and degradation reactions, including Hoffmann degradation and nucleophilic substitution, occur in the aforementioned cationic groups. Furthermore, studies have shown that the polyaryl ether backbone is prone to cleavage under alkaline conditions, while polymers without ether backbones and piperidinone structures are excellent alkali-resistant anion exchange membrane materials. However, despite significant progress in the alkali resistance of AEMs, most of these membranes still have shortcomings in physical properties. For example, in terms of mechanical durability, tensile strength is below 50 MPa and elongation at break is below 20%; in terms of dimensional stability, polybiphenylpiperidinone exhibits a high expansion rate (>200%) at 80°C. The poor mechanical properties and dimensional stability of AEMs directly affect the long-term use of the entire electrochemical device.
[0004] To improve the mechanical and dimensional stability of ionic polymers (AEMs), researchers have employed various modification methods, including crosslinking, branched copolymerization, and "pore-filling" composites. Among these, "pore-filling" composites are considered the most effective method for combining ionic polymers with porous substrates to create mechanically robust and durable materials, as porous substrates offer superior mechanical properties and chemical stability. However, significant differences exist between ionic polymers and porous substrates, such as hydrophilicity and hydrophobicity, making the complete wetting of the ionic polymer solution in a hydrophobic substrate and the stable two-phase composite a key challenge to be addressed.
[0005] Therefore, it is of great significance to research and develop a novel anion exchange membrane to solve the above problems. Summary of the Invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a pore-filled anion exchange membrane, its preparation method, and an electrolytic water hydrogen production device. The pore-filled anion exchange membrane is stable and dense, possessing good stability, airtightness, high conductivity, alkali resistance, and excellent water electrolysis performance.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0008] This invention provides a pore-filled anion exchange membrane, which is prepared by thermal crosslinking reaction of a pretreated polyethylene porous membrane and a biphenylpiperidone-styrene of Formula 1 located in its pores;
[0009] The polyethylene porous membrane is pretreated by soaking in an alcohol solvent.
[0010]
[0011] Formula 1;
[0012] Where nx and x are the degree of aggregation, 1≤n≤1000, 0.1≤x / (nx)≤1.
[0013] In the pore-filled anion exchange membrane of the present invention, the pretreated polyethylene porous membrane and the biphenylpiperidone-styrene shown in Formula 1 form a huge network structure after thermal crosslinking reaction. The crosslinking product with the network structure is tightly bound to the pretreated polyethylene porous membrane through "physical interlocking", which enhances the stability of the biphenylpiperidone-styrene shown in Formula 1 in the pretreated polyethylene porous membrane (substrate), so that the pore-filled anion exchange membrane has better performance in water electrolysis.
[0014] Specifically, the above-mentioned thermal crosslinking reaction involves the crosslinking of the olefin side chain in the biphenylpiperidone-styrene mixture shown in Formula 1 and the pretreated polyethylene porous membrane through carbon-carbon double bonds.
[0015] Preferably, the temperature of the thermal crosslinking reaction is 50℃-120℃; more preferably, it is 70℃-90℃. In some specific embodiments of the present invention, 80℃ is preferred.
[0016] Preferably, the porosity of the pretreated polyethylene porous membrane is 30%-80%; more preferably 40%-60%; and even more preferably 42%.
[0017] The thickness of the pretreated polyethylene porous membrane is 10-100 μm; more preferably 10-50 μm; and even more preferably 12 μm.
[0018] In some specific embodiments of the present invention, the biphenylpiperidone-styrene represented by Formula 1 is expressed as polybiphenylpiperidone-30% styrene (i.e., the grafting rate of styrene is 30%) having the following structure:
[0019] .
[0020] Preferably, the alcohol solvent is selected from one or more of ethanol, methanol, and isopropanol.
[0021] In this invention, the pore-filled anion exchange membrane can be represented as a polyethylene-polyphenylpiperidone-30% polystyrene (PE-pBP-30%) composite membrane.
[0022] The present invention also provides a method for preparing the above-mentioned pore-filled anion exchange membrane, comprising the following steps:
[0023] (1) Mix biphenyl, N-methyl-4-piperidone, trifluoromethanesulfonic acid, trifluoroacetic acid and solvent.
[0024] The reaction was carried out in an ice bath to give polydiphenylpiperidone;
[0025] (2) The polyphenylpiperidone, p-chloromethylstyrene obtained in step (1) and solvent are mixed and reacted. After the reaction is completed, iodomethane and potassium carbonate are added to the reaction system and a light-shielding reaction is carried out to obtain polyphenylpiperidone-styrene as shown in Formula 1.
[0026] (3) The poly(biphenylpiperidone-styrene) shown in Formula 1 is mixed with a solvent and degassed to obtain a casting solution;
[0027] (4) The casting liquid is added dropwise onto the pretreated polyethylene porous membrane, heated to carry out thermal cross-linking reaction, and dried to obtain a pore-filled anion exchange membrane.
[0028] This invention synthesizes an ether-free poly(biphenylpiperidone) backbone via a trifluoromethanesulfonic acid and trifluoroacetic acid-catalyzed polymerization method, and branches different proportions of p-chloromethylstyrene onto the side links, thereby obtaining the poly(biphenylpiperidone)-styrene structure shown in Formula 1. The poly(biphenylpiperidone)-styrene structure shown in Formula 1 is then prepared as a casting solution and slowly added dropwise onto a pretreated porous polyethylene membrane. Heating induces a crosslinking reaction between the poly(biphenylpiperidone)-styrene shown in Formula 1 and the carbon-carbon double bonds in the underlying porous polyethylene membrane. After drying, the pore-filled anion exchange membrane of this invention is obtained.
[0029] Preferably, in step (1), the molar ratio of biphenyl to N-methyl-4-piperidone is 1:(1.0-1.5); more preferably, it is 1:(1.0-1.2). In some specific embodiments of the present invention, a ratio of 1:1 is preferred.
[0030] Preferably, the molar ratio of biphenyl to trifluoromethanesulfonic acid in step (1) is 1:(6-12); more preferably, it is 1:(7-11). In some specific embodiments of the present invention, it is preferably 1:7. Preferably, the volume ratio of trifluoromethanesulfonic acid to trifluoroacetic acid in step (1) is 1:(0.01-0.1); more preferably, it is 1:(0.05-0.1); and even more preferably, it is 1:0.1.
[0031] The solvent in step (1) includes, but is not limited to, dichloromethane.
[0032] The preferred reaction time in step (1) under ice bath is 12-24 h.
[0033] Step (1) is to react in an ice bath until the viscosity of the reaction system is high. After the reaction is completed, the reaction is further separated and processed.
[0034] The preferred post-separation treatment involves slowly pouring the reaction solution into water to precipitate the polymer, followed by repeated washing and drying to obtain a white powder of poly(biphenylpiperidone). Preferably, in step (2), the molar ratio of p-chloromethylstyrene to poly(biphenylpiperidone) is (0.1-1):1.
[0035] The reaction in step (2) and the light-shielding reaction are both at room temperature; the reaction time is preferably 24-48 h.
[0036] The solvents used in step (2) include, but are not limited to, dimethyl sulfoxide, N-methylpyrrolidone, and N,N-dimethylformamide. In some specific embodiments of the present invention, dimethyl sulfoxide is used.
[0037] After the light-shielding reaction in step (2) is completed, post-processing such as separation is also included.
[0038] The separation specifically involves slowly pouring the solution from step (2) into acetone, washing, filtering, and drying to obtain the product, namely poly(biphenylpiperidone-styrene) as shown in Formula 1.
[0039] The room temperature is preferably 10℃-30℃. Preferably, the concentration of poly(biphenylpiperidone-styrene) of Formula 1 in the casting solution of step (3) is 2wt%-10wt%.
[0040] The solvents used in step (3) include, but are not limited to, dimethyl sulfoxide, N-methylpyrrolidone, and N,N-dimethylformamide. In some specific embodiments of the present invention, dimethyl sulfoxide is used.
[0041] In the above preparation method, the pretreatment method for the polyethylene porous membrane in step (4) is specifically as follows:
[0042] The hydrophilicity of polyethylene porous membranes is improved by immersing them in an alcohol solvent to clean the impurities inside the pores.
[0043] The pretreated porous polyethylene membrane is laid flat on a glass plate. Then, the casting solution is dropped onto its surface, filling the pores with the casting solution. Finally, a thermal cross-linking reaction is initiated by heating, followed by washing and drying to obtain the pore-filled anion exchange membrane.
[0044] The present invention does not impose any special limitations on the washing and drying in steps (1), (2) and (4) above, and any washing and drying method known to those skilled in the art is acceptable.
[0045] In this invention, the washing process uses pure water, and the drying process uses vacuum drying.
[0046] The method for preparing the pore-filled anion exchange membrane described in this invention effectively improves the density of the pore-filled anion exchange membrane through the synergistic effect of "physical interlocking" and pretreatment to improve the hydrophilicity of the porous polyethylene membrane substrate. At the same time, it gives the membrane excellent water electrolysis performance, good stability, airtightness, high conductivity and alkali resistance in water electrolysis applications.
[0047] The above preparation method is simple and efficient, and suitable for large-scale industrial production.
[0048] The present invention also provides a water electrolysis hydrogen production device, comprising the above-described pore-filled anion exchange membrane or the pore-filled anion exchange membrane prepared by the above-described preparation method.
[0049] Preferably, the water electrolysis hydrogen production device includes a membrane electrode, bipolar plates arranged in sequence, and sealing elements, etc.
[0050] The membrane electrode includes a gas diffusion layer, a catalyst layer, and the anion exchange membrane described in this invention.
[0051] Preferably, the electrolyte in the water electrolysis hydrogen production device is a KOH solution with a concentration of 0.1-1 mol / L.
[0052] The present invention also provides the application of the above-described pore-filled anion exchange membrane or the pore-filled anion exchange membrane prepared by the above-described preparation method in fuel cells and flow batteries.
[0053] Compared with the prior art, the pore-filled anion exchange membrane provided by the present invention is prepared by thermal crosslinking reaction of a pretreated polyethylene porous membrane and a biphenylpiperidone-styrene of Formula 1 located in the pores, wherein 1≤n≤1000, 0.1≤x / (nx)≤1; the polyethylene porous membrane is pretreated by immersion in an alcohol solvent. The pore-filled anion exchange membrane is stable and dense, and has good stability, airtightness, high conductivity, alkali resistance and excellent water electrolysis performance. Attached Figure Description
[0054] Figure 1 The 1H NMR spectrum of poly(biphenylpiperidone-30%) styrene (PBP-30%) in Example 1;
[0055] Figure 2 This is a photograph of the PE-pBP-30%-OH composite membrane used in Example 1.
[0056] Figure 3 This is an electron microscope cross-sectional image of the PE-pBP-30%-OH composite film in Example 1;
[0057] Figure 4 This is a hydrogen gas tightness diagram of the PE-pBP-30%-OH composite membrane in Example 1;
[0058] Figure 5 The diagram shows the conductivity properties of the PE-pBP-30%-OH composite membrane in Example 1.
[0059] Figure 6 This is a graph showing the conductivity degradation stability of the PE-pBP-30%-OH composite membrane in Example 1;
[0060] Figure 7 The graph shows the performance of the PE-pBP-30%-OH composite membrane in Example 1 based on the polarization curves of water electrolysis at different temperatures.
[0061] Figure 8 The graph shows the stability of the PE-pBP-30%-OH composite membrane in Example 1 under constant temperature and constant current density conditions during water electrolysis. Detailed Implementation
[0062] To further illustrate the present invention, the following detailed description of the pore-filled anion exchange membrane, its preparation method, and the water electrolysis hydrogen production device provided by the present invention is provided in conjunction with embodiments.
[0063] Example 1
[0064] (I) Preparation method of pore-filled composite membrane based on polyethylene-polyphenylpiperidone-30% styrene (30% is the grafting rate) (PE-pBP-30%)
[0065] (1) Dissolve 1.542 g (10 mmol) of biphenyl and 1.13 g (10 mmol) of N-methyl-4-piperidinone in 50 mL of dichloromethane and stir at 0 °C for 30 minutes; then add 5 mL of trifluoromethanesulfonic acid and 0.5 mL of trifluoroacetic acid dropwise, controlling the addition time to about 2 hours; then continue stirring at 0 °C for 24 hours until the solution becomes viscous. Wash the viscous solution with pure water and dry it under vacuum to obtain a white powder of polybiphenylpiperidinone.
[0066] (2) Disperse white powder polydiphenylpiperidone in 50 mL of dimethyl sulfoxide; add 0.458 g (3 mmol) of p-chloromethylstyrene and stir at room temperature for 24 hours; then add 1.42 g (10 mmol) of iodomethane and 1.382 g (10 mmol) of potassium carbonate and continue stirring for 24 hours; then wash the solution with pure water and vacuum dry to obtain a yellow powder, namely polydiphenylpiperidone-30% styrene. 1 H NMR spectrum as shown Figure 1 (As shown).
[0067] (3) Dissolve 1g of polydiphenylpiperidone-30% styrene polyelectrolyte in 20ml of dimethyl sulfoxide to prepare polydiphenylpiperidone-30% styrene solution, and perform degassing treatment to obtain casting solution;
[0068] (4) Cut a 10x10cm porous polyethylene (PE) membrane (with a porosity of 42% and a thickness of 12μm), immerse it in isopropanol solution for 24h, remove it and lay it flat on a glass plate. Turn on the heating plate to 80℃, drop the prepared poly(biphenylpiperidone)-30% styrene solution onto the porous PE membrane, heat it continuously for 24h and then dry it. Through thermal crosslinking reaction, a polyethylene-poly(biphenylpiperidone)-30% polystyrene (PE-pBP-30%) pore-filled composite membrane is obtained. Immerse PE-pBP-30% in 1mol / L sodium hydroxide aqueous solution for 24 hours, then take it out and wash it repeatedly with pure water to obtain a counterion of OH. - The alkaline anion exchange membrane PE-pBP-30%-OH, as shown in the physical photo. Figure 2 As shown.
[0069] (II) Application of PE-pBP-30%-OH composite membrane in anion exchange membrane water electrolysis for hydrogen production
[0070] The ethylene-polyphenylpiperidone-30% polystyrene (PE-pBP-30%-OH) pore-filled composite membrane prepared in (I) above was characterized structurally.
[0071] (1) SEM cross-sectional characterization
[0072] The prepared PE-pBP-30%-OH was dried in an oven, cut to a certain size, and subjected to liquid nitrogen brittle fracture. The morphology of the polymer cross-section was observed and analyzed using scanning electron microscopy. The results are as follows: Figure 3 As shown, its cross-section exhibits a nearly dense structure.
[0073] (2) Air tightness test
[0074] The hydrogen barrier properties of PE-pBP-30%-OH under different pressures were measured using the constant-pressure-variable-volume method. The prepared composite membrane was assembled in an airtightness testing apparatus, and different gas pressures (e.g., 2 bar-5 bar) were set. After stabilization for 1 hour, gas permeability was recorded and measured using a soap bubble flow meter and a stopwatch. The results are as follows: Figure 4 As shown, the results indicate that the membrane exhibits low hydrogen permeability at different pressures, but it remains intact at 5 bar, with a measured hydrogen permeation flux of 3.7 Barrer.
[0075] (3) Conductivity and alkali resistance tests of PE-pBP-30%-OH composite membrane
[0076] (3.1) OH of the PE-pBP-30%-OH membrane obtained in (a) - Ionic conductivity was detected using the four-electrode AC impedance method, and the hydroxide ion conductivity curve was obtained, as shown in the figure. Figure 5 As shown, the hydroxide ion conductivity of the PE-pBP-30%-OH membrane at 30℃-80℃ is 15-42 mS / cm. -1 .
[0077] (3.2) The alkali resistance test was performed on the OH- ion conductivity of the PE-pBP-30%-OH membrane obtained in (a). Figure 6 As shown in the figure. It can be seen that the OH- ion conductivity of the PE-pBP-30%-OH membrane is stable under 1M sodium hydroxide conditions at 80℃, as shown in the results. Figure 6 As shown.
[0078] (4) Electrolysis performance and stability test of PE-pBP-30%-OH composite membrane
[0079] (4.1) Electrolysis polarization curve tests were performed on the PE-pBP-30%-OH composite membrane obtained in (I). The electrolysis test apparatus was assembled in the following order: electrode plate-gas diffusion layer-catalyst layer-PE-pBP-30%-OH membrane-catalyst layer-gas diffusion layer-electrolysis plate. 1M KOH solution was used as the electrolyte at both electrodes. The apparatus was connected to an electrochemical workstation, and electrolysis polarization curve tests were conducted. The current density at different temperatures was measured to evaluate the electrolysis performance of the PE-pBP-30%-OH composite membrane. The results are as follows: Figure 7 As shown, the results indicate that the composite film can achieve a current density of 1.5 A cm⁻¹ at 80 °C and 2 V. -2 .
[0080] (4.2) The electrolytic stability of the PE-pBP-30%-OH composite membrane obtained in (I) was tested. Following the assembly method shown in (4.1), 1M KOH solution was used as the electrolyte at both electrodes, and the electrolysis was conducted at a constant temperature of 60℃ and a constant current density of 500 mA / cm². -2 Continuous water electrolysis tests were conducted to detect voltage changes and evaluate the water electrolysis stability of the prepared composite membrane. The results are as follows: Figure 8 As shown, the results indicate that at 500mA -2 After 600 hours of water electrolysis testing, the voltage increased by only 0.25mV. -1 It has good stability.
[0081] The above description of the embodiments is only for the purpose of helping to understand the method and core ideas of the present invention. It should be noted that those skilled in the art can make several improvements and modifications to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.
Claims
1. A pore-filled anion exchange membrane, characterized in that, It is prepared by thermal crosslinking reaction of a pretreated polyethylene porous membrane and a biphenylpiperidone-styrene of Formula 1 located in its pores; The above thermal crosslinking reaction is a crosslinking of the olefin side chain in the biphenylpiperidone-styrene shown in Formula 1 and the pretreated polyethylene porous membrane through carbon-carbon double bonds; After thermal cross-linking reaction, a network structure is formed. The cross-linking product with the network structure is tightly bonded to the pretreated polyethylene porous membrane through physical interlocking. The polyethylene porous membrane is pretreated by soaking in an alcohol solvent. Formula 1; Where nx and x are the degree of aggregation, 1≤n≤1000, 0.1≤x / (nx)≤1.
2. The pore-filled anion exchange membrane according to claim 1, characterized in that, The temperature of the thermal crosslinking reaction is 50℃-120℃.
3. The pore-filled anion exchange membrane according to claim 1, characterized in that, The porosity of the pretreated polyethylene porous membrane is 30%-80%; The thickness of the pretreated polyethylene porous membrane is 10-100 μm.
4. The pore-filled anion exchange membrane according to claim 1, characterized in that, The alcohol solvent is selected from one or more of ethanol, methanol, and isopropanol.
5. The method for preparing the pore-filled anion exchange membrane according to any one of claims 1-4, characterized in that, Includes the following steps: (1) Biphenyl, N-methyl-4-piperidone, trifluoromethanesulfonic acid, trifluoroacetic acid and solvent are mixed and reacted in an ice bath to obtain polybiphenylpiperidone; (2) The polyphenylpiperidone, p-chloromethylstyrene obtained in step (1) and solvent are mixed and reacted. After the reaction is completed, iodomethane and potassium carbonate are added to the reaction system and a light-shielding reaction is carried out to obtain polyphenylpiperidone-styrene as shown in Formula 1. (3) The poly(biphenylpiperidone-styrene) shown in Formula 1 is mixed with a solvent and degassed to obtain a casting solution; (4) The casting liquid is added dropwise onto the pretreated polyethylene porous membrane, heated to carry out a thermal crosslinking reaction, and dried to obtain the pore-filled anion exchange membrane according to any one of claims 1-4.
6. The preparation method according to claim 5, characterized in that, The molar ratio of biphenyl and N-methyl-4-piperidone in step (1) is 1:(1.0-1.5). The molar ratio of biphenyl and trifluoromethanesulfonic acid in step (1) is 1:(6-12). The volume ratio of trifluoromethanesulfonic acid to trifluoroacetic acid in step (1) is 1:(0.01-0.1).
7. The preparation method according to claim 5, characterized in that, The molar ratio of p-chloromethylstyrene and polydiphenylpiperidone in step (2) is (0.1-1):
1.
8. The preparation method according to claim 5, characterized in that, The concentration of poly(biphenylpiperidone-styrene) of Formula 1 in the casting solution of step (3) is 2wt%-10wt%.
9. A device for producing hydrogen by electrolysis of water, characterized in that, Includes the pore-filled anion exchange membrane according to any one of claims 1-4 or the pore-filled anion exchange membrane prepared by the preparation method according to any one of claims 5-8.
10. The application of the pore-filled anion exchange membrane according to any one of claims 1-4 or the pore-filled anion exchange membrane prepared by the preparation method according to any one of claims 5-8 in fuel cells and flow batteries.
Citation Information
Patent Citations
Polyarylpiperidine anion exchange membrane and preparation method and application thereof
CN111921566A
Anion exchange polymer as well as preparation method and application thereof
CN113801300A
Novel poly (spirobisindane-aryl piperidinium) copolymer ionomer, anion exchange membrane and preparation method of novel poly (spirobisindane-aryl piperidinium) copolymer ionomer
CN118613526A
Novel highly durable cross-linked poly(aryl piperidinium) copolymer ionomer, anion exchange membrane, and method for manufacturing same
WO2024014848A1