Visible light-induced transparent colored topcoat and method of making the same
By combining a phosphomolybdate/hydroxyethyl cellulose hybrid solution with a graphene-modified silicone-acrylic emulsion, a visible light-transparent colored topcoat is formed, solving the problem of uneven application and resulting in uneven coating, achieving uniformity and environmental friendliness, and improving the durability of the coating.
Patent Information
- Application Number
- CN202411970339.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-30
AI Technical Summary
Existing clear topcoat is colorless and transparent in both wet and dry film states. However, it is prone to uneven application during spraying, roller coating, or troweling, which can lead to color variations. Furthermore, uneven application thickness affects the aesthetic appearance and physical and chemical properties, and also results in VOC emissions.
Using a phosphomolybdate/hydroxyethyl cellulose hybrid solution, graphene-modified silicone-acrylic emulsion, and rheology modifiers, along with a reducing agent, a colored topcoat that is transparent under visible light is formed. The wet film is colored and becomes transparent when dry, avoiding uneven application and eliminating VOC emissions.
It achieves uniform coating that is transparent to visible light during construction, improves the durability and environmental friendliness of the coating, avoids VOC emissions, and solves the appearance problems caused by uneven construction.
Smart Images

Figure CN119684862B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a visible light transparent colored topcoat and its preparation method, which is applied in the field of topcoat production. Background Technology
[0002] With the continuous improvement of people's living standards and the advancement of social development, exterior wall faux stone coatings have emerged as a mainstream product in the real estate facade decoration field due to their rich colors, convenient construction, water-based environmental protection, and lightweight safety. Currently, the exterior wall faux stone coating system consists of: base layer → putty layer → primer layer → intermediate layer → faux stone coating layer → topcoat layer. The topcoat layer, as the first line of defense for the building facade, is constantly exposed to the environment and primarily functions to protect the wall by providing waterproofing, dustproofing, stain prevention, alkali resistance, and UV resistance, thus extending its service life. Therefore, the topcoat coating is an indispensable part of building and home decoration.
[0003] However, most of the topcoat clear coats on the market are applied by spraying and roller coating. Since the topcoat clear coat is colorless and transparent in both wet and dry film states, uneven application often leads to problems such as uneven roller coating (missed coating and overcoating, etc.) resulting in roller marks and mottling, local accumulation and mottling in spraying, and dripping and mottling in repeated application, which directly affect the overall appearance and physical and chemical properties of the facade.
[0004] Faced with the limitations and contradictory performance of the aforementioned products, researchers have implemented a series of improvement measures. For example, Chinese patent CN 116875136B discloses a trowel-applied, multi-colored, specially formulated, self-cleaning, scratch-resistant topcoat and its preparation method. By employing a trowel application method, it not only avoids the risks of missed areas and uneven application but also allows for a thicker coating and a fuller film effect. However, this patented product is still a colorless and transparent topcoat, and the uniformity of the film thickness cannot be controlled during the troweling process, inevitably leading to the accumulation of knife marks and uneven application. Furthermore, the thick trowel application not only fills the pores of the stone-like coating to a flat surface, affecting the textured effect of the stone, but also requires a higher coating weight, resulting in higher costs and time.
[0005] Therefore, it has become an urgent task to provide a visible light transparent colored topcoat that can be applied by roller coating or spraying, is colored in the wet film state and becomes transparent only in the dry film state, which is conducive to uniform coating, has good durability, and is environmentally friendly (the paint itself has no VOCs, and no VOCs are generated during the construction and film formation process). Summary of the Invention
[0006] To overcome the shortcomings of existing clear topcoats that are colorless and transparent in both wet and dry film states, and prone to uneven application and color blooming during spraying, roller coating, or troweling, this invention provides a visible light transparent colored topcoat and its preparation method. It uses a phosphomolybdate / hydroxyethyl cellulose hybrid solution as the color-changing substance, combined with a reducing agent, graphene-modified silicone-acrylic emulsion, and rheology modifier, and is formulated with other preferred components in the system in selected proportions. This method offers advantages such as roller or spray application, a colored wet film state that becomes transparent only in the dry film state, easy uniform coating, excellent durability, and environmental friendliness (the paint itself contains no VOCs, and no VOCs are generated during application and film formation).
[0007] The technical solution of the present invention is as follows:
[0008] A visible light transparent colored topcoat is mainly prepared from the following components in the following mass ratios:
[0009]
[0010] The phosphomolybdate / hydroxyethyl cellulose hybrid solution is an ethylene glycol solution of phosphomolybdate hybrid modified hydroxyethyl cellulose, prepared by the following method:
[0011] (1) A phosphomolybdate ethylene glycol solution was prepared by mixing phosphomolybdate and ethylene glycol at a mass ratio of 15-25:300, and a hydroxyethyl cellulose ethylene glycol solution was prepared by mixing hydroxyethyl cellulose and ethylene glycol at a mass ratio of 5-15:100.
[0012] (2) Then, at 20-23℃, the phosphomolybdate ethylene glycol solution is added dropwise to the hydroxyethyl cellulose ethylene glycol solution at a volume ratio of 1:1-1.2, and the mixture is stirred continuously for at least 2 hours to obtain the phosphomolybdate / hydroxyethyl cellulose hybrid solution.
[0013] The graphene-modified silicone-acrylic emulsion is prepared by emulsion copolymerization using organosilicon prepolymer and butyl acrylate as the main raw materials and graphene as the modifier.
[0014] The visible light transparent colored topcoat of this application uses a phosphomolybdate / hydroxyethyl cellulose hybrid solution as the color-changing substance, combined with a reducing agent, graphene-modified silicone-acrylic emulsion and rheology modifier, and is formulated with other preferred components in the system in the selected proportions. It has the advantages of being able to be applied by roller coating or spraying, being colored in the wet film state and becoming transparent only in the dry film state, which is conducive to uniform coating, and being green and environmentally friendly (the paint itself has no VOCs, and no VOCs are generated during the construction and film formation process). Figure 1 This is a schematic diagram illustrating the visible light transparency mechanism of the colored topcoat in this case. Under the action of a reducing agent, this colored topcoat promotes the transfer of hydrogen electrons from the OH groups in hydroxyethyl cellulose to Mo.6+ It is reduced to Mo 5+ It exhibits a pale blue, translucent, metastable state. Under the influence of visible light and oxygen, interatomic charge migration causes strong absorption, a visible light-induced transparency reaction process resulting from the electron transfer mechanism between hydroxyethyl cellulose and phosphomolybdic acid, which transforms Mo... 5+ Oxidation to Mo 6+ This process transforms the topcoat from a pale blue semi-transparent to a colorless and transparent state. The visible-light transparent colored topcoat in this case is a pale blue semi-transparent state, achieving visible-light oxidation and transparency in visible light and natural air. The coating process is clearly observable during roller or spray application, solving the problem of missed or excessive coatings caused by the colorless transparency of existing clear topcoats, which negatively impacts the film's appearance and physicochemical properties. Furthermore, it generates no VOCs during application and film formation, making it more environmentally friendly to workers and the environment. The system utilizes a graphene-modified silicone-acrylic emulsion, which imparts corrosion and mildew resistance to the colored topcoat. This, combined with the extended waterproof, mildew-proof, and corrosion-resistant properties of the rheology modifiers, eliminates the need for additional corrosion and mildew-proof additives in the formulation, enhancing coating durability and achieving zero VOCs in the system itself. This visible-light transparent colored topcoat fills a market gap and is of great significance to the development of new productivity in the coatings industry.
[0015] The reducing agent is an aqueous solution of stannous chloride with a concentration of 18-22 g / L.
[0016] The preferred reducing agent, stannous chloride, has strong reducing power, capable of reducing most of Mo6+ to Mo5+; secondly, it is readily soluble in water and ethylene glycol, exhibiting good compatibility in this topcoat formulation system and not compromising the stability of the topcoat; thirdly, the stability of the Mo valence state in its solution can be controlled by adjusting the amount added, ensuring that irreversible visible light oxidation to achieve transparency can occur; and fourthly, it is easy to store and transport, and has high safety, making it suitable for large-scale industrial production.
[0017] The rheology modifier is a fluorosilicone-modified urea solution, prepared by the following method:
[0018] Aqueous fluoroalkylsiloxane and polyurea solution with a concentration of 110-120 g / ml are mixed at a mass ratio of 1:3.5-4.5 and placed in a constant temperature water bath at 58-62℃. The mixture is stirred continuously for at least 3 hours, and then cooled to 20-23℃ to obtain fluorosilicone modified urea solution.
[0019] The selected rheology modifier, fluorosilicone-modified urea solution, solves the industry pain point of easy sedimentation in cellulose thickeners. It not only prevents sedimentation but also improves the surface smoothness of the coating, reduces the adhesion of the paint film surface, and has excellent stain resistance.
[0020] The phosphomolybdate is one or any combination of sodium phosphomolybdate or ammonium phosphomolybdate.
[0021] Sodium phosphomolybdate and ammonium phosphomolybdate have better water solubility and environmental friendliness than other phosphomolybdates, making them easier to dissolve and disperse in water-based coatings. The preparation processes of sodium phosphomolybdate and ammonium phosphomolybdate are relatively mature, and their procurement costs are relatively lower, making them suitable for large-scale industrial applications.
[0022] The multifunctional defoamer is a polymer-composite mineral oil-based defoamer, the alkaline pH adjuster is a multifunctional amine auxiliary agent, and the film-forming aid is a dodecyl alcohol ester.
[0023] The preferred multifunctional defoamer combines foam suppression, defoaming, and wetting effects. It simplifies formulation design and manufacturing processes, improves production efficiency, and reduces the cost of purchasing various additives and the storage space required.
[0024] The method for preparing the visible light transparent colored topcoat includes the following steps performed in sequence:
[0025] (1) Add water to the mixer, start the mixer, adjust the speed to 300-500 rpm, and add phosphomolybdate / hydroxyethyl cellulose hybrid solution, multifunctional defoamer and alkaline pH adjuster in sequence while stirring. Then increase the speed to 500-700 rpm and mix thoroughly until completely dissolved.
[0026] (2) Keep the mixer speed at 500-700 rpm, continue to add graphene-modified silicone-acrylic emulsion and film-forming aid, then increase the speed to 800-1000 rpm and continue to disperse until the mixture is uniform to obtain a mixture;
[0027] (3) Keep the mixer speed at 800-1000 rpm, slowly add the reducing agent and rheology modifier, so that the mixture obtained in step (2) gradually changes from a yellow semi-transparent state to a blue semi-transparent state, continue to disperse for 8-10 minutes, and then cool to 20-23℃ to obtain a visible light transparent colored topcoat.
[0028] The preparation method of the visible light transparent colored topcoat is simple and easy to operate.
[0029] Compared with the prior art, this invention application has the following advantages:
[0030] 1) The visible light transparent colored topcoat of this application uses a phosphomolybdate / hydroxyethyl cellulose hybrid solution as the color-changing substance, combined with a reducing agent, graphene-modified silicone-acrylic emulsion and rheology modifier, and is matched with other preferred components in the system in the preferred proportions. It has the advantages of being able to be applied by roller coating or spraying, being colored in the wet film state and becoming transparent only in the dry film state, which is conducive to uniform coating, and being green and environmentally friendly (the paint itself has no VOCs, and no VOCs are generated during the construction and film formation process).
[0031] 2) The addition of the preferred reducing agent improves the system stability, enabling the visible light transparent colored topcoat to be mass-produced industrially.
[0032] 3) The preferred rheology modifier, fluorosilicone-modified urea solution, solves the industry pain point of easy sedimentation of cellulose thickener, which not only plays a role in preventing sedimentation, but also improves the surface smoothness of the coating, reduces the adhesion of the paint film surface, and has excellent stain resistance.
[0033] 4) The preparation method of the visible light transparent colored topcoat is simple and easy to operate. Attached Figure Description
[0034] Figure 1 This is a schematic diagram of the visible light transparent mechanism of the visible light transparent colored topcoat and its preparation method described in this invention.
[0035] Figure 2 Example 2 of the visible light transparent colored topcoat and its preparation method described in this invention is a comparison of the visible light transparent sample effects under different oxygen concentrations.
[0036] Figure 3 This is the Mo3d atomic level XPS spectrum of the visible light transparent colored topcoat and its preparation method described in this invention (where (A) is...). Figure 2 (A) XPS spectrum of the topcoat; (B) for Figure 2 (B) XPS spectrum of the topcoat coating. Detailed Implementation
[0037] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments.
[0038] Example 1
[0039] The visible light transparent colored topcoat of this invention is mainly prepared from the following components in the following mass ratios:
[0040]
[0041] The phosphomolybdate / hydroxyethyl cellulose hybrid solution is an ethylene glycol solution of phosphomolybdate hybrid modified hydroxyethyl cellulose, prepared by the following method:
[0042] (1) A phosphomolybdate ethylene glycol solution was prepared by mixing phosphomolybdate and ethylene glycol at a mass ratio of 20:300, and a hydroxyethyl cellulose ethylene glycol solution was prepared by mixing hydroxyethyl cellulose and ethylene glycol at a mass ratio of 10:100.
[0043] (2) Then, at 21°C, the phosphomolybdate ethylene glycol solution was added dropwise to the hydroxyethyl cellulose ethylene glycol solution at a volume ratio of 1:1, and the mixture was stirred continuously for 2 hours to obtain the phosphomolybdate / hydroxyethyl cellulose hybrid solution.
[0044] The graphene-modified silicone-acrylic emulsion is prepared by emulsion copolymerization using organosilicon prepolymer and butyl acrylate as the main raw materials and graphene as the modifier.
[0045] The reducing agent is an aqueous solution of stannous chloride with a concentration of 20 g / L.
[0046] The rheology modifier is a fluorosilicone-modified urea solution, prepared by the following method:
[0047] Aqueous fluoroalkylsiloxane and a polyurea solution with a concentration of 100 g / ml were mixed at a mass ratio of 1:4 and placed in a constant temperature water bath at 60℃ for 3 hours. The mixture was then cooled to 21℃ to obtain a fluorosilicone modified urea solution.
[0048] The phosphomolybdate is sodium phosphomolybdate.
[0049] The multifunctional defoamer is a polymer-composite mineral oil-based defoamer, the alkaline pH adjuster is a multifunctional amine auxiliary agent, and the film-forming aid is a dodecyl alcohol ester.
[0050] The method for preparing the visible light transparent colored topcoat is characterized by comprising the following steps performed in sequence:
[0051] (1) Add water to the mixer, start the mixer, adjust the speed to 300 rpm, and add the phosphomolybdate / hydroxyethyl cellulose hybrid solution, multifunctional defoamer and alkaline pH adjuster in sequence while stirring. Then increase the speed to 500 rpm and mix thoroughly until completely dissolved.
[0052] (2) Keep the mixer speed at 500 rpm, continue to add graphene-modified silicone-acrylic emulsion and film-forming aid, then increase the speed to 800 rpm and continue to disperse until the mixture is uniform to obtain the mixture;
[0053] (3) Keep the mixer speed at 800 rpm, slowly add the reducing agent and rheology modifier, so that the mixture obtained in step (2) gradually changes from a yellow semi-transparent state to a blue semi-transparent state, continue to disperse for 8 minutes, and then cool to 21°C to obtain a visible light transparent colored topcoat.
[0054] Example 2
[0055] The visible light transparent colored topcoat of this invention is mainly prepared from the following components in the following mass ratios:
[0056]
[0057] The phosphomolybdate / hydroxyethyl cellulose hybrid solution is an ethylene glycol solution of phosphomolybdate hybrid modified hydroxyethyl cellulose, prepared by the following method:
[0058] (1) A phosphomolybdate ethylene glycol solution was prepared by mixing phosphomolybdate and ethylene glycol at a mass ratio of 15:300, and a hydroxyethyl cellulose ethylene glycol solution was prepared by mixing hydroxyethyl cellulose and ethylene glycol at a mass ratio of 15:100.
[0059] (2) Then, at 20°C, the phosphomolybdate ethylene glycol solution was added dropwise to the hydroxyethyl cellulose ethylene glycol solution at a volume ratio of 1:1.1, and the mixture was stirred continuously for 2.5 h to obtain the phosphomolybdate / hydroxyethyl cellulose hybrid solution.
[0060] The graphene-modified silicone-acrylic emulsion is prepared by emulsion copolymerization using organosilicon prepolymer and butyl acrylate as the main raw materials and graphene as the modifier.
[0061] The reducing agent is an aqueous solution of stannous chloride with a concentration of 18 g / L.
[0062] The rheology modifier is a fluorosilicone-modified urea solution, prepared by the following method:
[0063] Aqueous fluoroalkylsiloxane and a polyurea solution with a concentration of 110 g / ml were mixed at a mass ratio of 1:4.5 and placed in a constant temperature water bath at 58℃. The mixture was stirred continuously for 3.5 h, and then cooled to 23℃ to obtain a fluorosilicone modified urea solution.
[0064] The phosphomolybdate is ammonium phosphomolybdate.
[0065] The multifunctional defoamer is a polymer-composite mineral oil-based defoamer, the alkaline pH adjuster is a multifunctional amine auxiliary agent, and the film-forming aid is a dodecyl alcohol ester.
[0066] The method for preparing the visible light transparent colored topcoat includes the following steps performed in sequence:
[0067] (1) Add water to the mixer, start the mixer, adjust the speed to 400 rpm, and add phosphomolybdate / hydroxyethyl cellulose hybrid solution, multifunctional defoamer and alkaline pH adjuster in sequence while stirring. Then increase the speed to 600 rpm and mix thoroughly until completely dissolved.
[0068] (2) Keep the mixer speed at 600 rpm, continue to add graphene-modified silicone-acrylic emulsion and film-forming aid, then increase the speed to 900 rpm and continue to disperse until the mixture is uniform to obtain the mixture;
[0069] (3) Keep the mixer speed at 700 rpm, slowly add the reducing agent and rheology modifier, so that the mixture obtained in step (2) gradually changes from a yellow semi-transparent state to a blue semi-transparent state, continue to disperse for 9 minutes, and then cool to 20°C to obtain a visible light transparent colored topcoat.
[0070] Example 3
[0071] The visible light transparent colored topcoat of this invention is mainly prepared from the following components in the following mass ratios:
[0072]
[0073] The phosphomolybdate / hydroxyethyl cellulose hybrid solution is an ethylene glycol solution of phosphomolybdate hybrid modified hydroxyethyl cellulose, prepared by the following method:
[0074] (1) Phosphomolybdate and ethylene glycol were mixed at a mass ratio of 25:300 to obtain a phosphomolybdate ethylene glycol solution, and hydroxyethyl cellulose and ethylene glycol were mixed at a mass ratio of 5:100 to obtain a hydroxyethyl cellulose ethylene glycol solution.
[0075] (2) Then, at 23°C, the phosphomolybdate ethylene glycol solution was added dropwise to the hydroxyethyl cellulose ethylene glycol solution at a volume ratio of 1:1.2, and the mixture was stirred continuously for 3 hours to obtain the phosphomolybdate / hydroxyethyl cellulose hybrid solution.
[0076] The graphene-modified silicone-acrylic emulsion is prepared by emulsion copolymerization using organosilicon prepolymer and butyl acrylate as the main raw materials and graphene as the modifier.
[0077] The reducing agent is an aqueous solution of stannous chloride with a concentration of 22 g / L.
[0078] The rheology modifier is a fluorosilicone-modified urea solution, prepared by the following method:
[0079] Aqueous fluoroalkylsiloxane and a polyurea solution with a concentration of 120 g / ml were mixed at a mass ratio of 1:3.5 and placed in a constant temperature water bath at 62℃ for 4 hours with continuous stirring. The mixture was then cooled to 20℃ to obtain a fluorosilicone modified urea solution.
[0080] The phosphomolybdate is a combination of sodium phosphomolybdate and ammonium phosphomolybdate.
[0081] The multifunctional defoamer is a polymer-composite mineral oil-based defoamer, the alkaline pH adjuster is a multifunctional amine auxiliary agent, and the film-forming aid is a dodecyl alcohol ester.
[0082] The method for preparing the visible light transparent colored topcoat includes the following steps performed in sequence:
[0083] (1) Add water to the mixer, start the mixer, adjust the speed to 500 rpm, and add phosphomolybdate / hydroxyethyl cellulose hybrid solution, multifunctional defoamer and alkaline pH adjuster in sequence while stirring. Then increase the speed to 500-700 rpm and mix thoroughly until completely dissolved.
[0084] (2) Keep the mixer speed at 700 rpm, continue to add graphene-modified silicone-acrylic emulsion and film-forming aid, then increase the speed to 1000 rpm and continue to disperse until the mixture is uniform to obtain the mixture;
[0085] (3) Keep the mixer speed at 1000 rpm, slowly add the reducing agent and rheology modifier, so that the mixture obtained in step (2) gradually changes from a yellow semi-transparent state to a blue semi-transparent state, continue to disperse for 10 minutes, and then cool to 23°C to obtain a visible light transparent colored topcoat.
[0086] Raw material information involved in each embodiment
[0087] Graphene-modified silicone-acrylic emulsion: SD-5281, Jiangsu Shengda New Material Technology Co., Ltd.;
[0088] Multifunctional defoamer: ST 2410, BASF AG;
[0089] Alkaline pH adjuster: AMP-95, Dow Chemical Company;
[0090] Phosphomolybdate: PMoA, China National Pharmaceutical Group
[0091] Hydroxyethyl cellulose: EBS481 FQ, AkzoNobel
[0092] Ethylene glycol: Xiamen Xinlianfa Import & Export Co., Ltd.
[0093] Film-forming aids: 290Plus, Dow Chemical Company;
[0094] Reducing agent: CAS 7772-99-8, Nanjing Chemical Reagent;
[0095] Polyurea solution: BYK420, BYK Chemicals;
[0096] Waterborne fluoroalkylsiloxanes: SF-334, Guangdong Biaomei Fluorosilicone New Materials Co., Ltd.
[0097] Experimental data:
[0098] Comparative Example 1: The difference between this comparative example and Example 2 is that no reducing agent is added;
[0099] Comparative Example 2: The difference between this comparative example and Example 2 is that ordinary silicone-acrylic emulsion is used instead of the graphene-modified silicone-acrylic emulsion in Example 2;
[0100] Comparative Example 3: The difference between this comparative example and Example 2 is that no rheology modifier is added.
[0101] The various embodiments and comparative examples obtained in this case were analyzed and tested accordingly:
[0102] Testing methods: The performance indicators of the paint were tested in accordance with the standard HG / T 5065-2016 "Topcoat Varnish for Architectural Coatings"; the elemental types, chemical valence states and relative contents of each paint coating were analyzed using an EscaLab 250Xi X-ray photoelectron spectroscopy instrument manufactured by Thermo Fisher Scientific; and the color change of each paint under different oxygen concentrations was tested and analyzed using a self-made visible light oxidation in-situ film formation test device.
[0103] The results are as follows:
[0104] one, Figure 2 This is a comparison of the visible light transparency of the colored topcoat in Example 2 under different oxygen concentrations. The oxygen concentration conditions from left to right are: (A) 0% O2 + 100% N2; (B) 20% O2 + 80% N2; (C) 50% O2 + 50% N2. Figure 2 It can be clearly seen that the colored topcoat does not fade in an oxygen-free environment; when the oxygen concentration reaches 20% or above, the colored topcoat can completely undergo visible light oxidation to become transparent, which indicates that the oxygen concentration in the natural environment is sufficient to cause the colored topcoat to fade to a transparent state.
[0105] II. Mo3d atomic energy levels and Mo 5+ / Mo value analysis
[0106] Figure 3 The image shows the Mo3d atomic level XPS spectrum of the colored topcoat coating in Example 2, where (A) is... Figure 2 (A) XPS spectrum of the topcoat; (B) for Figure 2 (B) XPS spectra of the topcoat. Table 1 shows the binding energy of Mo3d and Mo before and after visible light transparentization. 5+ / Mo value test table.
[0107] Table 1. Binding energy of Mo3d and Mo before and after visible light transparent coating. 5+ / Mo value
[0108]
[0109] Combination Figure 3 As shown in Table 1, Mo under visible light and oxygen-free environment 5+ The 3d characteristic peaks are 231.66 eV and 234.87 eV, Mo 6+ The 3d characteristic peaks of Mo are 232.86 eV and 236.03 eV; under visible light and oxygen-rich conditions, Mo... 5+ The 3d characteristic peaks are 231.83 eV and 235.53 eV, Mo 6+ The 3d characteristic peaks are 233.06 eV and 236.20 eV, indicating that the binding energies of their 3d characteristic peaks changed under visible light in both oxygen-free and oxygen-containing environments, suggesting a change in the chemical environment of the Mo atom. After integration, the area occupied by each peak was calculated, and finally, the Mo... 5+ The ratio of / Mo. Mo dried under visible light and oxygen conditions. 5+ The proportion in Mo decreases, therefore Mo 6+ With the increased proportion of Mo, it is evident that phosphomolybdate / hydroxyethyl cellulose generates a derivative of Mo in the topcoat film. 5+ to Mo 6+ The visible light-transparent oxidation reaction.
[0110] III. Performance Testing of Coatings
[0111] Table 2 Results of various performance tests for coatings
[0112]
[0113] As shown in Table 2, the visible light transparent colored topcoats prepared in Examples 1-3 all meet the various standard requirements of HG / T 5065-2016 "Topcoat Varnish for Architectural Coatings". The topcoat prepared in Comparative Example 1 also meets the above standard requirements, indicating that the addition of reducing agent has little impact on the performance of the topcoat. However, the topcoat prepared in Comparative Example 2 showed the problem of artificial aging and bubble cracking, indicating that graphene-modified silicone-acrylic emulsion can make up for the defect of special additives in topcoat formulations that can shorten service life, thereby giving the coating excellent durability. The topcoat prepared in Comparative Example 3 showed the problem of sedimentation and stratification, indicating that fluorosilicone-modified urea solution, as a rheology modifier, played an anti-settling role in this formulation system.
[0114] IV. Detection of Coating Discoloration under Different Oxygen Concentrations
[0115] Table 3. Coating discoloration under different oxygen concentrations.
[0116] <![CDATA[O2 concentration]]> 0% 5% 15% 20% 30% 50% Example 2 × × √ √ √ √ Comparison 1 × × × × × × Comparison 2 × × × √ √ √
[0117] Where × indicates no color change; √ indicates transparency.
[0118] As shown in Table 3, the visible light transparent colored topcoat prepared in this application is a light blue semi-transparent color. When the oxygen concentration is 15%, the topcoat can change from light blue to transparent. However, Comparative Example 1 (without added reducing agent) did not change color when the oxygen concentration was as high as 50%. This indicates that after the addition of reducing agent, sufficient Mo5+ in the topcoat is ensured to present a light blue semi-transparent metastable state. Furthermore, under the action of visible light, oxygen will oxidize the Mo5+ in the topcoat to Mo6+, thereby fading to a transparent stable state.
[0119] V. In summary, the visible light transparent colored topcoat of this case has the advantages of being able to be applied by roller or spray, being colored in the wet film state and becoming transparent only in the dry film state, which is conducive to uniform coating, having good durability, and being green and environmentally friendly (the paint itself has no VOCs, and no VOCs are generated during the construction and film formation process).
Claims
1. A colored topcoat that is transparent to visible light, characterized in that: It is mainly prepared from the following components in the following mass ratios: 24-36 parts water 3-5 parts of phosphomolybdate / hydroxyethyl cellulose hybrid solution Multi-functional defoamer 0.2-0.4 parts 0.15-0.25 parts of alkaline pH adjuster Graphene-modified silicone-acrylic emulsion, 45-55 parts 4-6 parts of film-forming aid 9-11 parts reducing agent 0.45-0.55 parts of rheology modifier; The phosphomolybdate / hydroxyethyl cellulose hybrid solution is an ethylene glycol solution of phosphomolybdate hybrid modified hydroxyethyl cellulose, prepared by the following method: (1) Phosphomolybdate and ethylene glycol are mixed at a mass ratio of 15-25:300 to obtain a phosphomolybdate ethylene glycol solution, and hydroxyethyl cellulose and ethylene glycol are mixed at a mass ratio of 5-15:100 to obtain a hydroxyethyl cellulose ethylene glycol solution; (2) Then, at 20-23℃, the phosphomolybdate ethylene glycol solution is added dropwise to the hydroxyethyl cellulose ethylene glycol solution at a volume ratio of 1:1-1.2, and the mixture is stirred continuously for at least 2 h to obtain the phosphomolybdate / hydroxyethyl cellulose hybrid solution. The graphene-modified silicone-acrylic emulsion is prepared by emulsion copolymerization using organosilicon prepolymer and butyl acrylate as the main raw materials and graphene as the modifier.
2. The visible light transparent colored topcoat according to claim 1, characterized in that: The reducing agent is an aqueous solution of stannous chloride with a concentration of 18-22 g / L.
3. The visible light transparent colored topcoat according to claim 1, characterized in that: The rheology modifier is a fluorosilicone-modified urea solution, prepared by the following method: Aqueous fluoroalkylsiloxane and polyurea solution BYK420 are mixed at a mass ratio of 1:3.5-4.5 and placed in a constant temperature water bath at 58-62℃. The mixture is stirred continuously for at least 3 hours, and then cooled to 20-23℃ to obtain a fluorosilicone modified urea solution.
4. The visible light transparent colored topcoat according to claim 1, characterized in that: The phosphomolybdate is one or any combination of sodium phosphomolybdate or ammonium phosphomolybdate.
5. The visible light transparent colored topcoat according to claim 1, characterized in that: The multifunctional defoamer is a polymer-composite mineral oil-based defoamer, the alkaline pH adjuster is a multifunctional amine auxiliary agent, and the film-forming aid is a dodecyl alcohol ester.
6. The method for preparing a visible light transparent colored topcoat according to any one of claims 1-5, characterized in that: The steps are as follows, performed in sequence: (1) Add water to the mixer, start the mixer, adjust the speed to 300-500 rpm, and add phosphomolybdate / hydroxyethyl cellulose hybrid solution, multifunctional defoamer and alkaline pH adjuster in sequence while stirring. Then increase the speed to 500-700 rpm and mix thoroughly until completely dissolved. (2) Keep the mixer speed at 500-700 rpm, continue to add graphene-modified silicone-acrylic emulsion and film-forming aid, then increase the speed to 800-1000 rpm and continue to disperse until the mixture is uniform to obtain a mixture; (3) Keep the mixer speed at 800-1000 rpm, slowly add the reducing agent and rheology modifier, so that the mixture obtained in step (2) gradually changes from a yellow semi-transparent state to a blue semi-transparent state, continue to disperse for 8-10 min, and then cool to 20-23℃ to obtain a visible light transparent colored topcoat.
Citation Information
Patent Citations
A scraping type multi-colored special double-sided self-cleaning anti-scratch topcoat varnish and preparation method thereof
CN116875136B
Finish-coat paint for real stone paint and preparation method of finish-coat paint
CN105462411A
Inorganic-organic compound photosensitive color-changing water-based fluorocarbon varnish and preparation method thereof
CN110591468A