Composite separator, preparation and application thereof and zero-gap alkaline water electrolysis device

By in-situ growing layered hydrophilic nanoparticles on a Daramic porous membrane, the problems of low membrane mechanical strength and high gas permeability in zero-gap alkaline water electrolysis were solved, achieving high-efficiency electrolysis performance and improved product purity.

CN119685877BActive Publication Date: 2026-11-24DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311240385.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-25
Publication Date
2026-11-24
Estimated Expiration
2043-09-25

AI Technical Summary

Technical Problem

In existing zero-gap alkaline water electrolysis technology, the diaphragm has low mechanical strength and is easily punctured, and the gas products have high transmembrane permeability, which leads to increased internal resistance of the electrolyzer and reduced product purity.

Method used

In situ growth of layered hydrophilic nanoparticles on Daramic porous membranes enhances membrane mechanical strength and reduces gas permeability. Membrane properties are regulated by controlling the growth amount and morphology of nanoparticles.

Benefits of technology

It improves the mechanical strength and gas barrier capacity of the diaphragm, reduces electrolysis energy consumption, increases electrolysis efficiency and product purity, and broadens the application range of alkaline water electrolysis equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119685877B_ABST
    Figure CN119685877B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of water electrolysis, specifically relating to an alkali-resistant composite membrane material for zero-gap alkaline water electrolysis, its preparation method, and its application. The alkali-resistant composite membrane comprises a porous base membrane and layered inorganic particles grown in situ in the membrane pores and on the membrane surface. The porous base membrane is a commercially available Daramic membrane, and the layered inorganic particles are hydrophilic nanoparticles with good alkali resistance, uniformly grown in the membrane pores and on the membrane surface. The alkali-resistant composite membrane of this invention is low in cost and possesses good mechanical strength and high alkali resistance stability, maintaining a long lifespan even in the high-alkali concentration environment of alkaline water electrolysis (ALKWE). Furthermore, by controlling the structure of the nanoparticles and their growth amount in the membrane pores and on the membrane surface, the gas permeation problem of porous membrane materials can be effectively solved, enabling its application in zero-gap alkaline water electrolyzers. This reduces the electrode spacing on both sides of the membrane, improving electrolysis efficiency while simultaneously enhancing the stability of the electrolyzer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a composite membrane material for zero-gap alkaline water electrolysis, its preparation and application, and particularly to the application of this type of membrane in zero-gap alkaline water electrolysis devices. Background Technology

[0002] In recent years, against the backdrop of global efforts to address climate change and accelerate energy transition, hydrogen, as a clean energy source, holds promise for achieving the global goal of carbon-free energy and addressing the growing global energy shortage and environmental pollution. As an energy carrier with high gravimetric energy density, hydrogen is not only beneficial for large-scale, efficient storage and utilization of other renewable energy sources, but it is also widely used in various industries such as metallurgy, medicine, electronics, and food, becoming an indispensable resource in modern society. Compared to the energy-intensive and polluting chemical steam reforming process for hydrogen production, using electricity to electrolyze water for hydrogen production offers advantages such as high energy efficiency, high product yield, and low environmental pollution. Furthermore, when used in conjunction with green and clean energy power generation, it is expected to achieve zero pollution and zero emissions.

[0003] Among the various water electrolysis methods for hydrogen production, alkaline water electrolysis (ALKWE) is the most mature, offering advantages such as low manufacturing cost, long lifespan, large-scale production, high hydrogen purity, and simple operation. However, in alkaline water electrolyzers, to reduce gas transmembrane permeation, the electrodes need to maintain a certain distance from the membrane. Even a slight increase in electrode spacing leads to a sharp increase in the internal resistance of the electrolyzer. Furthermore, during electrolysis, the product hydrogen and oxygen are directly adsorbed onto the active electrode surface as bubbles, reducing the number of active sites and also increasing the internal resistance of the electrolyzer.

[0004] In response, the technology of "zero-gap alkaline water electrolyzers" has attracted increasing attention. Zero-gap alkaline water electrolyzers are a type of alkaline water electrolysis for hydrogen production. In a zero-gap alkaline water electrolyzer, the anode and cathode electrodes are tightly bonded to both sides of a diaphragm to reduce the electrode spacing. Simultaneously, this design prevents product bubbles from adsorbing onto the active electrode surfaces, thereby significantly reducing the internal resistance of the electrolyzer and improving electrolysis efficiency.

[0005] However, the technology for zero-gap alkaline electrolysis is still immature, and the materials used in traditional alkaline electrolysis cannot be directly applied to zero-gap electrolysis systems. Technological development is still constrained by the following issues: (1) The diaphragm has low mechanical strength. When the metal electrodes are tightly attached to both sides of the diaphragm, the diaphragm is easily punctured, causing a short circuit in the electrolytic cell.

[0006] (2) Increasing the membrane porosity or reducing the membrane thickness can reduce the membrane surface resistance, but it can also easily lead to the permeation of gas products across the membrane and reduce the purity of the products. Summary of the Invention

[0007] To address the aforementioned key technical problems, the present invention aims to provide a zero-gap diaphragm for alkaline water electrolysis, its preparation method, and its applications. This type of diaphragm uniformly grows hydrophilic layered inorganic nanoparticles with good alkali resistance on the pores and surface of a Daramic porous membrane. While reducing membrane surface resistance, the inorganic particles support the membrane pores, enhancing the membrane's mechanical strength. Furthermore, the hydrophilic nanoparticles within the pores and on the membrane surface exhibit high repulsion towards the gaseous products of electrolysis, effectively reducing gas transmembrane permeability, improving product purity, and reducing electrolysis energy consumption.

[0008] The objective of this invention can be achieved through the following technical solutions: 1. The objective of this invention is to provide an alkali-resistant composite membrane for use in a zero-gap alkaline water electrolysis device, wherein the alkali-resistant composite membrane comprises a porous base membrane and hydrophilic nanoparticles grown in situ on the base membrane; wherein the inorganic nanoparticles are uniformly grown in the pores of the base membrane and on the surface of the base membrane.

[0009] In the alkali-resistant composite diaphragm described in this invention, the inorganic nanoparticles are layered hydrophilic particles with excellent alkali resistance and stability. By controlling the amount of particles growing on the base membrane, the mechanical strength, ionic conductivity, and gas barrier properties of the diaphragm can be enhanced, thereby improving both the electrolysis efficiency and stability of the diaphragm.

[0010] 2. The second objective of this invention is to provide a method for preparing the alkali-resistant composite membrane described in the first objective, the method comprising the following steps: (1) Dissolve the inorganic metal salt in ultrapure water to obtain an inorganic metal salt solution; (2) Immerse the cleaned Daramic base membrane in the inorganic metal salt solution from step (1); (3) After adding nitrogen-containing organic matter or ammonium salt to the solution in step (2), a solvothermal reaction is carried out; (4) The composite membrane obtained in step (3) is immersed in potassium hydroxide solution, then washed with solvent and dried to obtain the alkali-resistant porous composite membrane.

[0011] The inorganic metal salt in step (1) is a combination of divalent and trivalent metal salts; the metal ion concentration ratio of divalent and trivalent metal salts is 2:1 or 4:1; wherein, the divalent metal salt is one or two of magnesium salt, cobalt salt, nickel salt, and zinc salt; and the trivalent metal salt is one or two of aluminum salt, iron salt, and chromium salt.

[0012] The inorganic metal salt in step (1) is selected from one of nitrates, sulfates, and chlorides.

[0013] Preferably, the weight percentage of inorganic salt is 10% to 15%, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, etc., but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0014] Preferably, the divalent inorganic metal salt is magnesium nitrate, and the trivalent inorganic metal salt is aluminum nitrate, with the ratio of magnesium nitrate to aluminum nitrate controlled at 2:1.

[0015] In step (2), the thickness of the Daramic base film is between 150 μm and 900 μm, the porosity is between 52% and 70%, and the pore size distribution ranges from 0.001 nm to 600 nm.

[0016] Before immersing the Daramic membrane in the inorganic metal salt solution described in step (1) in step (2), it needs to be cleaned. The cleaning steps are to immerse the Daramic membrane in a mixed solution of ethanol and methanol with a mixing ratio of 2:1 (60 °C, soaking for 3 hours), and then immerse it in ultrapure water (70 °C, soaking for 3 hours), and repeat this process three times.

[0017] In step (2), the solvothermal reaction temperature is 90 ℃~150 ℃ and the reaction time is 24 hours~72 hours. If this range is exceeded, the hydrophilic inorganic particles will not grow completely or the porous base film will be damaged.

[0018] Preferably, the reaction time is 48 hours.

[0019] Preferably, the reaction temperature is 100 ℃ to 110 ℃, for example, it can be 100 ℃, 101 ℃, 102 ℃, 103 ℃, 104 ℃, 105 ℃, 106 ℃, 107 ℃, 108 ℃, 109 ℃, 110 ℃, etc., but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0020] In step (4), the membrane after the solvothermal reaction needs to be soaked in a potassium hydroxide solution; the concentration of the potassium hydroxide solution is 1 mol∙L. -1 ~ 3 mol∙L -1 The soaking temperature is 30℃~50℃, and the soaking time is 48 hours~96 hours.

[0021] Preferably, the potassium hydroxide solution concentration is 3 mol∙L⁻¹ -1 The soaking temperature is 40 ℃ and the soaking time is 96 hours.

[0022] In step (4), the composite membrane soaked in potassium hydroxide solution is thoroughly washed with solvent and dried; the drying temperature is 30 ℃ ~ 60 ℃ and the drying time is 48 hours ~ 96 hours.

[0023] Preferably, the drying temperature is 30 °C.

[0024] 3. The third objective of this invention is to provide an application of the alkali-resistant composite diaphragm mentioned in the first objective above, for the electrolysis of water to produce hydrogen and oxygen. Specifically, it is a zero-gap alkali water electrolysis device.

[0025] The zero-gap alkaline water electrolysis device comprises a cathode end plate, a porous cathode gas diffusion electrode (GDE-cathode), the alkali-resistant composite diaphragm described in the first purpose, a felt anode gas diffusion electrode (GDE-anode), and an anode end plate arranged in sequence; wherein the porous cathode gas diffusion electrode and the felt anode gas diffusion electrode are respectively hot-pressed on both sides of the alkali-resistant composite diaphragm.

[0026] Optionally, the cathode end plate material is one of high-purity graphite plate, N4 high-purity nickel plate, TA2 titanium plate and 904L stainless steel plate; the anode end plate material is one of N4 high-purity nickel plate with a 2 μm platinum layer on the surface, TA2 titanium plate with a 2 μm platinum layer on the surface, 904L stainless steel plate with a 2 μm platinum layer on the surface and Hastelloy C276 with a 2 μm platinum layer on the surface.

[0027] The porous cathode gas diffusion electrode is made of nickel foam with a nickel-based catalyst sprayed on its surface; the felt anode gas diffusion electrode is a titanium felt with a 50 nm ~ 2 μm platinum layer on its surface.

[0028] Preferably, the porous cathode gas diffusion electrode has a nickel foam with a porosity of 96% and a thickness of 0.32 mm to 0.4 mm, and the catalyst is Raney nickel; the felt anode gas diffusion electrode has a platinum coating thickness of 2 μm, a titanium felt thickness of 250 μm, and a porosity of 50% to 60%.

[0029] In the zero-gap alkaline water electrolysis device, the porous cathode gas diffusion electrode and the felt anode gas diffusion electrode are respectively hot-pressed onto both sides of the alkali-resistant composite membrane.

[0030] Preferably, the hot-pressing temperature is 140 ℃ and the hot-pressing time is 40 seconds.

[0031] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0032] The alkali-resistant composite membrane of this invention comprises a porous base membrane and two-dimensional layered inorganic particles grown in situ in the membrane pores and on the membrane surface. The porous base membrane is a commercially available Daramic membrane, and the layered inorganic particles are hydrophilic nanoparticles with good alkali resistance, uniformly grown in the membrane pores and on the membrane surface. The alkali-resistant composite membrane of this invention is low in cost and possesses good mechanical strength and high alkali resistance stability, maintaining a long lifespan even in the high alkali concentration environment required for alkaline water electrolysis (ALKWE). Furthermore, by controlling the structure of the nanoparticles and their growth amount in the membrane pores and on the membrane surface, the gas permeation problem of porous membrane materials can be effectively solved, enabling its application in zero-gap alkaline water electrolyzers. This reduces the electrode spacing on both sides of the membrane, improving electrolysis efficiency while simultaneously enhancing the stability of the electrolyzer.

[0033] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention is the first to realize the in-situ growth of two-dimensional hydrophilic nanoparticles in Daramic porous membrane. By controlling the reaction conditions, the growth amount and morphology of the particles in the membrane can be controlled, thereby achieving the regulation of the properties of the composite membrane.

[0034] (2) The Daramic membrane used in this invention is low in cost and highly stable, and can be commercially purchased; the raw materials of hydrophilic nanoparticles are inexpensive, and the growth process of the particles is controllable, with high alkali resistance and stability, strong interaction with the base membrane, and not easy to fall off; the composite membrane preparation process is simple, meets the needs of large-scale application, and shows good application prospects.

[0035] (3) This invention is the first to realize the preparation of a composite membrane with good alkali resistance using Daramic membrane as a substrate, and the first to apply it to an alkaline water electrolysis device. The related alkaline water electrolysis device exhibits excellent stability, which broadens the selection range of alkali-resistant membranes for alkaline water electrolysis.

[0036] (4) The present invention utilizes layered nanoparticles to support the porous structure of the Daramic membrane, thereby improving the mechanical strength of the Daramic membrane-based porous composite membrane.

[0037] (5) The present invention utilizes hydrophilic nanoparticles to enhance the gas barrier ability of porous membranes, enabling them to be used in zero-gap alkaline water electrolyzers to prevent hydrogen and oxygen from crossing the membrane between the cathode and anode, thereby improving the purity of hydrogen in the product. Attached Figure Description

[0038] Figure 1 Microscopic morphology of the alkali-resistant composite membrane prepared in Example 1, and the corresponding elemental distribution; Figure 2 Magnified microstructure of the alkali-resistant composite diaphragm prepared in Example 1; Figure 2 'a' represents a magnification of 8000 times. Figure 2b represents a magnification of 30,000 times; Figure 3 Thermogravimetric analysis results of the alkali-resistant composite membrane and Daramic porous base membrane prepared in Example 1; Figure 4 Comparison of mechanical strength between the alkali-resistant composite membrane and the Daramic porous base membrane prepared in Example 1; Figure 5 A schematic diagram of an example of the zero-gap alkaline water electrolysis device of the present invention; in the figure, the reference numerals are: 1 is the cathode end plate; 2 is the diaphragm; 3 is the anode end plate; 4 is the cathode gas diffusion electrode; and 5 is the anode diffusion electrode. Detailed Implementation

[0039] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0040] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0041] Example 1 Preparation process of alkali-resistant composite membrane: (1) A. A commercially available Daramic porous membrane (membrane area 5cm*5cm) with a thickness of 180 μm, a pore size distribution range of 0.001 nm ~ 600 nm, and a porosity of 60% was immersed in a mixed solution of ethanol and methanol with a volume ratio of 2:1. The immersion temperature was 60 ℃ and the immersion time was 3 hours. B. Subsequently, the Daramic porous membrane was immersed in ultrapure water at a temperature of 70 ℃ and the immersion time was 3 hours.

[0042] Repeat steps A and B three times to obtain a cleaned Daramic porous base membrane.

[0043] (2) Preparation of inorganic metal salt solution: Dissolve 0.06 mol magnesium nitrate and 0.03 mol aluminum nitrate in 60 mL of ultrapure water. After the inorganic salt is completely dissolved, immerse the cleaned Daramic porous membrane in the inorganic salt solution at 60 °C for 10 hours. After the solution cools to room temperature, add 0.42 mol urea to the solution and sonicate for 1 hour to allow the nanoparticle precursor to fully penetrate into the porous structure of the Daramic membrane.

[0044] (3) The Daramic membrane with precursor in the pores in step (2) and the urea soaking solution are transferred to a stainless steel high-pressure reactor (100 mL) with a polytetrafluoroethylene (Teflon) liner and subjected to a solvothermal reaction at 110 °C for 48 hours.

[0045] (4) After the solvothermal reaction is completed, the resulting composite membrane is immersed in 3 mol·L⁻¹ water.-1 The membrane was immersed in potassium hydroxide solution at 40 °C for 96 hours. Subsequently, the composite membrane was cleaned with an ethanol-water solution (volume concentration 1:4) and dried at 50 °C for 72 hours to obtain the Daramic-based alkali-resistant composite membrane.

[0046] The microstructure of the alkali-resistant composite diaphragm was observed using scanning electron microscopy. Figure 1 The alkali-resistant composite membrane has a thickness of 170 μm, which is less than the thickness of the Daramic base membrane (180 μm), indicating that the Daramic-based composite membrane prepared using the composite membrane preparation method of this invention will be thinner. Elemental analysis clearly shows that hydrophilic layered nanoparticles are uniformly dispersed within the membrane. Magnification of the scanning electron microscope reveals that the inorganic nanoparticles have a two-dimensional layered structure (the lamellar plates of a single lamellar cell are 0.5 nm * 0.5 nm ~ 1.5 nm * 1.5 nm; the thickness of a single lamellar cell is 5 ~ 30 nm), growing uniformly within and on the membrane surface, with a particle size of 10 ~ 50 nanometers. Figure 2 'a' represents a magnification of 8000 times. Figure 2 (b represents a magnification of 30,000 times). The thermal stability of the membrane was analyzed using a thermogravimetric analyzer. Figure 3 The film exhibits thermal stability at 200 °C. Figure 4 Mechanical strength tests were conducted on the diaphragms, and the results showed that the alkali-resistant composite diaphragm had greater tensile strength and lower elongation at break than the Daramic porous base membrane. The alkali-resistant composite diaphragm was immersed in 6 mol∙L⁻¹ water. -1 The alkali resistance stability of the membrane was analyzed by periodically measuring the percentage of membrane mass loss (the percentage of membrane mass lost relative to the initial weight before soaking in the alkali solution) using potassium hydroxide solution (80 °C). The results showed that the composite membrane remained stable for 500 hours (Table 1). Gas barrier properties of the membrane were tested using a gas diffuser. The results showed that the commercially available Daramic membrane had poor gas barrier properties; even under zero pressure difference, gases could cross-flow between the membrane and its sides. In contrast, the alkali-resistant composite membrane with grown layered nanoparticles exhibited less than one-thousandth gas cross-flow under a pressure difference of 0.05 MPa, demonstrating that the composite membrane with grown layered particles possessed better gas barrier properties.

[0047] Table 1

[0048] The prepared alkali-resistant composite diaphragm was installed into a zero-gap alkaline water electrolysis device: First, a porous cathode gas diffusion electrode (with Raney nickel foam sprayed on its surface, wherein the area of ​​the foamed nickel is 2*2cm) was installed. 2 It has a porosity of 96%, a thickness of 0.4 mm, and a Raney nickel content of 1.5 mg / cm³. 2;) and felt-like anode gas diffusion electrode (plated with platinum-titanium felt, wherein the platinum plating thickness is 2μm, the titanium felt thickness is 250 μm, and the area is 2*2cm). 2 The membrane (with a porosity of 60%) was hot-pressed onto both sides of the alkali-resistant composite membrane (hot-pressing pressure: 2 MPa, temperature: 140 ℃, hot-pressing time: 40 seconds, membrane area: 4*4 cm). 2 ).

[0049] Then, the cathode end plate (TA2 titanium plate), porous cathode gas diffusion electrode, Daramic-based alkali-resistant composite diaphragm, felt anode gas diffusion electrode, and anode end plate (TA2 titanium plate with platinum plating on the side closest to the porous anode gas diffusion electrode, the platinum plating layer being 2 μm) are tightly stacked and connected together to assemble a gapless electrolysis device. Subsequently, 6 mol∙L⁻¹ is introduced into the electrolysis device through the end plate. -1 The electrolytic performance of potassium hydroxide solution (flow rate 10 mL / min) at 80 °C was tested. The electrolytic performance was as follows: at an electrolytic voltage of 1.8 V, the current density was 750 mA∙cm⁻¹. -2 .

[0050] Comparative Example 1

[0051] The process and conditions were the same as in Example 1, except that after cleaning the Daramy porous membrane according to step (1) of Example 1, it was directly transferred into a 100 mL stainless steel high-pressure reactor with a Teflon liner. 60 mL of ultrapure water was added to the reactor, and the reactor was maintained at 110 °C for 72 hours. After completion, the Daramy porous membrane was removed. The resulting membrane was then processed according to step (4) of Example 1 to obtain control membrane 1. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and conducting the tests were the same as in Example 1.

[0052] Comparative Example 2

[0053] The process and conditions were the same as in Example 1, except that after completing steps (1) and (2), the Daramic porous membrane soaked in a mixed solution of magnesium nitrate and aluminum nitrate and the urea-containing soaking solution were transferred into a stainless steel high-pressure reactor (100 mL) with a polytetrafluoroethylene (Teflon) liner and maintained at 30 °C for 72 hours. Subsequently, the membrane was removed, cleaned with an ethanol aqueous solution, and the membrane treatment was completed according to step (4) in Example 1 to obtain control membrane 2. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and testing were the same as in Example 1.

[0054] Comparative Example 3

[0055] The process and conditions are the same as in Example 1, except that after cleaning the Daramic porous membrane according to step (1) in Example 1, the membrane is directly immersed in 3 mol·L⁻¹ water. -1 The composite membrane was immersed in potassium hydroxide solution at 40 °C for 96 hours. Afterward, it was cleaned with an ethanol-water solution to obtain control membrane 3. The remaining procedures for assembling the membranes into the zero-gap alkaline electrolysis apparatus and conducting the tests were the same as in Example 1.

[0056] Comparative Example 4

[0057] The process and conditions were the same as in Example 1, except that after cleaning the Daramic porous membrane according to step (1) in Example 1, no other operations were performed, and the control membrane 4 was obtained directly. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and conducting the tests were the same as in Example 1.

[0058] Comparative Example 5

[0059] The process and conditions were the same as in Example 1, except that after completing steps (1) and (2) according to the operating method of Example 1, the Daramic porous membrane soaked in a mixed solution of magnesium nitrate and aluminum nitrate and the soaking solution were transferred into a stainless steel high-pressure reactor (100 mL) with a polytetrafluoroethylene (Teflon) liner. Urea was not added; instead, the membrane was directly subjected to a solvothermal reaction at 110 °C for 72 hours. Subsequently, the membrane was removed, cleaned with an ethanol aqueous solution, and the membrane treatment was completed according to step (4) in Example 1 to obtain control membrane 5. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and testing were the same as in Example 1.

[0060] Example 2

[0061] The process and conditions are the same as in Example 1, except that after cleaning the Daramic porous membrane according to step (1) in Example 1, the membrane is immersed in 60 mL of 1 mol·L⁻¹ solution. -1 l magnesium chloride and 0.5 mol∙L -1 The membrane was immersed in a mixed aqueous solution of aluminum chloride at a temperature of 60 °C for 10 hours. The Daramic porous membrane was then removed and treated according to steps (3) and (4) of Example 1 to obtain control membrane 6. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and conducting the tests were the same as in Example 1.

[0062] Comparative Example 6

[0063] The process and conditions were the same as in Example 1, except that after completing steps (1) and (2) according to the operating method of Example 1, the Daramic porous membrane soaked in a mixed solution of magnesium nitrate and aluminum nitrate and the urea-containing soaking solution were transferred into a stainless steel high-pressure reactor (100 mL) with a polytetrafluoroethylene (Teflon) liner, and subjected to a solvothermal reaction at 140 °C for 72 hours. After the reaction was completed, the membrane was removed, cleaned with an ethanol aqueous solution, and the membrane treatment was completed according to step (4) in Example 1 to obtain control membrane 7. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and testing were the same as in Example 1.

[0064] Comparative Example 7

[0065] The process and conditions were the same as in Example 1, except that after completing steps (1) and (2) according to the operating method of Example 1, the Daramic porous membrane soaked in a mixed solution of magnesium nitrate and aluminum nitrate and the urea-containing soaking solution were transferred into a stainless steel high-pressure reactor (100 mL) with a polytetrafluoroethylene (Teflon) liner, and subjected to a solvothermal reaction at 110°C for 24 hours. After the reaction was completed, the membrane was removed, cleaned with an ethanol aqueous solution, and the membrane treatment was completed according to step (4) in Example 1 to obtain control membrane 8. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and testing were the same as in Example 1.

[0066] Comparative Example 8

[0067] The process and conditions were the same as in Example 1, except that after completing steps (1) and (2) according to the operating method of Example 1, the Daramic porous membrane soaked in a mixed solution of magnesium nitrate and aluminum nitrate and the urea-containing soaking solution were transferred into a stainless steel high-pressure reactor (100 mL) with a polytetrafluoroethylene (Teflon) liner, and subjected to a solvothermal reaction at 140 °C for 24 hours. After the reaction was completed, the membrane was removed, cleaned with an ethanol aqueous solution, and the membrane treatment was completed according to step (4) in Example 1 to obtain control membrane 9. The remaining procedures for assembling the membrane into the zero-gap alkaline electrolysis device and testing were the same as in Example 1.

[0068] Comparative Example 9

[0069] The process and conditions are the same as in Example 1, except that after completing steps (1), (2), and (3) according to the operation method of Example 1, the membrane prepared by the solvothermal reaction is obtained, cleaned with an ethanol aqueous solution, and dried to obtain the control membrane 10. The rest of the operation method for assembling the membrane into the zero-gap alkaline electrolysis device and testing is the same as in Example 1.

[0070] Comparative Example 10

[0071] The process and conditions are the same as in Example 1, except that the alkali-resistant composite diaphragm is prepared according to the method described in Example 1. The prepared alkali-resistant composite diaphragm is directly assembled into the zero-gap water electrolysis device, except that the composite diaphragm is not hot-pressed to the gas diffusion electrodes of the cathode and anode before being installed. The remaining operations are the same as in Example 1.

[0072] Comparative Example 11

[0073] The process and conditions were the same as in Example 1, except that an alkali-resistant composite diaphragm was prepared according to the operating method of Example 1. Subsequently, the prepared alkali-resistant composite diaphragm was hot-pressed with the gas diffusion electrodes on both the cathode and anode sides. The hot-pressing pressure was 10 MPa, the temperature was 140 °C, and the hot-pressing time was 40 seconds. After hot-pressing, the zero-gap alkaline water electrolysis device was assembled according to Example 1, and the remaining operations were the same as in Example 1.

[0074] Comparative Example 12

[0075] The process and conditions were the same as in Example 1, except that an alkali-resistant composite diaphragm was prepared according to the operating method of Example 1. Subsequently, the prepared alkali-resistant composite diaphragm was hot-pressed with the gas diffusion electrodes on both the cathode and anode sides. The hot-pressing pressure was 2 MPa, the temperature was 140 °C, and the hot-pressing time was 3 minutes. After hot-pressing, the zero-gap alkaline water electrolysis device was assembled according to Example 1, and the remaining operations were the same as in Example 1.

[0076] Comparative Example 13

[0077] Following the procedure in Example 1, an alkali-resistant composite diaphragm was prepared. Subsequently, the prepared alkali-resistant composite diaphragm was hot-pressed with the gas diffusion electrodes on both the cathode and anode sides. The hot-pressing pressure was 2 MPa, the temperature was 30 °C, and the hot-pressing time was 40 seconds. After hot-pressing, the zero-gap alkaline water electrolysis device was assembled according to Example 1, with the remaining operating procedures and conditions being the same as in Example 1.

[0078] Comparative Example 14

[0079] The process and conditions are the same as in Example 1, except that an alkali-resistant composite diaphragm is prepared according to the operating method of Example 1. Subsequently, the prepared alkali-resistant composite diaphragm is hot-pressed with the gas diffusion electrodes on both the cathode and anode sides at a pressure of 2 MPa, a temperature of 140 °C, and a pressing time of 40 seconds. After hot pressing, the electrolysis device is assembled in the following order: cathode end plate (TA2 titanium plate), porous cathode gas diffusion electrode, the alkali-resistant composite diaphragm, felt anode gas diffusion electrode, and anode end plate (TA2 titanium plate with a platinum plating layer of 2 μm). The remaining operating procedures and conditions are the same as in Example 1.

[0080] Example 3

[0081] The process and conditions are the same as in Example 1, except that an alkali-resistant composite diaphragm is prepared according to the operating method of Example 1. Subsequently, the prepared alkali-resistant composite diaphragm is hot-pressed with the gas diffusion electrodes on both the cathode and anode sides at a pressure of 2 MPa, a temperature of 140 °C, and a pressing time of 40 seconds. After hot pressing, the electrolysis device is assembled in the following order: cathode end plate (high-purity graphite plate), porous cathode gas diffusion electrode, the alkali-resistant composite diaphragm, felt anode gas diffusion electrode, and anode end plate (TA2 titanium plate with a platinum coating of 2 μm). The remaining operating procedures and conditions are the same as in Example 1.

[0082] Example 4 The process and conditions are the same as in Example 1, except that an alkali-resistant composite diaphragm is prepared according to the operating method of Example 1. Subsequently, the prepared alkali-resistant composite diaphragm is hot-pressed with the gas diffusion electrodes on both the cathode and anode sides at a pressure of 2 MPa, a temperature of 140 °C, and a pressing time of 40 seconds. After hot pressing, the electrolysis apparatus is assembled in the following order: cathode end plate (N4 high-purity nickel plate), porous cathode gas diffusion electrode, the alkali-resistant composite diaphragm, felt anode gas diffusion electrode, and anode end plate (TA2 titanium plate with a 2 μm platinum coating). The remaining operating procedures and conditions are the same as in Example 1.

[0083] Example 5 The process and conditions are the same as in Example 1, except that an alkali-resistant composite diaphragm is prepared according to the operating method of Example 1. Subsequently, the prepared alkali-resistant composite diaphragm is hot-pressed with the gas diffusion electrodes on both the cathode and anode sides at a pressure of 2 MPa, a temperature of 140 °C, and a pressing time of 40 seconds. After hot pressing, the electrolysis apparatus is assembled in the following order: cathode end plate (TA2 titanium plate), porous cathode gas diffusion electrode, the alkali-resistant composite diaphragm, felt anode gas diffusion electrode, and anode end plate (N4 high-purity nickel plate with a platinum plating layer of 2 μm). The remaining operating procedures and conditions are the same as in Example 1.

[0084] The alkali-resistant composite diaphragm and the zero-gap alkaline water electrolysis device were tested: (1) The membrane surface resistance of the membranes obtained in the above embodiments and comparative examples was tested. The test method is as follows: The sheet resistivity of the membrane was tested in an H-type electrolytic cell (Tianjin Aida Hengsheng H-type electrolytic cell CH2001-S), and the resistance was calculated based on the slope of the IV curve. The resistances of assembled electrolytic cells with and without membranes were measured separately, and the difference between the two was used to calculate the membrane resistance. R A =A×(R1-R2) Where R A R1 is the surface resistance; A is the effective area of ​​the membrane; R1 and R2 are the resistances of the electrolytic cell with and without the membrane, respectively.

[0085] The membrane surface resistance test results of the diaphragms obtained in the above embodiments and comparative examples are listed in Table 2.

[0086] (2) The membranes obtained in the above embodiments and comparative examples were subjected to water electrolysis performance tests. The test methods are as follows: The assembled zero-gap alkaline water electrolysis device was circulated with 6 mol·L⁻¹ water. -1 A potassium hydroxide solution was used to maintain the apparatus temperature at 80 °C. The electrolytic voltage applied to the cathode and anode was increased from 1 V to 2 V at a rate of 20 mV·min. -1 The current density during voltage changes was measured.

[0087] The water electrolysis performance test results of the diaphragms obtained in the above embodiments and comparative examples are listed in Table 2 (current density corresponding to 1.8 V).

[0088] Table 2

[0089] The following points can be determined from Table (2): (1) As can be seen from Example 1, the alkali-resistant organic composite membrane obtained by the present invention has a small membrane surface resistance and a high ion conductivity. When assembled into the corresponding zero-gap alkaline water electrolysis device, it has good electrolysis performance.

[0090] (2) By comparing Examples 1, 2, 1, 2, 3, 4, and 5, it can be seen that the hydrophilic nanoparticles in the composite membrane can enhance the membrane stability, and the inorganic nano-ionic precursors of nitrate and chloride have little effect on the performance of the composite membrane. However, the membrane without the growth of inorganic nanoparticles has lower electrolytic performance in the electrolysis device. This is because without the support of nanoparticles, the internal pore structure of the membrane will collapse in concentrated alkali, resulting in an increase in the sheet resistance of the membrane. In addition, the membranes in Comparative Examples 2 and 5 contain inorganic salt precursors, which, although they do not have a significant impact on the sheet resistance of the membrane, will poison the catalyst in the electrolysis device, thus reducing the electrolytic performance.

[0091] (3) Comparing Example 1, Comparative Example 6, Comparative Example 7, and Comparative Example 8, it can be seen that changing the solvothermal reaction temperature and duration will affect the growth state of particles in the membrane. In Comparative Example 6, due to the excessively high reaction temperature, the particles in the membrane were severely stacked, resulting in an increase in the membrane surface resistance and a decrease in electrolysis efficiency; while in Comparative Example 7, the reaction time was too short, resulting in insufficient particle growth, causing the membrane to collapse rapidly in the alkali and its stability to deteriorate.

[0092] (4) Comparing Examples 3, 4, 5, and Comparative Example 14, it can be seen that the end plate material is closely related to the water electrolysis performance. When the anode end plate is changed to titanium without platinum plating, it will oxidize into titanium oxide at high potential, increasing the end plate resistance and causing a decrease in electrolysis performance; while changing the platinum-plated titanium plate to a platinum-plated nickel plate does not have a significant impact on performance. For the cathode end plate, nickel plate, titanium plate, and graphite plate have little impact on performance.

Claims

1. A method for preparing a composite diaphragm, characterized in that, The composite membrane comprises a Daramic porous base membrane and inorganic nanoparticles grown in situ on the base membrane; wherein the inorganic nanoparticles are metal hydroxides with a layered structure, and are grown in situ in the pores and on the surface of the base membrane; the process includes the following steps: (1) An inorganic metal salt is dissolved in water to obtain an inorganic metal salt solution; the inorganic metal salt in the inorganic metal salt solution is a combination of divalent and trivalent metal salts; the metal ion concentration ratio of divalent and trivalent metal salts in the inorganic metal salt solution is 2:1 to 4:1; the inorganic divalent metal salt is a magnesium salt; the inorganic trivalent metal salt is an aluminum salt; (2) Immerse the Daramic porous base membrane in the inorganic metal salt solution from step (1); (3) After adding nitrogen-containing organic matter to the solution in step (2), sonicate or stir for 0.5 to 2 hours to carry out a solvothermal reaction. The nitrogen-containing organic matter is urea. (4) The composite membrane obtained in step (3) is immersed in an alkaline solution of sodium hydroxide and / or potassium hydroxide with a pH value greater than or equal to 12, and then washed with solvent and dried to obtain the composite membrane.

2. The preparation method according to claim 1, characterized in that, The particle size of inorganic particles is 10 nm to 50 nm; The layered structure is a two-dimensional sheet structure, with the sheet plates of a single sheet cell being 0.5 nm × 0.5 nm ~ 1.5 nm × 1.5 nm; the thickness of a single sheet cell is 5 ~ 30 nm.

3. The preparation method according to claim 1, characterized in that, The thickness of a single lamellar cell is 15 ~ 20 nm.

4. The preparation method according to claim 1, characterized in that, The inorganic metal salt is one or more of the following: metal nitrates, sulfates, and chlorides; The soaking temperature in step (2) is 50~80 ℃, and the soaking time is 8~48 hours; the membrane area is (3cm* 3 cm) ~ (6cm *6cm), the molar concentration of the inorganic metal salt solution is 1 mol / L ~ 3 mol / L; After step (3), the molar concentration of the nitrogen-containing organic compound in the solution is 6 mol / L ~ 9 mol / L. The solvothermal reaction temperature is 90 ℃~110 ℃, and the reaction time is 48 hours~72 hours.

5. The preparation method according to claim 4, characterized in that, In step (1), the ratio of the concentrations of divalent and trivalent metal ions in the inorganic metal salt solution is 3-4:

1. Step (2) The molar concentration of the inorganic metal salt solution is 1.5 ~ 1.8 mol / L; After step (3), the molar concentration of the nitrogen-containing organic compound in the solution is 7 mol / L; The solvothermal reaction temperature was 100 °C, and the reaction time was 72 hours.

6. The preparation method according to claim 1, characterized in that, Before immersing the Daramic base membrane in the inorganic metal salt solution of step (1) in step (2), the Daramic porous base membrane is cleaned. The cleaning method is as follows: 1) Immerse the Daramic substrate membrane in an organic solvent composed of ethanol and methanol; wherein the volume ratio of ethanol to methanol is 1:2 to 2:1; the immersion time is 3 to 6 hours, and the immersion temperature is 30 to 70 ℃. 2) Take out the Daramic base membrane from step 1) and immerse it in water; the immersion time is 3 to 6 hours and the immersion temperature is 30 to 70 ℃; 3) Repeat steps 1) to 2) 0-4 times; In step (4), the composite membrane obtained by the solvothermal reaction in step (3) is immersed in sodium hydroxide and / or potassium hydroxide with a pH value greater than or equal to 12, the immersion temperature is 30 ℃~ 50 ℃, and the immersion time is 48 hours~ 96 hours; In step (4), the composite membrane that has been soaked in alkaline solution is washed with a solvent, and the cleaning solvent is an ethanol aqueous solution with a volume concentration of 1:3 to 1:

5. In step (4), the cleaned composite membrane is dried at a temperature of 30 ℃ to 60 ℃ for a duration of 48 hours to 96 hours.

7. The preparation method according to claim 6, characterized in that, Step 3) Repeat steps 1)~2) 2-3 times. In step (4), the composite membrane obtained by the solvothermal reaction in step (3) is immersed in sodium hydroxide and / or potassium hydroxide with a pH of 12~14, the immersion temperature is 40 ℃, and the immersion time is 96 hours.

8. The application of a composite separator prepared by the method of any one of claims 1 to 2, characterized in that, The composite diaphragm is used in the processes of electrolyzing alkaline water to produce hydrogen and oxygen.

9. A zero-gap alkaline water electrolysis device, characterized in that, The zero-gap alkaline water electrolysis device comprises a cathode end plate, a porous cathode gas diffusion electrode, a composite membrane prepared by the method of preparing the composite membrane according to any one of claims 1 to 3, a felt anode gas diffusion electrode, and an anode end plate arranged in sequence; wherein the porous cathode gas diffusion electrode and the felt anode gas diffusion electrode are respectively hot-pressed on both sides of the composite membrane prepared by the method of preparing the composite membrane according to any one of claims 1 to 3.

10. The zero-gap alkaline water electrolysis device according to claim 9, characterized in that, The cathode end plate material is one of the following: high-purity graphite plate, N4 high-purity nickel plate, TA2 titanium plate, and 904L stainless steel plate; The anode end plate material is one of the following: N4 high-purity nickel plate with a 1-3 μm platinum layer on the surface near the felt-shaped anode gas diffusion electrode; TA2 titanium plate with a 1-3 μm platinum layer on the surface near the felt-shaped anode gas diffusion electrode; 904L stainless steel plate with a 1-3 μm platinum layer on the surface near the felt-shaped anode gas diffusion electrode; and Hastelloy C276 with a 1-3 μm platinum layer on the surface near the felt-shaped anode gas diffusion electrode. The porous cathode gas diffusion electrode is coated with a layer of 1~3 mg / cm³. 2 The nickel-based catalyst is made of foamed nickel; the nickel-based catalyst is one or more of Raney nickel, nickel sulfide, NiMo alloy or NiAl; The porosity of the nickel foam is 95% ~ 98%, and the thickness is 0.32 mm ~ 0.4 mm; The felt-like anode gas diffusion electrode is a titanium felt coated with metallic platinum; the thickness of the metallic platinum coating is 50 nm ~ 2 μm; the thickness of the titanium felt is 100 μm ~ 300 μm; and the porosity of the titanium felt is 40% ~ 80%.

11. The zero-gap alkaline water electrolysis device according to claim 9 or 10, characterized in that, The cathode gas diffusion electrode and the anode gas diffusion electrode are hot-pressed on both sides of the composite diaphragm prepared by the preparation method described in any one of claims 1-3; the hot-pressing temperature is 100 ℃~140 ℃, and the hot-pressing time is 10 seconds~1 minute; The alkaline solution used for electrolysis is an aqueous solution of potassium hydroxide or sodium hydroxide with a concentration of 0.5 mol / L to 10 mol / L.

Citation Information

Patent Citations

  • Hydrotalcite in-situ growth composite membrane, and preparation method and application thereof

    CN112928322A

  • Organic-inorganic composite membrane as well as preparation method and application thereof

    CN114181426A

  • Composite membrane as well as preparation method and application thereof

    CN114614039A

  • Zero-gap alkaline water electrolysis hydrogen production electrolytic bath device

    CN116411297A

  • Porous composite membrane, preparation method thereof and application of porous composite membrane in alkaline zinc-based flow battery

    CN118136873A