Highly transparent rare earth ultraviolet shielding material, preparation method and application thereof
By preparing porous polyetherimide-coated rare earth silicates and highly transparent rare earth shielding materials, the problem of strong hiding power and low transparency of inorganic ultraviolet shielding agents on textiles was solved, achieving strong ultraviolet shielding and heat insulation effects under high transparency, and improving the stability and ultraviolet protection performance of the materials.
Patent Information
- Application Number
- CN202510026044.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-01-08
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-01-08
AI Technical Summary
When existing inorganic UV shielding agents are used on textiles, they have problems such as strong hiding power, high UV transmittance, and unstable physicochemical properties, making it difficult to maintain high transparency and high UV protection performance.
A primer and topcoat are prepared by coating rare earth silicate materials and highly transparent rare earth shielding materials with porous polyetherimide, and by ball milling, calcination and spray drying. Combining the characteristics of rare earth elements, a coating with microporous structure and hollow nanoparticles is formed to enhance the ultraviolet absorption and reflection performance.
It achieves strong UV shielding with high transparency, reduces fabric surface temperature, improves weather resistance and physicochemical stability, and maintains the original color of the fabric.
Smart Images

Figure CN119708938B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional materials, and in particular relates to a highly transparent rare earth ultraviolet shielding material, its preparation method, and its application. Background Technology
[0002] The Earth is constantly exposed to sunlight, and the solar spectrum includes infrared, visible, and ultraviolet light. Ultraviolet light travels from the sun through the atmosphere to the Earth's surface. The intensity of ultraviolet radiation varies depending on altitude, ozone layer concentration, and weather conditions, with higher intensity in summer and at high altitudes. Appropriate ultraviolet radiation can promote metabolism, enhance calcium absorption, and has antibacterial and anti-mite effects. However, rapid industrialization and frequent human activities in recent years have had a severe impact on the environment. Nitrogen oxides from industrial waste and vehicle exhaust, as well as gases like Freon used in daily life, have depleted the ozone layer (the ultraviolet absorption and protection layer), weakening its protective effect and making the ultraviolet radiation reaching the Earth's surface stronger. Prolonged exposure to ultraviolet radiation can cause irreversible damage to the human body and objects. Therefore, strengthening ultraviolet protection in daily life is extremely important for our health and safety. UV-protective clothing can effectively reduce damage to outdoor personnel, especially in summer when ultraviolet radiation is strong, at the beach, and in certain special working environments. Research on textiles with excellent UV resistance is urgently needed.
[0003] Currently, UV-resistant textiles primarily acquire their UV protection properties through finishing techniques, a process involving the application of functional auxiliaries to the fabric. These auxiliaries are generally classified into two main categories: organic UV shielding agents and inorganic UV shielding agents. Compared to organic types, inorganic UV shielding agents are preferred due to their higher safety, stability, and wider UV absorption range.
[0004] Common inorganic UV shielding agents include titanium dioxide (TiO2), cerium dioxide (CeO2), and zinc oxide (ZnO). However, a drawback of these materials is that their strong blocking ability can alter the original color of the fabric. Therefore, it is crucial to develop a novel inorganic UV shielding material that can maintain high transparency, withstand high temperatures, exhibit strong stability, and have a broad UV absorption range. Summary of the Invention
[0005] In view of this, the present invention aims to propose a highly transparent rare earth ultraviolet shielding material, its preparation method and application, in order to solve the problems of strong UV-resistant component coverage, high UV transmittance and unstable physicochemical properties in the prior art.
[0006] To achieve the above objectives, the technical solution of the present invention is implemented as follows:
[0007] A highly transparent rare-earth ultraviolet shielding material, comprising a primer and a topcoat;
[0008] The primer comprises the following components in parts by weight: 20-50 parts of porous polyetherimide-coated rare earth silicate material, 10-50 parts of first waterborne resin, 0.1-5 parts of first pre-dispersant, 1-10 parts of first additive, and 10-30 parts of deionized water.
[0009] The topcoat comprises the following components in parts by weight: 20-50 parts of high-transparency rare earth shielding material, 10-50 parts of second water-based resin, 0.1-5 parts of second pre-dispersant, 1-10 parts of second additive, and 10-30 parts of deionized water.
[0010] Among them, rare earth silicates are (La a Y b Sm c Dy d )2Si2O7, 0<a,b,c,d<1, a+b+c+d=1; the highly transparent rare earth shielding material is La m Ce n Y x Al2B2SiO8(OH)2,0 <m,n,x<0.67,m+n+x=0.67。
[0011] Furthermore, the porous polyetherimide-coated rare earth silicate material is prepared by the following method:
[0012] 1) Weigh out rare earth oxides and silicon dioxide, mix them evenly in proportion, and then add deionized water to mix;
[0013] 2) Load the prepared material from step 1) into a ball mill for ball milling. After the process is complete, remove the material, dry it, and obtain the rare earth silicate precursor.
[0014] 3) Place the rare earth silicate precursor obtained in step 2) in a tube furnace and calcine it to obtain rare earth silicate (La). a Y b Sm c Dy d )2Si2O7;
[0015] 4) Grind the rare earth silicate obtained in step 3);
[0016] 5) Dissolve the polyetherimide particles in N-methylpyrrolidone to obtain a transparent, dark yellow polyetherimide solution;
[0017] 6) Weigh out the rare earth silicate and polyetherimide solution, mix them evenly and then stir ultrasonically. After the reaction is complete, centrifuge and dry to obtain porous polyetherimide-coated rare earth silicate material.
[0018] Furthermore, in step 2), the ball milling speed is 300-600 r / min, the ball milling reaction is carried out for 12-18 h, and the drying is carried out at 60-80℃ for 8-12 hours;
[0019] In step 3), the calcination temperature is 1200-1500℃ and the calcination time is 3-6 hours;
[0020] In step 4), the particle size after grinding is 500-800 nm;
[0021] In step 5), the dissolution temperature of the polyetherimide particles is 50-70℃;
[0022] In step 6), ultrasonic stirring is performed for 20-60 minutes, and the drying temperature is 60-80℃.
[0023] Furthermore, in step 1), the molar ratio of rare earth oxides to silicon oxide is 1:2;
[0024] Rare earth oxides are a mixture of lanthanum oxide, yttrium oxide, dysprosium oxide, and samarium oxide;
[0025] In step 6), the ingredients include 50-70 parts of rare earth silicate and 30-50 parts of polyether imide solution by weight.
[0026] Furthermore, the highly transparent rare-earth shielding material is prepared by the following method:
[0027] 1) Weigh boric acid, silicon dioxide, rare earth oxides, and aluminum oxide and put them into a ball mill jar, then add deionized water and mix.
[0028] 2) Load the prepared material from step 1) into a ball mill for ball milling;
[0029] 3) The ball-milled material from step 2) is filtered, washed, and dried to obtain La. m Ce n Y x Al2B2SiO8(OH)2 powder was then placed in a tube furnace and calcined to obtain blocky La. m Ce n Y x Al2B2SiO8(OH)2;
[0030] 4) Add deionized water to the material obtained in step 3), and then add blocky La. m Ce n Y x A high-transparency rare earth shielding material slurry can be obtained by grinding 1-8% of Al2B2SiO8(OH)2 as a grinding dispersant until the particle size is ≤100nm.
[0031] 5) The highly transparent rare earth shielding material slurry obtained in step 4) is dried into nano-sized powder by spray drying.
[0032] Further, in step 1), the molar ratio of boric acid:silicon oxide:aluminum oxide:rare earth oxide is 1:1:1:0.67; the rare earth oxide is a mixture of lanthanum oxide, cerium oxide, and yttrium oxide.
[0033] In step 2), the ball milling speed is 300-800 r / min, and the ball milling time is 8-16 hours;
[0034] In step 3), the drying temperature is 60-80℃, the calcination temperature is 400-600℃, and the calcination time is 3-6 minutes.
[0035] In step 4), the grinding and dispersing agent is fatty acid polyethylene glycol ester;
[0036] Step 5) The powder obtained after spray drying has a particle size of 400-600 nm.
[0037] Furthermore, both the first waterborne resin and the second waterborne resin are selected from one or more of acrylic resin, polyurethane resin, pure acrylic emulsion, and silicone-modified acrylic emulsion.
[0038] Both the first predispersant and the second predispersant are selected from one or more of BYK-2013, BYK-190, sodium hexametaphosphate, sodium pyrophosphate, and polyvinyl alcohol;
[0039] Both the first and second additives are selected from one or more of the following: wetting agents, thickeners, leveling agents, defoamers, antisettling agents, and film-forming aids.
[0040] The present invention also provides a method for preparing a highly transparent rare-earth ultraviolet shielding material as described above, the method comprising the following steps:
[0041] 1) Preparation of primer coating
[0042] 1.1) Weigh the first aqueous resin, the first predispersant, and deionized water, and stir and disperse for 60-90 minutes;
[0043] 1.2) Add porous polyetherimide-coated rare earth silicate material to step 1.1) and stir and disperse for 60-90 minutes, then add the first additive and continue stirring for 10-30 minutes to obtain the primer coating.
[0044] 2) Preparation of surface coating
[0045] 2.1) Weigh the second aqueous resin, the second predispersant, and deionized water, and stir and disperse for 60-90 minutes;
[0046] 2.2) Add the highly transparent rare earth shielding material to step 2.1) and stir and disperse for 60-90 minutes. Then add the second additive and continue stirring for 10-30 minutes to obtain the topcoat.
[0047] The present invention also provides an application of the high-transparency rare earth ultraviolet shielding material as described above in the fields of home textiles, outdoor products, clothing fabrics and industrial textiles. In application, the primer is scraped onto the surface of the fabric and cured at 130-150℃ for 3-5 minutes to complete the primer coating; the topcoat is scraped onto the surface of the primer and cured at 130-150℃ for 3-5 minutes to complete the topcoat coating.
[0048] Furthermore, the basis weight of the primer coating is 40-55 g / m². 2 The basis weight of the coating and topcoat should be maintained at 15-25 g / m². 2 between.
[0049] Compared with existing technologies, the high-transparency rare-earth ultraviolet shielding material and its preparation method described in this invention have the following advantages:
[0050] (1) The high-transparency rare earth ultraviolet shielding material described in this invention has excellent selective shielding properties for light. The material has strong absorption capacity in the 280-400nm wavelength band and transmittance ≤1%, while the transmittance for visible light and near-infrared light remains basically unchanged. Applying it to the surface of fabric can not only prevent ultraviolet rays and resist aging, but also ensure that the original fabric color is not affected.
[0051] (2) The present invention prepares a porous polyetherimide-coated rare earth silicate material by surface modification. As a heat insulation material, it has a unique microporous particle structure that couples multiple scattering and surface phonon polarons. When coated on the fabric surface, the coating has a solar reflectivity of 91% and an emissivity of 96% in the 8-14μm band. It can effectively block and radiate solar radiation heat, thereby reducing the temperature of the fabric surface and the bottom of the fabric.
[0052] (3) The present invention uses a spray drying process to prepare a highly transparent rare earth shielding material with hollow nano-sized powder. When the material is formulated into a coating and applied to the surface of a fabric, a static air layer is formed between the nano-powders, which greatly reduces the thermal conductivity of the coating and thus effectively prevents heat conduction.
[0053] (4) The highly transparent rare earth shielding material and the porous polyetherimide-coated rare earth silicate material prepared by this invention are both obtained by high-temperature calcination and have stable physical and chemical properties. The coating fabric prepared in this way has strong weather resistance and is not easy to decompose. Attached Figure Description
[0054] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:
[0055] Figure 1 SEM image of the UV-protective heat-insulating coating fabric prepared in Example 1;
[0056] Figure 2 La, a highly transparent rare-earth shielding material prepared in Example 1 0.67 / 3 Ce 0.67 / 3 Y 0.67 / 3 SEM image of Al2B2SiO8(OH)2. Detailed Implementation
[0057] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.
[0058] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0059] Example 1: High Transparency Rare Earth Ultraviolet Shielding Material and its Preparation
[0060] A highly transparent rare-earth ultraviolet shielding material, comprising a primer and a topcoat;
[0061] The primer comprises the following components in parts by weight: 30 parts of porous polyetherimide-coated rare earth silicate material, 15 parts of acrylic resin, 15 parts of waterborne polyurethane resin, 2 parts of BYK-2013, 2 parts of thickener, 2 parts of film-forming aid, 2 parts of wetting agent, 2 parts of defoamer, and 30 parts of deionized water.
[0062] The topcoat comprises the following components in parts by weight: 20 parts of high-transparency rare earth shielding material, 40 parts of water-based acrylic resin, 3 parts of sodium hexametaphosphate, 2 parts of anti-settling agent, 2 parts of film-forming aid, 1 part of wetting agent, 1 part of defoamer, 1 part of leveling agent, and 30 parts of deionized water.
[0063] The porous polyetherimide-coated rare earth silicate material is prepared by the following method:
[0064] 1) Weigh out lanthanum oxide, yttrium oxide, samarium oxide, dysprosium oxide and silicon oxide according to a molar ratio of 0.25:0.25:0.25:0.25:2, mix them evenly, and then add deionized water to make the solid content 50%.
[0065] 2) The material prepared in step 1) is loaded into a ball mill and ball-milled at a speed of 500 r / min for 15 h. After the reaction is completed, the material is taken out and dried at 70°C for 12 h to obtain rare earth silicate precursor.
[0066] 3) Place the rare earth silicate precursor obtained in step 2) in a tube furnace and calcine it at 1450℃ for 5 hours to obtain rare earth silicate (La). 0.25 Y 0.25 Sm 0.25 Dy 0.25 )2Si2O7;
[0067] 4) Grind the rare earth silicate obtained in step 3) to a particle size of 500-800 nm;
[0068] 5) Dissolve polyetherimide particles in N-methylpyrrolidone at 60°C to obtain a transparent, dark yellow polyetherimide solution;
[0069] 6) Weigh out 60 parts of rare earth silicate (La) 0.25 Y 0.25 Sm 0.25 Dy 0.25 )2Si2O7 and 40 parts of polyetherimide solution were mixed evenly and then ultrasonically stirred for 40 minutes. After the reaction was completed, the mixture was centrifuged and then dried at 70°C and 60% relative humidity for 12 hours to obtain porous polyetherimide-coated rare earth silicate material.
[0070] The highly transparent rare-earth shielding material is prepared by the following method:
[0071] 1) Weigh lanthanum oxide, cerium oxide, yttrium oxide, boric acid, silicon oxide, and aluminum oxide in a molar ratio of 0.67 / 3:0.67 / 3:0.67 / 3:1:1:1 and place them in a ball mill jar, adding an appropriate amount of deionized water; 2) Load the materials prepared in step 1) into a ball mill and ball mill them at a speed of 700 r / min for 15 hours;
[0072] 3) The ball-milled material from step 2) is filtered, washed, and dried at 60°C to obtain La. 0.67 / 3 Ce 0.67 / 3 Y 0.67 / 3Al2B2SiO8(OH)2 powder was then placed in a tube furnace and calcined at 600℃ for 5 hours to obtain blocky La. 0.67 / 3 Ce 0.67 / 3Y 0.67 / 3 Al2B2SiO8(OH)2;
[0073] 4) Add deionized water to the material obtained in step 3) to make the solid content reach 50%, and then add blocky La. 0.67 / 3 Ce0.67 / 3 Y 0.67 / 3 A high-transparency rare earth shielding material slurry can be obtained by grinding Al2B2SiO8(OH)2 with 5% by mass of fatty acid polyethylene glycol ester as a grinding dispersant until the particle size is ≤100nm.
[0074] 5) The highly transparent rare earth shielding material slurry obtained in step 4) is spray-dried into nano-sized powder with a particle size ≤500nm.
[0075] like Figure 2 La, a highly transparent rare earth shielding material 0.67 / 3 Ce 0.67 / 3 Y 0.67 / 3 The SEM image of Al2B2SiO8(OH)2 shows that La 0.67 / 3 Ce 0.67 / 3 Y 0.67 / 3 Al2B2SiO8(OH)2 is a type of nanoparticle with a hollow structure.
[0076] The preparation method of the above-mentioned highly transparent rare-earth ultraviolet shielding material includes the following steps:
[0077] 1) Preparation of primer coating
[0078] 1.1) Weigh 15 parts of acrylic resin, 15 parts of waterborne polyurethane resin, 2 parts of BYK-2013 and 30 parts of deionized water and stir and disperse for 80 min;
[0079] 1.2) Add 30 parts of porous polyetherimide-coated rare earth silicate material to step 1.1) and stir and disperse for 80 minutes. Then add 2 parts of thickener, 2 parts of film-forming aid, 2 parts of wetting agent and 2 parts of defoamer and continue stirring for 30 minutes to obtain the primer coating.
[0080] 2) Preparation of surface coating
[0081] 2.1) Weigh 40 parts of water-based acrylic resin, 3 parts of sodium hexametaphosphate and 30 parts of deionized water and stir and disperse for 80 minutes;
[0082] 2.2) Add 20 parts of high-transparency rare earth shielding material to step 2.1) and stir and disperse for 80 minutes. Then add 2 parts of anti-settling agent, 2 parts of film-forming agent, 1 part of wetting agent, 1 part of defoamer and 1 part of leveling agent and continue stirring for 30 minutes to obtain the topcoat.
[0083] In application, the primer is applied to the fabric surface and cured at 140℃ for 5 minutes to complete the primer coating. The topcoat is then applied to the primer surface and cured at 140℃ for 5 minutes to complete the topcoat coating, thus completing the preparation of the UV-protective heat-insulating coating fabric. The weight gain of the primer coating is 50 g / m². 2The increase in the weight of the topcoat is 20 g / m². 2 .
[0084] like Figure 1 SEM image of the prepared UV-protective heat-insulating coating fabric.
[0085] Example 2
[0086] Based on Example 1 above, the molar ratio of lanthanum oxide, yttrium oxide, samarium oxide, dysprosium oxide, and silicon oxide in the preparation of porous polyetherimide-coated rare earth silicate material was 0.20:0.30:0.28:0.22:2, resulting in a rare earth silicate (La... 0.20 Y 0.30 Sm 0.28 Dy 0.22 )2Si2O7;
[0087] The molar ratio of lanthanum oxide, cerium oxide, yttrium oxide, boric acid, silicon oxide, and aluminum oxide in the preparation of a highly transparent rare-earth shielding material was 0.15:0.35:0.17:2:1:2. The resulting highly transparent rare-earth shielding material was La. 0.15 Ce 0.35 Y 0.17 Al2B2SiO8(OH)2.
[0088] Example 3
[0089] Based on Example 1 above, the molar ratio of lanthanum oxide, yttrium oxide, samarium oxide, dysprosium oxide, and silicon oxide in the preparation of porous polyetherimide-coated rare earth silicate material was 0.10:0.40:0.15:0.35:2, resulting in a rare earth silicate (La... 0.10 Y 0.40 Sm 0.15 Dy 0.35 )2Si2O7;
[0090] The molar ratio of lanthanum oxide, cerium oxide, yttrium oxide, boric acid, silicon oxide, and aluminum oxide in the preparation of a highly transparent rare-earth shielding material was 0.25:0.15:0.27:2:1:2. The resulting highly transparent rare-earth shielding material was La... 0.25 Ce 0.15 Y 0.27 Al2B2SiO8(OH)2.
[0091] Example 4
[0092] Based on the above Example 1, the primer comprises the following components in parts by weight: 40 parts of porous polyetherimide-coated rare earth silicate material, 15 parts of acrylic resin, 15 parts of waterborne polyurethane resin, 3 parts of BYK-2013, 4 parts of thickener, 2 parts of film-forming aid, 1 part of wetting agent, 1 part of defoamer, and 19 parts of deionized water.
[0093] The coating material comprises the following components in parts by weight: 21 parts of high-transparency rare earth shielding material, 45 parts of water-based acrylic resin, 3 parts of sodium hexametaphosphate, 1 part of anti-settling agent, 3 parts of thickener, 2 parts of film-forming aid, 1 part of wetting agent, 1 part of defoamer, 1 part of leveling agent, and 25 parts of deionized water.
[0094] Example 5
[0095] Based on Example 1 above, both the first aqueous resin and the second aqueous resin are silicone-modified acrylic emulsions.
[0096] Comparative Example 1
[0097] The difference from Example 1 is that the heat-insulating component, porous polyetherimide-coated rare-earth silicate material, and the UV-protective component, highly transparent rare-earth shielding material, were not added. The specific preparation steps are as follows:
[0098] 1) Preparation of primer coating
[0099] 1.1) Weigh 22.5 parts of acrylic resin, 22.5 parts of waterborne polyurethane resin, 2 parts of BYK-2013 and 45 parts of deionized water and stir and disperse for 80 min;
[0100] 1.2) Add 2 parts thickener, 2 parts film-forming aid, 2 parts wetting agent and 2 parts defoamer to step 1.1) and continue stirring for 30 minutes to obtain the primer coating.
[0101] 2) Preparation of surface coating
[0102] 2.1) Weigh 50 parts of water-based acrylic resin, 3 parts of sodium hexametaphosphate and 40 parts of deionized water and stir and disperse for 80 minutes;
[0103] 2.2) Add 2 parts of anti-settling agent, 2 parts of film-forming aid, 1 part of wetting agent, 1 part of defoamer and 1 part of leveling agent to step 2.1) and continue stirring for 30 minutes to obtain the topcoat.
[0104] Comparative Example 2
[0105] The difference from Example 1 is that the heat-insulating component porous polyetherimide-coated rare earth silicate material was not added to the primer, while the topcoat formulation remained unchanged.
[0106] Preparation of primer:
[0107] 1) Weigh 22.5 parts of acrylic resin, 22.5 parts of waterborne polyurethane resin, 2 parts of BYK-2013 and 45 parts of deionized water and stir and disperse for 80 min;
[0108] 2) Add 2 parts thickener, 2 parts film-forming aid, 2 parts wetting agent and 2 parts defoamer to step 1) and continue stirring for 30 minutes to obtain the primer coating.
[0109] Comparative Example 3
[0110] The difference from Example 1 is that the primer formulation remains unchanged, but the topcoat does not contain UV-protective components or highly transparent rare earth shielding materials.
[0111] Preparation of topcoat:
[0112] 1) Weigh 50 parts of water-based acrylic resin, 3 parts of sodium hexametaphosphate and 40 parts of deionized water and stir and disperse for 80 minutes;
[0113] 2) Add 2 parts anti-settling agent, 2 parts film-forming aid, 1 part wetting agent, 1 part defoamer and 1 part leveling agent to step 1) and continue stirring for 30 minutes to obtain the topcoat.
[0114] Comparative Example 4
[0115] The difference from Example 1 is that the rare earth silicate prepared in the primer is not coated with porous polyetherimide, and the rare earth silicate material is obtained after calcination and grinding, while the topcoat formulation remains unchanged.
[0116] Comparative Example 5
[0117] The difference from Example 1 is that the UV-protective component in the topcoat, the highly transparent rare-earth shielding material, is La obtained directly by oven drying in step 3). 0.67 / 3 Ce 0.67 / 3 Y 0.67 / 3 Al2B2SiO8(OH)2 is no longer subjected to calcination and spray drying, and the primer remains unchanged.
[0118] Comparative Example 6
[0119] The difference from Example 1 is that the rare earth oxides in the porous polyetherimide-coated rare earth silicate material are lanthanum oxide, yttrium oxide, and samarium oxide, and the molar ratio of lanthanum oxide, yttrium oxide, samarium oxide, and silicon oxide is 1 / 3:1 / 3:1 / 3:2, while the topcoat remains unchanged.
[0120] Comparative Example 7
[0121] The difference from Example 1 is that the rare earth oxides in the porous polyetherimide-coated rare earth silicate material are lanthanum oxide, yttrium oxide, and dysprosium oxide, and the molar ratio of lanthanum oxide, yttrium oxide, dysprosium oxide, and silicon oxide is 1 / 3:1 / 3:1 / 3:2, while the topcoat remains unchanged.
[0122] Comparative Example 8
[0123] The difference from Example 1 is that the rare earth oxides in the porous polyetherimide-coated rare earth silicate material are lanthanum oxide, samarium oxide, and dysprosium oxide, and the molar ratio of lanthanum oxide, samarium oxide, dysprosium oxide, and silicon oxide is 1 / 3:1 / 3:1 / 3:2, while the topcoat remains unchanged.
[0124] Comparative Example 9
[0125] The difference from Example 1 is that the molar ratio of lanthanum oxide, yttrium oxide, samarium oxide, dysprosium oxide and silicon oxide in the porous polyetherimide-coated rare earth silicate material is 1:1:1:1:1.
[0126] Comparative Example 10
[0127] The difference from Example 1 is that the rare earth oxides in the high-transparency rare earth shielding material are lanthanum oxide and cerium oxide, and the molar ratio of lanthanum oxide, cerium oxide, boric acid, silicon oxide and aluminum oxide is 0.67 / 2:0.67 / 2:1:1:1, while the primer coating remains unchanged.
[0128] Comparative Example 11
[0129] The difference from Example 1 is that the rare earth oxides in the high-transparency rare earth shielding material are lanthanum oxide and yttrium oxide, and the molar ratio of lanthanum oxide, yttrium oxide, boric acid, silicon oxide and aluminum oxide is 0.67 / 2:0.67 / 2:1:1:1, while the primer coating remains unchanged.
[0130] Comparative Example 12
[0131] The difference from Example 1 is that the rare earth oxides in the high-transparency rare earth shielding material are cerium oxide and yttrium oxide, and the molar ratio of cerium oxide, yttrium oxide, boric acid, silicon oxide and aluminum oxide is 0.67 / 2:0.67 / 2:1:1:1, while the primer coating remains unchanged.
[0132] Comparative Example 13
[0133] The difference from Example 1 is that the molar ratio of lanthanum oxide, cerium oxide, yttrium oxide, boric acid, silicon oxide and aluminum oxide in the high-transparency rare earth shielding material is 1:1:1:1:1:1, while the primer coating remains unchanged.
[0134] The UV-resistant heat-insulating coated fabrics prepared in Examples 1-5 and Comparative Examples 1-13 were tested for reflectivity, emissivity, heat shielding rate, UV transmittance, and UPF value. The results are shown in Table 1.
[0135] Table 1. Comparison of performance indicators between Examples 1-5 and Comparative Examples 1-12
[0136]
[0137]
[0138] As shown in Table 1, the UV-resistant and heat-insulating coated fabrics prepared using Examples 1-5 have a UPF value greater than 400, a UV transmittance of less than 1%, and a heat-blocking rate of greater than 45%, exhibiting excellent UV protection and heat-blocking functions.
[0139] A comparison of Example 1 and Comparative Examples 1-3 shows that adding porous polyetherimide-coated rare earth silicate material and highly transparent rare earth shielding material to the primer and topcoat, respectively, can effectively improve the UV protection and heat shielding effects of the fabric.
[0140] As shown in Comparative Example 4, if the heat-insulating component in the primer is only rare earth silicate (La... 0.25 Y 0.25 Sm 0.25 Dy 0.25 )2Si2O7, without porous polyetherimide coating on the surface, still has a certain heat-shielding effect, but the heat-shielding performance is reduced. This indicates that the microporous structure on the material surface can couple multiple scattering and surface phonon polarons, improve the fabric's solar reflection and emissivity in the 8-14μm band, effectively block solar radiation heat, and thus reduce the temperature of the fabric surface and inside the fabric.
[0141] As shown in Comparative Example 5, the high-transparency rare earth shielding material prepared by simple drying and pulverization has a larger size. Under the same addition amount, the UV shielding material coverage on the fabric surface is low, which leads to high UV transmittance and a corresponding decrease in UPF value.
[0142] A comparison of Example 1 and Comparative Examples 6-8 shows that only by adding rare earth elements to the porous polyetherimide-coated rare earth silicate material according to the scheme of this application can the reflectivity, emissivity, and heat-shielding effect of the coating fabric be improved. This is because different rare earth ions have different responses to specific wavelengths of light. Therefore, by reasonably combining multiple rare earth elements, the material can reflect a wider range of spectra, thereby improving the overall reflectivity. Secondly, each rare earth element usually has its characteristic emission wavelength. By combining different rare earth elements, emission light covering a wider spectral range can be obtained. Thirdly, the presence of multiple rare earth elements in rare earth silicates will form a more complex crystal structure and grain boundaries, which helps to increase phonon scattering, thereby reducing the thermal conductivity of the material and exhibiting better heat insulation performance. In addition, different rare earth elements in multi-element rare earth silicates may introduce more types of defects or impurities, which can hinder the propagation of heat flow, increase the thermal resistance of the material, and thus improve the heat insulation effect.
[0143] By comparing Example 1 with Comparative Examples 10-12, it can be seen that only by adding rare earth elements to the highly transparent rare earth shielding material according to the scheme of this application can the UV protection effect of the fabric be improved. This is because different rare earth elements have different absorption bands of ultraviolet rays. By mixing multiple rare earth elements, a wider range of ultraviolet rays can be absorbed, including UVA (long-wave ultraviolet rays), UVB (medium-wave ultraviolet rays), and even some UVC (short-wave ultraviolet rays), thus providing more comprehensive ultraviolet protection. In addition, different rare earth elements in multi-element rare earth silicates may produce synergistic effects. In addition to improving ultraviolet absorption, they may also improve other properties, such as increasing the material's anti-aging properties, improving wear resistance, or enhancing color stability.
[0144] A comparison of Example 1 and Comparative Example 9 shows that an excessively high proportion of rare earth elements also reduces the reflectivity, emissivity, and heat-shielding properties of the fabric. This is mainly because an excessive amount of rare earth elements may increase the chemical reactivity of the material, especially in high-temperature or humid environments. This may cause the material to react with other substances (such as moisture or oxygen in the air), thereby affecting its thermal insulation performance.
[0145] As can be seen from the comparison between Example 1 and Comparative Example 13, changing the content of rare earth elements also reduces the UV protection of the fabric. This is mainly because if the proportion of rare earth elements is too high or too low, it may change the absorption band of the material, thereby affecting its absorption efficiency for specific wavelengths of ultraviolet light, resulting in uneven UV protection performance and poor UV protection effect. In addition, if the element ratio is unbalanced, it may reduce the photostability of the raw materials, making the material more prone to degradation under long-term ultraviolet irradiation, thereby affecting its long-lasting UV protection performance.
[0146] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A highly transparent rare-earth ultraviolet shielding material, characterized in that: Includes primer and topcoat; The primer comprises the following components in parts by weight: 20-50 parts of porous polyetherimide-coated rare earth silicate material, 10-50 parts of first waterborne resin, 0.1-5 parts of first pre-dispersant, 1-10 parts of first additive, and 10-30 parts of deionized water. The topcoat comprises the following components in parts by weight: 20-50 parts of high-transparency rare earth shielding material, 10-50 parts of second water-based resin, 0.1-5 parts of second pre-dispersant, 1-10 parts of second additive, and 10-30 parts of deionized water. Among them, rare earth silicates are (La a Y b Sm c Dy d )2Si2O7, 0<a,b,c,d<1, a+b+c+d=1; the highly transparent rare earth shielding material is La m Ce n Y x Al2B2SiO8(OH)2,0 <m,n,x<0.67,m+n+x=0.67; Porous polyetherimide-coated rare earth silicate materials are prepared by the following method: 1) Weigh out rare earth oxides and silicon dioxide, mix them evenly in the specified proportions, and then add deionized water to mix. 2) Load the prepared material from step 1) into a ball mill for ball milling. After the process is complete, remove the material, dry it, and obtain the rare earth silicate precursor. 3) Place the rare earth silicate precursor obtained in step 2) in a tube furnace and calcine it to obtain rare earth silicate (La). a Y b Sm c Dy d )2Si2O7; 4) Grind the rare earth silicate obtained in step 3); 5) Dissolve the polyetherimide particles in N-methylpyrrolidone to obtain a transparent, dark yellow polyetherimide solution; 6) Weigh out the rare earth silicate and polyetherimide solution, mix them evenly and then stir ultrasonically. After the reaction is complete, centrifuge and dry to obtain porous polyetherimide-coated rare earth silicate material.
2. The highly transparent rare-earth ultraviolet shielding material according to claim 1, characterized in that: In step 2), the ball milling speed is 300-600 r / min, the ball milling reaction is carried out for 12-18 h, and the drying is carried out at 60-80℃ for 8-12 hours; In step 3), the calcination temperature is 1200-1500℃, and the calcination time is 3-6 hours; In step 4), the particle size after grinding is 500-800 nm; In step 5), the dissolution temperature of the polyetherimide particles is 50-70℃; In step 6), ultrasonic stirring is performed for 20-60 minutes, and the drying temperature is 60-80℃.
3. The highly transparent rare-earth ultraviolet shielding material according to claim 1, characterized in that: In step 1), the molar ratio of rare earth oxides to silicon oxide is 1:2; Rare earth oxides are a mixture of lanthanum oxide, yttrium oxide, dysprosium oxide, and samarium oxide; In step 6), the rare earth silicate comprises 50-70 parts by weight and the polyetherimide solution comprises 30-50 parts by weight.
4. The highly transparent rare-earth ultraviolet shielding material according to claim 1, characterized in that: The highly transparent rare-earth shielding material is prepared by the following method: a. Weigh boric acid, silicon dioxide, rare earth oxides, and aluminum oxide and put them into a ball mill jar, then add deionized water and mix. b. Load the prepared material from step a into a ball mill for ball milling; c. The ball-milled material from step b is filtered, washed, and dried to obtain La. m Ce n Y x Al2B2SiO8(OH)2 powder was then placed in a tube furnace and calcined to obtain blocky La. m Ce n Y x Al2B2SiO8(OH)2; d. Add deionized water to the material obtained in step c, and then add blocky La. m Ce n Y x A high-transparency rare earth shielding material slurry can be obtained by grinding 1-8% of Al2B2SiO8(OH)2 as a grinding dispersant until the particle size is ≤100nm. e. The highly transparent rare earth shielding material slurry obtained in step d is processed into nano-sized powder by spray drying.
5. The highly transparent rare-earth ultraviolet shielding material according to claim 4, characterized in that: In step a, the molar ratio of boric acid:silicon oxide:aluminum oxide:rare earth oxide is 1:1:1:0.67; the rare earth oxide is a mixture of lanthanum oxide, cerium oxide, and yttrium oxide. In step b, the ball milling speed is 300-800 r / min, and the ball milling time is 8-16 hours; In step c, the drying temperature is 60-80℃, the calcination temperature is 400-600℃, and the calcination time is 3-6 hours; The grinding and dispersing agent in step d is fatty acid polyethylene glycol ester; The powder obtained after spray drying in step e has a particle size of 400-600 nm.
6. The highly transparent rare-earth ultraviolet shielding material according to claim 1, characterized in that: Both the first waterborne resin and the second waterborne resin are selected from one or more of acrylic resin and polyurethane resin; Both the first predispersant and the second predispersant are selected from one or more of BYK-2013, BYK-190, sodium hexametaphosphate, sodium pyrophosphate, and polyvinyl alcohol; Both the first and second additives are selected from one or more of the following: wetting agents, thickeners, leveling agents, defoamers, antisettling agents, and film-forming aids.
7. A method for preparing a highly transparent rare-earth ultraviolet shielding material as described in any one of claims 1-6, characterized in that: The method includes the following steps: 1) Preparation of primer coating 1.1) Weigh the first aqueous resin, the first predispersant, and deionized water, and stir and disperse for 60-90 minutes; 1.2) Add porous polyetherimide-coated rare earth silicate material to step 1.1) and stir and disperse for 60-90 minutes, then add the first additive and continue stirring for 10-30 minutes to obtain the primer coating. 2) Preparation of surface coating 2.1) Weigh the second aqueous resin, the second predispersant, and deionized water, and stir and disperse for 60-90 minutes; 2.2) Add the highly transparent rare earth shielding material to step 2.1) and stir and disperse for 60-90 minutes. Then add the second additive and continue stirring for 10-30 minutes to obtain the topcoat.
8. The application of a highly transparent rare-earth ultraviolet shielding material as described in any one of claims 1-6 in the fields of home textiles, outdoor products, and clothing fabrics, characterized in that: When applying, apply the primer to the fabric surface and cure it at 130-150℃ for 3-5 minutes to complete the primer application; apply the topcoat to the primer surface and cure it at 130-150℃ for 3-5 minutes to complete the topcoat application.
9. The application of the high-transparency rare-earth ultraviolet shielding material according to claim 8 in the fields of home textiles, outdoor products, and clothing fabrics, characterized in that: The base coat weight is 40-55 g / m². 2 The basis weight of the coating and topcoat should be maintained at 15-25 g / m². 2 between.
Citation Information
Patent Citations
Rare earth oxide-based nanometer ultraviolet shielding material and preparation method thereof
CN105565373A
High-hardness YAG-based composite structure transparent ceramic and preparation method thereof
CN113149632A