A poly-p-dioxanone degradable melt-blown nonwoven material and a method of making and use thereof

By optimizing the twin-screw extruder and hot airflow drawing process, the problem of unstable parameters in the production process of polydioxanone meltblown nonwoven materials was solved, realizing the efficient production and high-performance polydioxanone biodegradable meltblown nonwoven materials, which are widely used in clinical medicine, sanitary materials, agriculture and food packaging.

CN119711049BActive Publication Date: 2026-11-20TIANJIN UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510085001.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-01-20
Publication Date
2026-11-20
Estimated Expiration
2045-01-20

AI Technical Summary

Technical Problem

The existing technology for producing meltblown nonwoven materials using polydioxanone as a raw material lacks clear process guidance, resulting in unstable product quality, large performance fluctuations, and difficulty in fully realizing its potential in meltblown nonwoven materials.

Method used

The process involves heating and melting poly(p-dioxanone) chips using a twin-screw extruder, then extruding them through a spinneret and drawing them at high speed in a hot airflow to form fibers. By precisely controlling the temperature of each section of the screw, the airflow pressure, and the temperature, and optimizing the meltblown process parameters, the uniformity and consistency of the fibers are ensured.

Benefits of technology

It has achieved efficient and stable production of polydioxanone biodegradable meltblown nonwoven materials, improving the material's mechanical strength, biodegradability, filtration performance, air permeability and chemical stability, making it suitable for clinical medicine, hygiene materials, agriculture and food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005249865600000221
    Figure BDA0005249865600000221
Patent Text Reader

Abstract

The application discloses a preparation method and application of a poly-p-dioxanone degradable melt-blown non-woven material, and relates to the technical field of melt-blown non-woven materials. The melt-blown non-woven material is prepared from poly-p-dioxanone as raw material, is extruded by a spinneret after being heated and melted by a double-screw extruder, is high-speed drawn in a hot air flow to form fibers, and is collected by a receiving device after being self-bonded into a web. The melt-blown non-woven material has good performance effects in mechanical strength, biodegradability, filtering performance, air permeability, humidity resistance and chemical stability, and can be widely applied to surgical dressings, wound dressing materials, mask materials and protective clothing materials in the clinical medical field, sanitary napkin materials, paper diaper materials and wet wipe materials in the sanitary material field, plant covering materials and seed coating materials in the agricultural field, and food preservation packaging materials in the food packaging field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nonwoven materials technology, and in particular to a polydioxanone biodegradable meltblown nonwoven material, its preparation method, and its application. Background Technology

[0002] Poly(p-dioxanone) ketone (PPDO), a novel biodegradable material, is an aliphatic polyester ether. The ester bonds in its molecular backbone give PPDO excellent biodegradability, allowing it to gradually decompose in the natural environment or within organisms. This effectively avoids the continuous environmental stress caused by the long-term retention of traditional non-degradable materials and the potential for foreign body residue in biomedical applications. Simultaneously, its excellent biocompatibility ensures that the material can coexist harmoniously with biological tissues without triggering harmful immune responses or inflammation, greatly improving its safety in biomedical applications. Furthermore, under specific physiological conditions, it can be absorbed by human tissues at a predetermined rate, eliminating the need for secondary surgery and reducing patient suffering and medical costs. The presence of ether bonds in its molecular backbone gives the polymer both good strength and excellent toughness, and it is currently used in the preparation of biodegradable surgical sutures, playing an important role in clinical medicine.

[0003] Meltblown nonwoven technology is a type of polymer direct web forming method. It involves extruding polymer melt from a screw extruder and then subjecting the melt stream to extreme stretching through a high-speed, high-temperature airflow to form ultrafine fibers. These fibers are then aggregated onto a web forming curtain to form a fiber web, which is finally reinforced through self-adhesion to create meltblown nonwoven materials. Meltblown nonwoven materials play a crucial role in medical protective equipment (such as masks and protective clothing) and hygiene products (such as sanitary napkins and diapers) due to their excellent barrier filtration and breathability.

[0004] The production of poly(p-dioxanone) nonwoven materials using the melt-blown method has the advantages of short process flow and high production efficiency. The resulting poly(p-dioxanone) nonwoven materials retain the original advantages of microfiber and also have biodegradability, biocompatibility, absorbability, and excellent strength and toughness. It has great application potential in medical protection, hygiene materials, environmental protection (such as biodegradable filter materials in air filtration and water purification), agriculture (such as biodegradable plant covering materials and seed coating materials), and food packaging (biodegradable food preservation packaging materials).

[0005] Despite the numerous advantages of meltblown nonwoven technology, unprecedented challenges exist when using poly(p-dioxanone) as a raw material in meltblown production. The production process of meltblown nonwoven materials involves multiple critical steps, including feeding, screw melting and extrusion, filtration, die spinning, high-temperature, high-speed airflow stretching to form ultrafine fibers, and finally bonding onto the fabric. However, to date, there is a severe lack of data on meltblown processes using poly(p-dioxanone) as a raw material. This results in a lack of clear process guidance in actual production, making it difficult to accurately control parameters at each stage. Consequently, product quality becomes unstable, performance fluctuates significantly, and the full potential of poly(p-dioxanone) in meltblown nonwoven materials cannot be realized.

[0006] Therefore, it is necessary to design a method for preparing poly(p-dioxanone) meltblown nonwoven materials that can fully utilize the excellent properties of PPDO raw materials, while optimizing the meltblown process to improve product quality and stability, thus laying a solid foundation for the widespread application of poly(p-dioxanone) meltblown nonwoven materials in the medical field and other related fields. Summary of the Invention

[0007] The purpose of this invention is to provide a biodegradable poly(p-dioxanone) meltblown nonwoven material that solves the above-mentioned technical problems.

[0008] Another object of the present invention is to provide a method for preparing the above-mentioned polydioxanone degradable meltblown nonwoven material.

[0009] Another object of the present invention is to provide an application of the above-mentioned polydioxanone biodegradable meltblown nonwoven material.

[0010] Therefore, the technical solution of the present invention is as follows:

[0011] A biodegradable polydioxanone meltblown nonwoven material is made from polydioxanone as raw material. After being heated and melted by a twin-screw extruder, the material is extruded through a spinneret and stretched at high speed in a hot air stream to form fibers. The fibers are then self-adhesive and formed into a web, which is collected by a receiving device to obtain the meltblown nonwoven material.

[0012] This poly(p-dioxanone) biodegradable meltblown nonwoven material uses poly(p-dioxanone) (PPDO) as a key raw material. Its unique molecular structure and the ester bonds in the main chain are the key factors that endow the material with excellent biodegradability. This allows the material to decompose gradually in the natural environment or in organisms according to a specific degradation mechanism, effectively avoiding the environmental pressure caused by the long-term retention of traditional non-degradable materials and the problem of foreign matter residue that may occur in biomedical applications. The presence of ether bonds in the molecular chain brings good strength and excellent toughness to the material. This combination of strength and toughness makes it less prone to breakage when subjected to external forces, and can meet the needs of use under various complex working conditions.

[0013] In the first step of preparing degradable meltblown nonwoven materials of polydioxanone, the polydioxanone used for slicing is first strictly limited to a viscosity of 1.5 dL / g to 2 dL / g and a melt index of 20 g / 10 min to 25 g / 10 min. For polydioxanone with the above performance parameters, its glass transition temperature range is generally -9℃ to -11℃ and its melting temperature range is generally 97℃ to 115℃. The aforementioned limitations on the raw material performance parameters of poly(p-dioxanone) are intended to ensure that the chips can be smoothly melted and plasticized in subsequent processing, ultimately forming a high-performance meltblown nonwoven material. Specifically, a suitable viscosity range ensures the material's flowability and processability in the screw extruder, while the melt index affects the material's melting rate and molding performance. Through extensive screening experiments, the applicant discovered that when the viscosity and melt index of poly(p-dioxanone) are outside the suitable range, the resulting fibers exhibit significant problems such as uneven fiber thickness and poor molding effect. Furthermore, the glass transition temperature and melting temperature of poly(p-dioxanone) are related to the processing temperature settings in subsequent melt extrusion and stretching processes, thereby enabling the preparation of meltblown nonwoven materials based on materials with suitable parameters.

[0014] Before fiberizing the poly(p-dioxanone) chips, vacuum heating drying is preferred to ensure the chips reach a suitable physical state, guaranteeing a smooth subsequent melt extrusion process. Specifically, the drying temperature is precisely controlled between 50℃ and 70℃, and the drying time is between 12h and 48h. Extensive screening experiments have shown that using the aforementioned temperature and time ranges allows for the thorough removal of internal moisture while maintaining the chips' inherent properties. This prevents defects such as bubbles caused by moisture vaporization during high-temperature melting, which could affect the material's mechanical properties. Furthermore, the vacuum drying environment helps lower the boiling point of moisture, accelerates the drying process, and improves production efficiency.

[0015] In the heating and melting stage, the melting and extrusion process of the chips in the twin-screw extruder is one of the core links of the entire process. The precise setting of the temperature in each section of the screw is crucial. The temperature of the first zone is set at 85℃~95℃. Within this temperature range, the chips begin to soften under heat, laying the foundation for the subsequent melting process, while avoiding excessively high temperatures that could cause the chips to melt prematurely and affect the normal material transport. The temperature of the second zone is set at 155℃~165℃ to further promote the melting of the chips, gradually transforming the material into a uniform melt state. The temperatures of the third and fourth zones are both maintained at 170℃~180℃. The polymer melt in these two zones is fully plasticized under high temperature and the shearing action of the screw, achieving a highly uniform state and ensuring the quality and performance stability of the melt. The die temperature is set at 170℃~180℃, preferably consistent with the aforementioned temperatures of the third and fourth zones, so that the melt can maintain good fluidity and pressure distribution within the die, thereby being uniformly extruded from the spinneret to form a fine and uniform filamentous melt flow, providing a good foundation for the subsequent airflow drawing process.

[0016] Through extensive screening experiments, the applicant discovered that whether the temperature settings in each zone during the heating and melting stage meet the aforementioned limits significantly impacts the performance of the final meltblown nonwoven material. Specifically, when the temperature in zone one is set too low, the chips are not sufficiently softened, resulting in poor material flowability. Under the screw's push, the material is difficult to convey forward smoothly, leading to material accumulation in zone one, uneven melting, and ultimately, uneven fiber thickness, affecting the product's mechanical properties. Conversely, when the temperature in zone one is set too high, the chips melt prematurely, causing localized melt aggregation and poor flow, resulting in unstable material conveying, affecting the continuity of subsequent processing, and potentially leading to polymer degradation due to localized overheating, reducing the molecular weight of the melt. The temperature in Zone 2 affects the strength and toughness of the fibers. If the temperature in Zone 2 is set too low, the chips cannot melt sufficiently, resulting in a large number of incompletely melted particles in the melt. These particles can cause nodules and uneven fiber thickness during subsequent extrusion and airflow stretching. Conversely, if the temperature in Zone 2 is set too high, the polymer may degrade rapidly due to overheating. The degraded polymer chains break, altering the melt viscosity. This affects the tensile properties of the fibers during subsequent airflow stretching, making it difficult to form uniform ultrafine fibers, and may even lead to fiber breakage during stretching, resulting in decreased product strength and flexibility. If the temperature in Zone 3 is set too low, the melt is not sufficiently plasticized, resulting in uneven arrangement and distribution of internal molecular chains. This uneven melt cannot form a uniform fiber structure during extrusion and stretching, leading to significant differences in fiber diameter. Conversely, if the temperature in Zone 3 is set too high, the polymer undergoes excessive thermal oxidation, which not only alters the polymer's chemical structure and reduces the material's biodegradability but also produces low-molecular-weight volatiles. These volatiles form pores inside the fibers, affecting fiber density and reducing material strength. They may also affect the material's air permeability and filtration performance. Regarding die temperature settings, if the die temperature is set too low, the melt viscosity increases, reducing fluidity and causing uneven melt flow within the die. This results in inconsistent extrusion pressure of the filament bundles when extruded from the spinneret, leading to uneven filament thickness. If the die temperature is set too high, the melt may further degrade while remaining in the die. Furthermore, excessively high temperatures can cause the melt to become tangled and adhered before airflow stretching after extrusion due to reduced viscosity, resulting in abnormal fiber morphology and an inability to form a uniform fiber web.

[0017] In the airflow drawing process, the filaments ejected from the spinneret enter the high-temperature, high-speed airflow drawing zone. The airflow pressure is set between 0.1 MPa and 0.5 MPa, and the airflow temperature is set between 160°C and 180°C. Specifically, airflow drawing is a crucial step in transforming the melt stream into ultrafine short fibers. Precise control of airflow pressure and temperature directly affects key indicators such as fiber diameter, orientation, and mechanical properties. Appropriate airflow pressure provides sufficient tensile force, allowing the filaments to be stretched into ultrafine short fibers under the action of airflow, while airflow temperature affects the viscosity and fluidity of the melt, thus influencing the fiber forming process. By precisely adjusting the airflow pressure and temperature, ultrafine short fibers with different performance characteristics can be prepared according to actual needs.

[0018] Through extensive screening experiments, the applicant discovered that in the airflow stretching molding step, an excessively high aspect ratio results in uneven fiber distribution, while an excessively low aspect ratio leads to significant differences in fiber thickness. Excessive airflow pressure causes fibers to be too thin and unevenly distributed, making them prone to breakage, while insufficient airflow pressure results in coarser fibers. Furthermore, in this step, excessively high temperatures cause a significant decrease in polymer melt viscosity, making fibers prone to overstretching and potentially triggering polymer thermal decomposition or thermal oxidation reactions. Excessively low temperatures result in incomplete fiber stretching, leading to coarse and uneven fiber diameters, reducing product strength and flexibility.

[0019] In summary, the parameters set in the various preparation steps of this polydioxanone biodegradable meltblown nonwoven material are not isolated but rather synergistic and mutually influential. The reasonable temperature distribution in each section of the screw is closely related to the melt's fluidity and plasticization degree, thus affecting the melt's pressure stability and extrusion uniformity during spinning. The pressure and temperature of the airflow stretching process need to be matched with the spinning parameters to ensure that the filaments extruded from the spinneret can be stretched into ideal ultrafine short fibers under suitable conditions. Through in-depth research and optimized combination of these process parameters, the entire preparation process has achieved efficient and stable operation, ensuring the consistency and reliability of product performance.

[0020] This polydioxanone biodegradable meltblown nonwoven material is used in the clinical medical field as a material for surgical dressings, wound bandages, masks, and protective clothing; and in the field of hygiene materials as a material for sanitary napkins, diapers, and wet wipes.

[0021] In the agricultural field, this polydioxanone biodegradable meltblown nonwoven material is used as a material for making plant cover cloth and seed coating. This material can provide functions such as heat preservation, moisture retention and weed prevention in the early stage of crop growth, and degrades naturally in the later stage of crop growth without the need for manual cleaning, thus reducing agricultural production costs and environmental pollution.

[0022] This polydioxanone biodegradable meltblown nonwoven material is used in the food packaging field as a material for food preservation packaging. This material can effectively extend the shelf life of food and can naturally degrade after disposal, solving the white pollution problem caused by traditional plastic packaging.

[0023] Furthermore, the preparation process of this invention is relatively simple. Starting from the drying of slicing, it goes through a series of continuous processing steps to directly produce meltblown nonwoven material, without the need for complex intermediate steps or additional processing procedures. This simplified process not only reduces energy consumption and equipment investment during production but also reduces product quality instability caused by complex processes. At the same time, the high production efficiency enables the material to be mass-produced in a short time, meeting the growing market demand for high-performance, environmentally friendly nonwoven materials, resulting in good economic benefits and market competitiveness.

[0024] Compared with existing technologies, this polydioxanone biodegradable meltblown nonwoven material uses polydioxanone as raw material. After being heated and melted by a twin-screw extruder, it is extruded through a spinneret and formed at high speed in a hot airflow. It has excellent performance in mechanical strength (including tensile strength and flexibility), biodegradability (absorbability), filtration performance, breathability, moisture resistance, and chemical stability. This makes it widely applicable in clinical medicine for surgical dressings, wound dressings, mask materials, and protective clothing materials; in hygiene products for sanitary napkins, diapers, and wet wipes; in agriculture for plant covering materials and seed coating materials; and in food packaging for food preservation packaging materials. Detailed Implementation

[0025] The present invention will be further described below with reference to specific embodiments, but the following embodiments are by no means intended to limit the present invention.

[0026] Example 1

[0027] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0028] S1. Take polydioxanone slices with a viscosity of 1.5 dL / g, a melt index of 25 g / 10 min, a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat and dry the slices at a drying temperature of 50℃ for 12 hours.

[0029] S2. The dried slices are fed into a twin-screw extruder. The temperature of the twin-screw extruder is set to 85℃ in zone 1, 155℃ in zone 2, 170℃ in zone 3, 170℃ in zone 4, and 170℃ at the die.

[0030] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 13:1. The molten stream extruded from the spinneret is stretched by an airflow at a temperature of 160℃ and a pressure of 0.1MPa to form ultrafine short fibers. These fibers are then self-adhesive and formed into a web, which is collected by a receiving device to obtain meltblown nonwoven material.

[0031] Example 2

[0032] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0033] S1. Take polydioxanone slices with a viscosity of 1.8 dL / g, a melt index of 22 g / 10 min, a glass transition temperature of -10℃, and a melting temperature of 105℃; vacuum heat and dry the slices at a drying temperature of 60℃ for 30 h.

[0034] S2. The dried slices are fed into a twin-screw extruder. The temperature of the twin-screw extruder is set to 90℃ in zone 1, 160℃ in zone 2, 175℃ in zones 3 and 4, and 175℃ in the die.

[0035] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 15:1. The fine stream of melt extruded from the spinneret is stretched by an airflow at a temperature of 170℃ and a pressure of 0.3MPa to form ultrafine short fibers. These fibers are then self-adhesive and formed into a web, which is collected by a receiving device to obtain meltblown nonwoven material.

[0036] Example 3

[0037] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0038] S1. Take polydioxanone slices with a viscosity of 2 dL / g, a melt index of 20 g / 10 min, a glass transition temperature of -11℃, and a melting temperature of 115℃; vacuum heat and dry the slices at a drying temperature of 70℃ for 48 h.

[0039] S2. The temperature of the screw in zone 1 is set to 95℃, the temperature in zone 2 is set to 165℃, the temperature in zones 3 and 4 is set to 180℃, and the temperature of the die head is set to 180℃.

[0040] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 20:1. The airflow pressure is increased to 0.5MPa and the airflow temperature is raised to 180℃, stretching the melt stream into ultra-fine short fibers. These fibers are then self-adhesive and collected by a receiving device to obtain meltblown nonwoven material.

[0041] Example 4

[0042] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0043] S1. Take polydioxanone slices with a viscosity of 1.6 dL / g, a melt index of 23 g / 10 min, a glass transition temperature of -10℃, and a melting temperature of 100℃; vacuum heat and dry the slices at a drying temperature of 55℃ for 20 h.

[0044] S2, the temperature of the screw in zone 1 is set to 88℃, the temperature in zone 2 is set to 158℃, the temperature in zones 3 and 4 is set to 172℃, and the temperature of the die head is set to 172℃;

[0045] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 12:1. The airflow pressure is increased to 0.2MPa and the airflow temperature is raised to 165℃, stretching the melt stream into ultra-fine short fibers. These fibers are then self-adhesive and collected by a receiving device to obtain meltblown nonwoven material.

[0046] Example 5

[0047] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0048] S1. Take polydioxanone slices with a viscosity of 1.9 dL / g, a melt index of 21 g / 10 min, a glass transition temperature of -10.5℃, and a melting temperature of 110℃; vacuum heat and dry the slices at a drying temperature of 65℃ for 35 h.

[0049] S2, screw zone 1 temperature 92℃, zone 2 temperature 162℃, zone 3 and zone 4 temperatures are both 178℃, die head temperature 178℃;

[0050] S3. After being heated and melted, the melt is extruded through a spinneret with an aspect ratio of 18:1. The airflow pressure is increased to 0.4MPa and the airflow temperature is raised to 175℃, stretching the melt stream into ultrafine short fibers. These fibers are then self-adhesive and collected by a receiving device to obtain meltblown nonwoven material.

[0051] Example 6

[0052] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0053] S1. Take polydioxanone slices with a viscosity of 1.7 dL / g, a melt index of 24 g / 10 min, a glass transition temperature of -9.5℃, and a melting temperature of 103℃; vacuum heat and dry the slices at a drying temperature of 60℃ for 25 h.

[0054] S2, screw zone 1 temperature 90℃, zone 2 temperature 160℃, zone 3 and zone 4 temperatures are both 176℃, die head temperature 176℃;

[0055] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 16:1. The airflow pressure is increased to 0.35MPa and the airflow temperature is raised to 172℃, stretching the melt stream into ultra-fine short fibers. These fibers are then self-adhesive and collected by a receiving device to obtain meltblown nonwoven material.

[0056] Example 7

[0057] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0058] S1. Take polydioxanone slices with a viscosity of 1.55 dL / g, a melt index of 24.5 g / 10 min, a glass transition temperature of -9.2℃, and a melting temperature of 98℃; vacuum heat and dry the slices at a drying temperature of 52℃ for 15 h.

[0059] S2, screw zone 1 temperature 86℃, zone 2 temperature 156℃, zone 3 and zone 4 temperatures are both 172℃, die head temperature 172℃;

[0060] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 11:1. The airflow pressure is increased to 0.15MPa and the airflow temperature is raised to 162℃, stretching the melt stream into ultra-fine short fibers. These fibers are then self-adhesive and collected by a receiving device to obtain meltblown nonwoven material.

[0061] Example 8

[0062] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0063] S1. Take polydioxanone slices with a viscosity of 1.85 dL / g, a melt index of 21.5 g / 10 min, a glass transition temperature of -10.8℃, and a melting temperature of 112℃; vacuum heat and dry the slices at a drying temperature of 68℃ for 45 h.

[0064] S2, screw zone 1 temperature 94℃, zone 2 temperature 164℃, zone 3 and zone 4 temperatures are both 176℃, die head temperature 176℃;

[0065] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 19:1. The airflow pressure is increased to 0.45MPa and the airflow temperature is raised to 178℃, stretching the melt stream into ultra-fine short fibers. These fibers are then self-adhesive and collected by a receiving device to obtain meltblown nonwoven material.

[0066] Example 9

[0067] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0068] S1. Take polydioxanone slices with a viscosity of 1.95 dL / g, a melt index of 20.5 g / 10 min, a glass transition temperature of -10.5℃, and a melting temperature of 114℃; vacuum heat and dry the slices at a drying temperature of 65℃ for 38 hours.

[0069] S2, screw zone 1 temperature 93℃, zone 2 temperature 163℃, zone 3 and zone 4 temperatures are both 179℃, die head temperature 179℃;

[0070] S3. After being heated and melted, the melt is extruded through a spinneret with a length-to-diameter ratio of 17:1. The airflow pressure is increased to 0.38MPa and the airflow temperature is raised to 175℃, stretching the melt stream into ultra-fine short fibers. These fibers are then self-adhesive and collected by a receiving device to obtain meltblown nonwoven material.

[0071] Comparative Example 1

[0072] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0073] S1. Prepare polydioxanone slices with a viscosity of 1 dL / g, a melt index of 25 g / 10 min, a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat the slices to dry them at a temperature of 50℃ for 12 hours.

[0074] S2. Place the dried slices into a twin-screw extruder. Set the temperature of the twin-screw extruder to 85℃ in zone 1, 155℃ in zone 2, 170℃ in zone 3, 170℃ in zone 4, and 170℃ at the die.

[0075] S3. After being heated and melted, it is extruded through a spinneret with a length-to-diameter ratio of 10:1, and stretched by an airflow at a temperature of 160℃ and a pressure of 0.1MPa.

[0076] Comparative Example 2

[0077] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0078] S1. Prepare polydioxanone slices with a viscosity of 2 dL / g, a melt index of 15 g / 10 min (below the specified range), a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat and dry the slices at a drying temperature of 50℃ for 12 hours.

[0079] S2. Place the dried slices into a twin-screw extruder. Set the temperature of the twin-screw extruder to 85℃ in zone 1, 155℃ in zone 2, 170℃ in zone 3, 170℃ in zone 4, and 170℃ at the die.

[0080] S3. After being heated and melted, it is extruded through a spinneret with a length-to-diameter ratio of 13:1, and stretched by an airflow at a temperature of 160℃ and a pressure of 0.1MPa.

[0081] Comparative Example 3

[0082] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0083] S1. Take polydioxanone slices with a viscosity of 1.5 dL / g, a melt index of 25 g / 10 min, a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat and dry the slices at a drying temperature of 40℃ for 12 hours.

[0084] S2. The dried slices are placed into a twin-screw extruder. The temperature of the twin-screw extruder is set as follows: Zone 1: 85℃, Zone 2: 155℃, Zone 3: 170℃, Zone 4: 170℃, and Die: 170℃.

[0085] S3. After being heated and melted, the fibers are extruded through a spinneret with a length-to-diameter ratio of 13:1. They are then stretched by an airflow at a temperature of 160℃ and a pressure of 0.1MPa to form ultrafine short fibers, which are then self-adhesively bonded into a web and collected by a receiving device.

[0086] Comparative Example 4

[0087] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0088] S1. Take polydioxanone slices with a viscosity of 1.5 dL / g, a melt index of 25 g / 10 min, a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat and dry the slices at a drying temperature of 50℃ for 12 hours.

[0089] S2. The dried slices are fed into a twin-screw extruder. The temperature of the twin-screw extruder is set to 85℃ in zone 1, 155℃ in zone 2, 170℃ in zone 3, 170℃ in zone 4, and 170℃ at the die.

[0090] S3. After being heated and melted, it is extruded through a spinneret with a length-to-diameter ratio of 13:1, and stretched by an airflow at a temperature of 150℃ and a pressure of 0.1MPa.

[0091] Comparative Example 5

[0092] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0093] S1. Take polydioxanone slices with a viscosity of 1.5 dL / g, a melt index of 25 g / 10 min, a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat and dry the slices at a drying temperature of 50℃ for 12 hours.

[0094] S2. The dried slices are placed into a twin-screw extruder. The temperature of the twin-screw extruder is set as follows: Zone 1: 85℃, Zone 2: 155℃, Zone 3: 170℃, Zone 4: 170℃, and Die: 170℃.

[0095] S3. After being heated and melted, the material is extruded through a spinneret with a length-to-diameter ratio of 13:1. It is then stretched by an airflow at a temperature of 160℃ and a pressure of 0.05MPa.

[0096] Comparative Example 6

[0097] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0098] S1. Take polydioxanone slices with a viscosity of 1.5 dL / g, a melt index of 25 g / 10 min, a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat and dry the slices at a drying temperature of 50℃ for 12 hours.

[0099] S2. The dried slices are placed into a twin-screw extruder. The temperature of the twin-screw extruder is set to 100℃ in zone 1, 155℃ in zone 2, 170℃ in zone 3, 170℃ in zone 4, and 170℃ at the die.

[0100] S3. After being heated and melted, it is extruded through a spinneret with a length-to-diameter ratio of 13:1, and stretched by an airflow at a temperature of 160℃ and a pressure of 0.1MPa.

[0101] Comparative Example 7

[0102] A biodegradable poly(p-dioxanone) meltblown nonwoven material is prepared by the following method:

[0103] S1. Take polydioxanone slices with a viscosity of 1.5 dL / g, a melt index of 25 g / 10 min, a glass transition temperature of -9℃, and a melting temperature of 97℃; vacuum heat and dry the slices at a drying temperature of 50℃ for 12 hours.

[0104] S2. The dried slices are fed into a twin-screw extruder. The temperature of the twin-screw extruder is set to 85℃ in zone 1, 155℃ in zone 2, 170℃ in zone 3, 170℃ in zone 4, and 170℃ at the die.

[0105] S3. After being heated and melted, it is extruded through a spinneret with a length-to-diameter ratio of 5:1, and stretched by an airflow at a temperature of 160℃ and a pressure of 0.1MPa.

[0106] Performance testing:

[0107] (I) Microstructure testing:

[0108] Scanning electron microscope (SEM) images of the meltblown nonwoven materials prepared in Examples 1 to 9 were collected to determine the fiber diameter; the fiber diameter results for each example are shown in Table 1 below.

[0109] Table 1:

[0110] Test case Fiber diameter (μm) Example 1 2.5~4.5 Example 2 3.5~5.0 Example 3 4.0~6.0 Example 4 2.0~3.5 Example 5 5.0~7.0 Example 6 3.0~5.0 Example 7 2.0~4.0 Example 8 3.5~5.5 Example 9 2.5~3.5

[0111] As shown in Table 1, the fiber diameters of the poly(p-dioxanone) meltblown nonwoven materials prepared in Examples 1 to 9 range from 2.0 μm to 7.0 μm. Fiber diameter has a significant impact on material properties in many ways. Generally, finer fibers can form a denser structure, which significantly improves the filtration performance of the material. When filtering small particles, the smaller and more uniformly distributed pores between fine fibers effectively intercept smaller particles. Furthermore, Table 1 shows that the fiber diameter distribution is uniform for each material, with the diameter difference between fibers of different diameters not exceeding 2 mm. This is crucial for the stability of material properties; a uniform fiber diameter distribution indicates a consistent internal structure, resulting in better stability and reliability in mechanical properties. However, due to their structural characteristics, fine fibers are relatively less breathable. When air passes through materials made of fine fibers, it needs to pass through narrower and more tortuous channels, which increases the resistance to airflow and reduces the breathability. Conversely, materials with larger fiber diameters have a relatively loose structure and larger gaps between fibers, allowing air to flow more easily and thus having higher breathability. Therefore, a suitable fiber diameter is needed to balance the influence of fiber diameter and the porosity between fibers on the performance of meltblown nonwoven materials.

[0112] Furthermore, there are significant differences in fiber diameter among the poly(p-dioxanone) meltblown nonwoven materials prepared in each embodiment. That is, by adjusting the process parameters during the preparation process, poly(p-dioxanone) meltblown nonwoven materials with different specified fiber distribution characteristics can be obtained. Specifically, in addition to factors such as the viscosity of the raw material, the melt index, and the temperature settings of each zone of the twin-screw extruder affecting the fluidity and processability of the melt, and thus affecting the fiber formation, the spinneret aspect ratio and airflow stretching parameters also play a key role in the fiber diameter. For example, a larger spinneret aspect ratio and appropriate airflow stretching pressure and temperature help to refine the melt stream, resulting in finer fibers.

[0113] Compared to Example 1, Comparative Example 1 was prepared using poly(p-dioxanone) chips with excessively low viscosity. The resulting poly(p-dioxanone) meltblown nonwoven material had a fiber diameter range of 2.0 μm to 8.0 μm, showing a significant difference in fiber diameter compared to Example 1, resulting in poorer fiber web uniformity. This is likely because low-viscosity melts are easier to stretch into fine fibers, but due to their excessive "softness," they are difficult to maintain a stable shape during stretching, easily leading to localized overstretching or understretching, thus resulting in inconsistent fiber diameters and poor fiber web uniformity. In another comparative experiment, when poly(p-dioxanone) chips with excessively high viscosity were used, the melt flow in the screw extruder was too poor during processing, making material transport difficult. The extruded filaments also showed uneven thickness, resulting in a meltblown nonwoven material with large differences in fiber diameter and an overall coarser fiber size, which also affected the performance of the meltblown nonwoven material.

[0114] Compared to Example 1, Comparative Example 2 was prepared using poly(p-dioxanone) chips with an excessively low melt index. During processing, due to the low melt index, the melt was difficult to stretch and refine. During extrusion, some melt could not be extruded smoothly, clogging the spinneret orifices and preventing fiber formation, thus failing to produce meltblown nonwoven material. In another comparative experiment, when poly(p-dioxanone) chips with an excessively high melt index were used, the melt flow rate was too fast during extrusion, making it difficult to precisely control the forming process. This resulted in inconsistent fiber thickness and a tendency for fiber breakage, similarly affecting the performance of the meltblown nonwoven material.

[0115] Compared to Example 1, the fiber diameter range of the poly(p-dioxanone) meltblown nonwoven material prepared in Comparative Example 4 is 5.0 μm to 7.0 μm, which is significantly larger than that in Example 1. This is likely because the airflow temperature in the airflow drawing step in this comparative example was set too low, resulting in increased melt viscosity, poor flowability, and difficulty in fully drawing the filaments into ultrafine short fibers. The resulting fibers were coarser and less uniform in diameter. In another comparative experiment, if the airflow temperature was set too high in the airflow drawing step, the melt viscosity would drop sharply, leading to decreased stability of the filaments during drawing and problems such as filament bundling and adhesion. This resulted in uneven fiber diameters and some fibers being too thin, thus affecting the overall performance of the nonwoven material.

[0116] Compared to Example 1, the fiber diameter of the poly(p-dioxanone) meltblown nonwoven material prepared in Comparative Example 5 ranged from 5.5 μm to 7.5 μm, which was significantly larger than that in Example 1. This is likely because the airflow pressure in the airflow drawing step of this comparative example was insufficient, resulting in inadequate tension in the fiber bundle and thus a coarser fiber diameter. In another comparative experiment, if the airflow pressure was set too high during the airflow drawing step, the excessive tension on the fiber bundle could lead to overstretching or even breakage of the fibers, resulting in excessively fine and unevenly distributed fibers, which would negatively impact the mechanical properties and quality stability of the nonwoven material.

[0117] Compared to Example 1, in the poly(p-dioxanone) meltblown nonwoven material prepared in Comparative Example 6, some fibers had a diameter less than 2 μm, while others had a diameter greater than 10 μm. This is likely due to: excessively high temperature in Zone 1 causing premature melting and adhesion of the fiber slices to the screw, resulting in poor material transport, uneven extrusion melt, and significant differences in fiber diameter. This fiber diameter distribution leads to a chaotic internal structure, preventing the formation of a dense and uniform fiber web, severely affecting the material's microstructure and consequently its overall performance.

[0118] Compared with Example 1, the fiber diameter of the poly(p-dioxanone) meltblown nonwoven material prepared in Comparative Example 7 ranges from 6.5 μm to 8.5 μm, which is significantly larger than that in Example 1. The reason for this is that the spinneret aspect ratio was set too small in the airflow stretching step of the comparative example, resulting in uneven shearing action on the melt when it is extruded from the spinneret, leading to large differences in the thickness of the resulting filament bundles. Furthermore, it is difficult to form ultrafine short fibers during the airflow stretching process, resulting in uneven fiber distribution in the nonwoven material.

[0119] (II) Mechanical property testing:

[0120] The mechanical properties of the meltblown nonwoven materials prepared in Examples 1 to 9 were tested, and the specific test results are shown in Table 2 below.

[0121] Table 2:

[0122] Test case Tensile strength (MPa) Elongation at break (%) Example 1 9.5 205 Example 2 12.8 185 Example 3 14.5 155 Example 4 8.2 225 Example 5 15.8 125 Example 6 10.8 192 Example 7 6.8 230 Example 8 12.2 168 Example 9 7.5 215

[0123] As can be seen from the results in Table 2, the tensile strength of the meltblown nonwoven materials prepared in Examples 1 to 9 is between 6.8 MPa and 15.8 MPa, and the elongation at break is between 125% and 230%, indicating that the materials have both good strength and flexibility. Among them, the meltblown nonwoven material prepared in Example 3 has better mechanical property matching. The reason for this is that the good matching between the raw material viscosity and melt index and the processing temperature results in good fiber formation and tight molecular chain arrangement. The elongation at break test results of the meltblown nonwoven materials prepared in Examples 1 and 7 are better than the tensile strength test results, and they have better flexibility and can withstand greater deformation. The reason for this is that the raw material viscosity is lower, and the fiber formation is not tight enough during processing.

[0124] Compared with Example 1, the tensile strength of the meltblown nonwoven material prepared in Comparative Example 1 was 5.5 MPa and the elongation at break was 150%, which was significantly lower than that of Example 1. The reason for this is that, according to the microstructure test results of the comparative example, the fiber diameter bundles formed during the processing of the comparative example were uneven, resulting in uneven stress distribution inside the material. Under the action of external force, the thinner parts were more likely to break first, which led to a decrease in the overall material strength. Therefore, the mechanical strength of the meltblown nonwoven material could not meet the requirements for normal use.

[0125] Compared with Example 1, the tensile strength of the meltblown nonwoven material prepared in Comparative Example 3 was 4.0 MPa and the elongation at break was 130%, which was significantly lower than that of Example 1. The reason for this is that the drying temperature was too low before the screw melt extrusion step, resulting in insufficient removal of moisture from the chips. As a result, the moisture in the chips vaporized during the high-temperature melting process, generating a large number of bubbles, which caused the internal structure of the fibers to be loose, and the strength of the nonwoven material decreased significantly, failing to meet the expected product performance standards.

[0126] Compared to Example 1, the tensile strength of the meltblown nonwoven material prepared in Comparative Example 5 was 7.0 MPa, and the elongation at break was 140%, significantly lower than that of Example 1. The reason for this is that, although generally, larger fiber diameters may result in better tensile strength, in Comparative Example 5, the fiber diameters were not only large but also unevenly distributed, leading to structural defects within the material. Under stress, stress concentrated on some of the larger fibers, which lacked sufficient tight interweaving and support from finer fibers, resulting in uneven stress transmission throughout the material. Simultaneously, the large proportion and unreasonable distribution of coarse fibers limited the material's deformation capacity under stress, leading to poor flexibility. In practical applications, this uneven structure easily causes breakage at stress concentration points, failing to meet product quality standards.

[0127] Compared with Example 1, the tensile strength of the meltblown nonwoven material prepared in Comparative Example 7 was 6.0 MPa and the elongation at break was 160%, which was significantly lower than that of Example 1. The reason for this is that, according to the microstructure test results of the comparative example, the fiber diameter bundles formed in the comparative example during the processing were uneven, resulting in an uneven internal structure of the material. Under stress, the deformation of each part was inconsistent, causing stress concentration, resulting in poor mechanical properties and failing to meet the application requirements.

[0128] In practical applications, the tensile strength test results of the meltblown nonwoven material of the present invention can meet the requirements of the medical protection field for the materials used in the production of masks and protective clothing. It can withstand a certain amount of external force without easily breaking. Furthermore, the meltblown nonwoven material of the present invention has a high elongation at break, meaning that the material has good deformability, allowing it to adapt to different shape changes during use without breaking. Therefore, it can also be used in the field of hygiene materials for products such as sanitary napkins and diapers. It can naturally bend and stretch with the movement of the human body, providing a comfortable user experience.

[0129] (III) Degradation performance test:

[0130] The degradation performance of the meltblown nonwoven materials prepared in Examples 1 to 9 was tested, including degradation performance tests in simulated soil environment (agricultural topsoil with pH = 6.5 to 7.5 and water content of 20% to 25%) and degradation performance tests in simulated human tissue fluid environment (phosphate buffer solution with pH = 7.4 at 37°C). The specific test results are shown in Table 3 below.

[0131] Table 3:

[0132] Test case Weight loss rate (%) of soil environmental materials Weight loss rate of materials in tissue fluid environment (%) Example 1 48 96 Example 2 42 92 Example 3 38 88 Example 4 60 99 Example 5 32 84 Example 6 45 94 Example 7 58 98 Example 8 36 90 Example 9 50 97

[0133] As shown in Table 3, the meltblown nonwoven materials prepared in Examples 1 to 9 exhibited a weight loss rate of 32%–60% after 6 months in a simulated soil environment and 84%–99% after 6 months in a simulated human tissue fluid environment. This indicates that the materials can achieve a certain degree of degradation under different environments, consistent with the degradation characteristics of poly(p-dioxanone). Generally, meltblown nonwoven materials with finer fiber diameters have a larger specific surface area, resulting in a correspondingly increased contact area with the degradation medium in soil and tissue fluid environments, which is more conducive to the degradation reaction and leads to a relatively faster degradation rate. Taking Examples 4 and 7 as examples, the fibers in Example 4 are finer than those in Example 7, resulting in a larger specific surface area for the material in Example 4. In a simulated soil environment, the weight loss rate of Example 4 reached 60%, higher than the 58% of Example 7. In a simulated human tissue fluid environment, the weight loss rate of Example 4 was 99%, also slightly higher than the 98% of Example 7. This is consistent with the principle that finer fiber diameters are more conducive to degradation.

[0134] In practical applications, the meltblown nonwoven material of this invention can degrade at the expected rate in both soil and human tissue fluid environments, effectively avoiding the pollution of soil, water, and other ecological environments caused by the long-term accumulation of traditional non-degradable materials. This aligns with the concept of sustainable development and is particularly suitable for disposable medical and hygiene products. Simultaneously, the material's excellent biocompatibility ensures that it will not trigger harmful immune responses or inflammatory reactions when in contact with biological tissues, greatly improving its safety in the biomedical field. This expands its application prospects in the medical protection field beyond its use as a material for masks and protective clothing; it can also be used in situations involving close contact with human tissue, such as wound dressings and surgical dressings. The biodegradability of this material within the human body allows it to be absorbed by human tissue at a predetermined rate, eliminating the need for secondary surgery and reducing patient suffering and medical costs, thus facilitating clinical medical applications.

[0135] Furthermore, the biodegradability of the meltblown nonwoven material of this invention enables its application in agriculture (such as biodegradable plant mulch materials and seed coating materials) and food packaging (biodegradable food preservation packaging materials). Specifically, in agriculture, biodegradable plant mulch materials can naturally degrade during the later stages of crop growth, eliminating the need for manual cleanup and reducing agricultural production costs and environmental pollution. In food packaging, biodegradable food preservation packaging materials can naturally degrade after disposal, solving the white pollution problem caused by traditional plastic packaging. This wide range of applications provides a solid foundation for the market promotion and industrial development of the material, yielding significant social and economic benefits.

[0136] (iv) Filtration performance test:

[0137] The filtration performance of the meltblown nonwoven materials prepared in Examples 1 to 9 was tested, specifically their filtration efficiency for particles of 0.5 μm, 1 μm and 5 μm were tested, and the test results are shown in Table 4 below.

[0138] Table 4:

[0139] Test case 0.5μm filtration efficiency (%) 1μm filtration efficiency (%) 5μm filtration efficiency (%) Example 1 94 96 99 Example 2 93 95 98 Example 3 91 93 97 Example 4 96 97 99.5 Example 5 90 94 96 Example 6 93.5 96.5 98.5 Example 7 95 97 99.8 Example 8 92 95 97.5 Example 9 93 95 99.2

[0140] As shown in Table 4, the meltblown nonwoven materials prepared in Examples 1 to 9 exhibit filtration efficiencies of 90%–96% for 0.5 μm particles, 93%–97% for 1 μm particles, and 96%–99.8% for 5 μm particles. Compared to the filtration standards for meltblown nonwoven materials generally used in medical protection and hygiene fields, this material demonstrates high filtration efficiency for particles of different sizes. Typically, the medical protective mask standard GB 19083-2010 requires a filtration efficiency of no less than 95% for 0.3 μm non-oily particles. The filtration efficiency of the material of this invention for 0.5 μm particles is close to or exceeds some existing product standards, and its filtration efficiency for 1 μm and 5 μm particles is even more outstanding. This indicates that the meltblown nonwoven material possesses excellent filtration performance and can effectively intercept various common microparticles, demonstrating significant advantages in filtration applications.

[0141] Compared with Example 1, the poly(p-dioxanone) meltblown nonwoven material prepared in Comparative Example 4 has a filtration efficiency of 75% for 0.5 μm particles, 85% for 1 μm particles, and 90% for 5 μm particles, which is significantly lower than that of Example 1. The reason for this is that, according to the microstructure test results of this comparative example, the airflow temperature setting in the airflow stretching step is too low, making it difficult for the filament bundle to be fully stretched into ultra-fine short fibers. The fiber diameter is relatively large and uneven, resulting in excessively large and unevenly distributed pores between the fibers, making it easier for particles to penetrate the material. This results in poor filtration performance of the nonwoven material, which cannot meet the application requirements.

[0142] In practical applications, the excellent filtration performance of the meltblown nonwoven material of the present invention further enhances its applicability in the aforementioned medical and hygiene products, as well as medical protective products.

[0143] (V) Breathability Test:

[0144] The air permeability of the meltblown nonwoven materials prepared in Examples 1 to 9 was tested, and the specific test results are shown in Table 5 below.

[0145] Table 5:

[0146] Test case Example 1 Example 2 Example 3 Example 4 Example 5 air permeability 305mm / s 310mm / s 315mm / s 290mm / s 450mm / s Test case Example 6 Example 7 Example 8 Example 9 air permeability 320mm / s 300mm / s 330mm / s 335mm / s

[0147] As shown in Table 5, the air permeability of the meltblown nonwoven materials prepared in Examples 1 to 9 ranges from 290 mm / s to 450 mm / s. In the field of medical protective and hygiene products, air permeability is one of the important indicators for measuring the comfort and suitability of materials. For medical masks, excessively high air permeability may prevent effective blocking of airborne particles, bacteria, and viruses, reducing the protective effect; excessively low air permeability will increase the wearer's breathing resistance, causing stuffiness and reducing wearing comfort.

[0148] Generally, the breathability of common medical surgical masks is required to be no less than 240 mm / s to balance protective performance and wearing comfort. The meltblown nonwoven material prepared in this invention has a breathability between 290 mm / s and 450 mm / s. This breathability range not only ensures that the material has a certain level of protection, allowing the internal fiber structure to effectively intercept tiny particles in the air, but also ensures that air can pass through the material relatively smoothly, providing users with a comfortable breathing experience. In the field of hygiene products, such as sanitary napkins and diapers, a suitable breathability can keep the product dry, reduce discomfort caused by moisture accumulation, and improve user satisfaction. Therefore, the breathability of the meltblown nonwoven material of this invention meets the requirements for breathability in medical protection and hygiene products, and has good applicability in practical applications.

[0149] In the above embodiments, meltblown nonwoven materials with finer fiber diameters (such as in Embodiments 4 and 7) exhibit relatively low air permeability due to their relatively dense fiber web structure, small gaps between fibers, and greater entanglement and bonding, resulting in a tortuous and narrow airflow path and greater resistance to air passage. Conversely, meltblown nonwoven materials with coarser fiber diameters (such as in Embodiment 5) exhibit higher air permeability due to their relatively loose fiber web structure, large gaps between fibers, and difficulty in tightly bonding to form larger pores, allowing air to pass through more easily.

[0150] Compared with Example 1, the meltblown nonwoven material prepared in Comparative Example 3 had a low drying temperature and insufficient moisture removal in the slices. As a result, the moisture easily vaporized during the high-temperature melting process, generating a large number of bubbles. This led to a loose internal structure and a significant increase in air permeability. Excessive air permeability would affect its barrier effect against microorganisms, particles, etc., and would not meet the expected performance standards of medical and health products.

[0151] Compared to Example 1, the air permeability of the poly(p-dioxanone) meltblown nonwoven material prepared in Comparative Example 4 was 400 mm / s, significantly higher than that of Example 1. This is likely because, according to the microstructure test results of this comparative example, the airflow temperature setting in the airflow stretching step was too low, resulting in coarser and uneven fiber diameters, larger gaps between fibers, and easier airflow. In the field of medical protective and hygiene products, while higher air permeability allows for smoother airflow, it can lead to decreased filtration performance, failing to effectively intercept fine particles and pathogens, and thus failing to meet the comprehensive performance requirements of medical protective masks and hygiene products.

[0152] In practical applications, the excellent breathability of the meltblown nonwoven material of this invention further enhances its applicability in the aforementioned medical and hygiene products, as well as medical protective products. In the field of medical protective equipment, suitable breathability ensures that masks, protective clothing, and other products can effectively block harmful substances such as bacteria and viruses while allowing users to breathe freely, improving wearing comfort and compliance, and reducing protective gaps caused by discomfort. In the field of hygiene products, sanitary napkins, diapers, and other products have excellent breathability, effectively reducing moisture accumulation and lowering the risk of skin discomfort and disease caused by dampness, providing users with a dry and comfortable experience. Furthermore, in industrial settings with strict hygiene requirements, such as food processing workshops and pharmaceutical workshops, work clothes and air filtration equipment made from this material can also provide excellent breathability and filtration, ensuring the hygiene and safety of the production environment.

[0153] (vi) Application Environment Simulation Test:

[0154] The meltblown nonwoven materials prepared in Examples 1 to 9 were subjected to simulated tests in different application environments. Specifically, each meltblown nonwoven material was placed in environments with humidity of 30%RH, 60%RH, and 90%RH, respectively, and the temperature was maintained at 25°C for 72 hours. Each meltblown nonwoven material was also immersed in 75% alcohol and iodine solution for 2 hours, with the immersion process conducted at 25°C. The tensile strength and elongation at break of the materials after treatment in different simulated environments were tested, and the specific test results are shown in Table 6.

[0155] Table 6:

[0156]

[0157] As shown in Table 6, under different humidity conditions, the tensile strength of the material remains high at 30% RH, but the elongation at break is reduced due to the limited flexibility of the molecular chains caused by low moisture content. At 60% RH, moisture absorption leads to a decrease in tensile strength and an increase in elongation at break. At 90% RH, a large amount of water absorption results in a significant decrease in tensile strength and a substantial increase in elongation at break. Poly(p-dioxanone) itself has good chemical stability and some tolerance to alcohol and iodine. After soaking in alcohol, the tensile strength decreases slightly. Alcohol has certain solubility and penetrability, allowing it to penetrate into the material and disrupt the entanglement and bonding between fibers, making the material structure loose and thus reducing its strength. On the other hand, the penetration of alcohol causes plastic deformation of the fibers under tension, thereby increasing the elongation at break, but the increase is limited. After soaking in iodine, solvent swelling slightly reduces the tensile strength, while the elongation at break may not change much or may increase slightly due to the small swelling and insignificant damage.

Claims

1. A method for preparing a polydioxanone biodegradable meltblown nonwoven material, characterized in that, It uses poly(p-dioxanone) as raw material, which is heated and melted in a twin-screw extruder, then extruded through a spinneret and drawn at high speed in a hot airflow to form fibers. The fibers are then self-adhesive and collected by a receiving device. The viscosity of poly(p-dioxanone) is 1.5 dL / g to 2 dL / g, and the melt index is 20 g / 10 min to 25 g / 10 min. In the heating and melting step, the temperature of the twin-screw extruder is set as follows: Zone 1: 85℃ to 95℃, Zone 2: 155℃ to 165℃, Zone 3: 170℃ to 180℃, Zone 4: 170℃ to 180℃, and Die: 170℃ to 180℃. In the airflow drawing and forming step, the spinneret length-to-diameter ratio is (10 to 20):1, the airflow pressure is 0.1 MPa to 0.5 MPa, and the airflow temperature is 160℃ to 180℃.

2. The method for preparing the poly(p-dioxanone) biodegradable meltblown nonwoven material according to claim 1, characterized in that, The raw material is polydioxanone chips, which are dried under vacuum heating. The vacuum heating drying conditions are: drying temperature set at 50℃~70℃, and drying time at 12h~48h.

3. A polydioxanone biodegradable meltblown nonwoven material prepared by the preparation method as described in any one of claims 1 or 2.

4. An application of the poly(p-dioxanone) biodegradable meltblown nonwoven material as described in claim 3, characterized in that, In the field of clinical medicine, it is used as a material for surgical dressings, wound bandages, masks, and protective clothing; in the field of hygiene materials, it is used as a material for sanitary napkins, diapers, and wet wipes.

5. An application of the poly(p-dioxanone) biodegradable meltblown nonwoven material as described in claim 3, characterized in that, In the agricultural field, it is used as a material for making plant mulch and seed coatings.

6. An application of the poly(p-dioxanone) biodegradable meltblown nonwoven material as described in claim 3, characterized in that, In the food packaging industry, it is used as a material for making food preservation packaging.

Citation Information

Patent Citations

  • Segmented, epsilon-caprolactone-rich, poly(epsilon-caprolactone-co-p-dioxanone) copolymers for medical applications and devices therefrom