A thick coating with corrosion resistance and fire resistance performance for steel structure

The multi-layered steel structure coating solves the problems of insufficient durability and corrosion resistance of fire-retardant coatings for steel structures, achieving effective fire protection and long-term corrosion resistance in fires.

CN119775843BActive Publication Date: 2026-11-20SUZHOU DACHENG ENVIRONMENTAL PROTECTION NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411954046.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-27
Publication Date
2026-11-20
Estimated Expiration
2044-12-27

AI Technical Summary

Technical Problem

Existing fire-retardant coatings for steel structures lack durability and have poor corrosion resistance, making the coatings prone to cracking and powdering in fires, thus failing to effectively protect the mechanical properties of the steel structure.

Method used

The coating employs a multi-layer structure design consisting of a composite resin-modified zinc-rich primer, a heat-insulating and anti-corrosion coating, a lightweight fire-retardant coating, and a weather-resistant finishing layer. By rationally proportioning the materials in each layer, a dense interlayer structure is formed. The coating's anti-corrosion and fire-retardant properties are improved by utilizing the cathodic protection of the composite resin-modified zinc-rich primer, the multi-layered lamellar structure of the heat-insulating and anti-corrosion coating, and the barrier effect of the nano-alumina dispersion.

Benefits of technology

It maintains good corrosion resistance during long-term use and provides effective flame-retardant isolation and fire protection in the event of a fire, delaying the spread of corrosive media and improving the fire resistance and service life of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119775843B_ABST
    Figure CN119775843B_ABST
Patent Text Reader

Abstract

The application belongs to the field of chemical steel structure fire prevention, and more particularly relates to a thick coating with corrosion resistance and fire resistance for steel structure. The thick coating with corrosion resistance and fire resistance for steel structure comprises, in order based on the surface of a steel substrate, a composite resin modified zinc-rich primer, a heat-insulating and corrosion-resistant coating, a lightweight fire-resistant coating and a finishing weather-resistant layer. The heat-insulating and corrosion-resistant coating comprises, in parts by weight, 80-120 parts of a composite resin emulsion, 52.5-76.7 parts of a curing aid, 30-40 parts of a nano-aluminum oxide dispersion liquid, 66.5-133.5 parts of an active enhancement powder, 0.3-0.6 parts of an anti-settling agent and 0.3-0.6 parts of a cellulose ether. The active enhancement powder comprises slag powder, steel slag powder, sodium silicate, basalt flake and quartz powder. The thick coating with corrosion resistance and fire resistance for steel structure has excellent fire resistance, super-high salt mist resistance, good adhesion and compactness between coatings, good long-term use performance and meets the demand of building fire-resistant coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of fire protection for chemical steel structures, and more specifically, relates to a thick coating for steel structures with corrosion resistance and fire protection properties. Background Technology

[0002] With the rapid development of modern construction, steel structures, with their advantages of good mechanical properties, high strength, light weight, and high space utilization, are widely used in modern buildings such as steel structure parking lots, industrial plants, stadiums, stations, airports, and bridges. However, steel structures themselves have poor corrosion resistance and fire resistance, and are extremely conductive to heat. When the temperature reaches 450℃, their mechanical properties begin to deteriorate, and the deterioration effect becomes more severe as the temperature rises. When the temperature reaches 580℃, their mechanical strength drops to less than half of that at room temperature, making it unable to meet the supporting function of buildings and structures. Therefore, in order to prevent the collapse of buildings due to the reduced strength of the steel structure after a fire, which could cause huge losses to people's lives and property, fire protection must be provided for steel structure buildings.

[0003] Fire-retardant coatings for steel structures are classified into two main categories based on their working principle: intumescent and non-intumescent. Non-intumescent fire-retardant coatings do not expand during a fire. They rely on the non-combustible nature and low thermal conductivity of the material, or the heat absorption and flame retardant properties of the material in the coating, to delay the temperature rise of the steel. Therefore, they are usually thick coatings to protect steel structures. However, the durability of the coating is insufficient after application. It is prone to cracking, peeling, or blistering due to insufficient adhesion between coating layers and between the coating and the substrate. Over time, the fire-retardant performance decreases, and even powdering and peeling may occur. In addition, the coating has poor corrosion resistance. After long-term use, the underlying rust will bring huge safety hazards to the coating. Summary of the Invention

[0004] In view of the problems of insufficient durability and poor corrosion resistance of existing fire-retardant thick coatings, this application provides a thick coating with corrosion resistance and fire resistance for steel structures.

[0005] In a first aspect, this application provides a thick coating for steel structures with corrosion resistance and fire resistance, employing the following technical solution: A thick coating for steel structures with corrosion resistance and fire resistance comprises a composite resin modified zinc-rich primer, a heat-insulating and anti-corrosion coating, a lightweight fire-retardant coating, and a decorative weather-resistant layer sequentially disposed on the surface of a steel substrate. By weight, the heat-insulating and anti-corrosion coating comprises 80-120 parts of composite resin emulsion, 52.5-76.7 parts of curing aid, 30-40 parts of nano-alumina dispersion, 66.5-133.5 parts of active reinforcing powder, 0.3-0.6 parts of anti-settling agent, and 0.3-0.6 parts of cellulose ether, wherein the active reinforcing powder comprises slag powder, steel slag powder, sodium silicate, basalt flakes, and quartz powder.

[0006] By adopting the above technical solution and designing a multi-layer thick coating for steel structures, the coating consists of a composite resin modified zinc-rich primer, a heat-insulating and anti-corrosion coating, a lightweight fire-retardant coating, and a weather-resistant finishing layer. The materials in each layer are rationally proportioned and the interlayer structure is dense, which can maintain good corrosion resistance during long-term use and provide effective flame-retardant isolation and fire protection in the event of a fire.

[0007] Composite resin-modified zinc-rich primer provides cathodic protection to steel through sacrificial zinc powder rust prevention. The composite resin modification enhances chemical solvent resistance, corrosion resistance, and adhesion, resulting in coatings with excellent weather resistance and strong adhesion. The heat-insulating and anti-corrosion coating utilizes the high bonding strength between the composite resin emulsion and basalt flakes, forming a multi-layered, parallel, stacked barrier effect with excellent shielding performance. It divides the resin into several small spaces, effectively improving stress concentration within the resin. The flakes can form a staggered arrangement, making the penetration of corrosive media more circuitous, thus delaying the diffusion of corrosive media. The path and time of penetration into the metal surface are improved, thereby enhancing the anti-corrosion performance of the coating. Furthermore, the addition of nano-alumina dispersion provides excellent temperature resistance and fire resistance, significantly improving the density, anti-corrosion performance, and flame retardancy of the paint film. Additionally, the nano-alumina dispersion enhances dispersibility and interfacial properties, preventing sedimentation and ensuring interfacial compatibility between basalt flakes and the composite resin solution. The addition of curing aids, anti-settling agents, and cellulose ethers further improves the dispersibility and high / low temperature stability of the thermal insulation and anti-corrosion coating material, enhancing its corrosion resistance and enabling its use in harsh environments with large temperature differences.

[0008] Preferably, the active reinforcing powder further includes quartz sand.

[0009] The addition of quartz sand to the active reinforcing powder further improves the high temperature resistance and chemical stability of the heat insulation and anti-corrosion coating. Furthermore, the small particle size of quartz sand can further enhance the density of the active reinforcing powder in the heat insulation and anti-corrosion coating, and it also has corrosion resistance itself.

[0010] The composite resin emulsion comprises an organosilicon acrylate hybrid epoxy resin and an organosilicon emulsion. The mass ratio of the organosilicon acrylate hybrid epoxy resin to the organosilicon emulsion is (1.5-4):1.

[0011] Organosilicon acrylates exhibit good weather resistance and water resistance, but their room temperature curing rate is slow. Hybrid epoxy resins, which are easily cured at room temperature, undergo free radical polymerization on the ortho- and tertiary carbons of their ether bonds. The epoxy groups are directly grafted into the acrylic resin before ring-opening, preventing excessive -OH groups from causing explosive gelation. This provides a certain degree of storage stability. During curing, the ring-opening of the epoxy groups significantly improves interlayer adhesion, resulting in excellent bonding performance with various materials. This gives the composite resin emulsion chemical solvent resistance and corrosion resistance. By adding a certain proportion of organosilicon emulsion to the system, the Si-O-Si structure can improve the hardness and crosslinking density of the resin film, increase the material's density and impact resistance, and improve salt spray resistance, acid and alkali resistance, and temperature resistance, thereby enhancing the coating's strength and overall corrosion resistance. However, if the content of the organosilicon acrylate hybrid epoxy resin is too low, it may lead to insufficient interlayer adhesion, easily causing voids between layers, affecting the material's corrosion resistance and durability.

[0012] The mass ratio of the composite resin emulsion, nano-alumina dispersion, and basalt flakes is (2-4):1:(0.2-0.45).

[0013] By using a specific ratio of composite resin emulsion, nano-alumina dispersion, and basalt flakes, the heat-insulating and anti-corrosion coating maintains good interlayer adhesion and density, forming a barrier layer that effectively isolates corrosive media, significantly increasing the difficulty for corrosive media to enter the coating film. The introduction of inorganic nano-alumina dispersion improves the heat resistance of the intermediate coating, enabling it to maintain the adhesion of the high-barrier, heat-resistant, and anti-corrosion coating to the metal surface for a certain period of time, thus significantly improving the anti-corrosion performance of the system and the adhesion performance of the fire-retardant coating. However, if the content of composite resin emulsion is too low, the adhesion performance will be insufficient and the strength will be poor. If the content of nano-alumina dispersion is too low, the heat resistance will be insufficient, and the dispersibility of basalt flakes will be weak. Furthermore, the interfacial interaction between basalt flakes and resin will be poor, making it difficult to control the arrangement of basalt flakes and affecting the corrosion resistance of the anti-corrosion coating.

[0014] In one specific implementation, the weather-resistant decorative layer comprises 60-70 parts by weight of silicone acrylate hybrid epoxy resin, 30-40 parts by weight of FEVE emulsion, 33.7-44.7 parts by weight of curing aid, 0.2-0.4 parts by weight of leveling agent, 5-8 parts by weight of nano calcium carbonate, and 3-6 parts by weight of color paste.

[0015] The mass ratio of the FEVE emulsion to nano-calcium carbonate is (4-8):1.

[0016] By adopting the above technical solution, the addition of FEVE resin to organosilicon acrylate hybrid epoxy resin further improves the chemical inertness of the coating surface and introduces a large number of FC bonds, resulting in stronger stability. The introduction of nano-calcium carbonate significantly enhances the density of the cured paint film, preventing chalking and fading, and strengthening the weather resistance and color retention of the protective surface layer, as well as its ability to resist various corrosive media. This ensures the entire fireproof system has excellent weather resistance, maintains its fireproof capability for a long time, and extends its service life. However, excessive FEVE emulsion content can lead to excessive coating rigidity, poor elasticity, unstable performance, and in severe cases, cracking and peeling.

[0017] In one specific implementation scheme, the composite resin modified zinc-rich primer comprises, by weight, 80-120 parts of composite resin emulsion, 92-108 parts of zinc-rich reinforcing powder, 39.3-47.7 parts of curing aid, and 5-8 parts of nano-alumina dispersion; the zinc-rich reinforcing powder comprises slag powder, sodium silicate, and zinc powder.

[0018] The mass ratio of the slag powder, sodium silicate and zinc powder is (1.8-4):1:(9-16).

[0019] By adopting the above technical solution, the organosilicon-acrylic hybrid epoxy resin in the composite resin emulsion enhances the adhesion and bonding strength of the metal substrate. The introduction of a certain proportion of organosilicon resin improves the density, weather resistance, salt spray resistance, acid and alkali resistance, and temperature resistance of the paint film. The addition of a nano-alumina dispersion suitable for the primer film quality gives the primer excellent temperature resistance and fire resistance, significantly improving the density, corrosion resistance, and flame retardancy of the paint film. The interaction between the inorganic nanomaterial slag powder and sodium silicate within a certain range cuts off the channels formed by water evaporation after resin film formation, significantly improving the sealing effect of the water-based resin coating. Combined with zinc powder, this creates a high level of corrosion resistance to the metal surface, exhibiting strong adhesion to the metal substrate and good resistance to salt spray and damp heat. However, insufficient zinc powder content may affect the salt spray resistance of the primer.

[0020] In one specific implementation, the curing aid includes a curing agent, a wetting agent, a dispersant, a defoamer, a film-forming aid, and deionized water.

[0021] By adopting the above technical solution and adding curing aids, the adhesion and density of the coating and the coatings are improved, and the curing rate and production efficiency are increased.

[0022] In summary, this application has the following beneficial effects: 1. Through the design of a thick-coated multi-layer structure for steel structure, it is composed of composite resin modified zinc-rich primer, heat insulation and anti-corrosion coating, lightweight fireproof coating and weather-resistant finishing layer. The material ratio of each layer is reasonable and the interlayer structure is dense, which can maintain good corrosion resistance during long-term use and provide effective flame-retardant isolation and fire protection in the event of a fire.

[0023] The composite resin-modified zinc-rich primer provides cathodic protection to steel by sacrificing zinc powder for rust prevention. The composite resin modification enhances chemical solvent resistance, corrosion resistance, and adhesion, resulting in a coating with excellent weather resistance and strong adhesion. The heat-insulating and anti-corrosion coating achieves high bonding strength between the composite resin emulsion and basalt flakes, forming a multi-layered, parallel, stacked barrier effect with excellent shielding performance. The flakes can form a staggered arrangement, making the penetration of corrosive media more circuitous, thus delaying the path and time of corrosion diffusion and intrusion into the metal surface, thereby improving the coating's anti-corrosion performance. Furthermore, the addition of nano-alumina dispersion significantly improves the film's density, anti-corrosion performance, and flame retardancy, enhances dispersibility and interfacial properties to prevent sedimentation, and ensures interfacial compatibility between the basalt flakes and the composite resin solution.

[0024] 2. Organosilicon acrylates exhibit good weather resistance and water resistance, but their room temperature curing rate is slow. Hybrid epoxy resins, which are easily cured at room temperature, undergo free radical polymerization on the ortho- and tertiary carbons of their ether bonds. The epoxy groups are directly grafted into the acrylic resin before ring-opening, preventing excessive -OH groups from causing explosive gelation. This results in a certain degree of storage stability. During curing, the ring-opening of the epoxy groups significantly improves interlayer adhesion, leading to excellent bonding performance with various materials. This gives the composite resin emulsion chemical solvent resistance and corrosion resistance. By adding a certain proportion of organosilicon emulsion to the system, the Si-O-Si structure can improve the hardness and crosslinking density of the resin film, increase the material's density and impact resistance, and improve salt spray resistance, acid and alkali resistance, and temperature resistance, thereby enhancing the coating's strength and overall corrosion resistance.

[0025] 3. The addition of FEVE resin to organosilicon acrylate hybrid epoxy resin further improves the chemical inertness of the coating surface and introduces a large number of FC bonds, resulting in stronger stability. The introduction of nano-calcium carbonate significantly enhances the density of the cured paint film, preventing chalking and fading, and strengthening the weather resistance and color retention of the protective layer, as well as its ability to resist various corrosive media. This ensures that the entire fireproof system has excellent weather resistance, maintains its fireproof capability for a long time, and extends its service life. Excessive FEVE emulsion content will lead to excessive coating rigidity, poor elasticity, unstable performance, and in severe cases, cracking and peeling. Attached Figure Description

[0026] Figure 1This is a schematic diagram of the overall cross-sectional structure of the thick coating with corrosion resistance and fire resistance provided in Embodiment 1 of this application, applied to a steel substrate.

[0027] Explanation of reference numerals in the attached drawings: 1. Steel substrate; 2. Composite resin modified zinc-rich primer; 3. Heat-insulating and anti-corrosion coating; 4. Lightweight fire-retardant coating; 5. Finishing weather-resistant layer. Detailed Implementation

[0028] The present application will be further described in detail below with reference to the embodiments.

[0029] Some of the raw materials used in the preparation examples and embodiments: silicone emulsion, model: Dowsil 8016; Curing agent: Aradur 3951; Wetting agent: TSF-1700; Dispersant: VK.DP2100; Defoamer: PX-122; Film-forming aid: TEXANOL; Nano alumina dispersion: Nano alumina alcohol dispersion, 5-10nm particle size, 20wt% isopropanol solution; Slag powder: Ultrafine slag powder (specific surface area ≥600 m² / kg); Steel slag powder: Ultrafine steel slag powder (specific surface area ≥600 m² / kg); Sodium silicate: Purchased from Shandong Duofeng Chemical Co., Ltd.; Zinc powder: FZN30; Anti-settling agent: BYK-R605; Cellulose ether: Hydroxypropyl methylcellulose: Purchased from Weifang Lite Composite Materials Co., Ltd.; Basalt flakes (80-100 mesh). Brand: NCE; Quartz powder (300nm); Quartz sand (10-20 mesh); High-alumina cement is aluminate cement, model: CA50-II (G6); Glass powder is low-melting-point glass powder (200-2000 mesh); Hollow glass beads (600 mesh) brand: Senade; Barium sulfate model: CX-325; Aluminum hydroxide purchased from Langfang Pengcai Fine Chemical Co., Ltd.; Silica fume item number: dy88 purchased from Lingshou County Dongyan Mineral Products Co., Ltd.; Light sand is expanded perlite, purchased from Henan Xinyang Changxin Mining Co., Ltd.; FEVE emulsion grade: ZH-01; Nano calcium carbonate model: CCR-6525; Leveling agent is organosilicon leveling agent; Color paste model: LuconylBlack 0066; Organosilicon acrylic resin model: SH-024.

[0030] Unless otherwise specified, all raw materials used in the examples and comparative examples are commercially available products.

[0031] Preparation Example 1 Organosilicon acrylate hybrid epoxy resin: Take 12g butyl acrylate, 5g ethylene glycol dimethacrylate, 1.8g maleic anhydride and 0.3g γ-aminopropyltriethoxysilane, add 38ml ethyl acetate to react, and react at 70℃ for 2h under the action of azobisisobutyronitrile, and discharge to obtain copolymer; at room temperature, add 5g SiO2 sol formed by partial hydrolysis of tetraethyl orthosilicate, then add 10g of E-44 epoxy resin with a mass fraction of 12% and 3g of γ-aminopropyltriethoxysilane with a mass fraction of 4%, stir at room temperature, and after the solvent evaporates, the organosilicon acrylate hybrid epoxy resin is obtained.

[0032] Example 1 A thick coating for steel structures with corrosion resistance and fire resistance comprises the following components: a composite resin-modified zinc-rich primer 2, a heat-insulating and anti-corrosion coating 3, a lightweight fire-resistant coating 4, and a decorative weather-resistant layer 5 sequentially disposed on the surface of a steel substrate 1. The composite resin-modified zinc-rich primer 2 comprises the following components by weight: 100g of composite resin emulsion, 108g of zinc-rich reinforcing powder, 40.9g of curing aid, and 5g of nano-alumina dispersion; wherein the composite resin emulsion is 70g of the organosilicon acrylate hybrid epoxy resin prepared in Preparation Example 1 and 30g of organosilicon emulsion; the zinc-rich reinforcing powder is slag powder, sodium silicate, and zinc powder in a mass ratio of 1.8:1:9; the curing aid is 10g of curing agent, 0.1g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.6g of film-forming aid, and 29.7g of deionized water; The heat-insulating and anti-corrosion coating 3 comprises the following components by mass: 100g of composite resin emulsion, 53.4g of curing aid, 40g of nano-alumina dispersion, 72.2g of active reinforcing powder, 0.5g of anti-settling agent, and 0.5g of cellulose ether. The composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 1.5:1. The active reinforcing powder includes 20g of slag powder, 10g of steel slag powder, 2g of sodium silicate, 15.2g of basalt flakes, and 25g of quartz powder. The mass ratio of the composite resin emulsion, nano-alumina dispersion, and basalt flakes is 2.5:1:0.38. The curing aid consists of 10g of curing agent, 0.3g of wetting agent, 0.4g of dispersant, 0.3g of defoamer, 0.6g of film-forming aid, and 41.8g of deionized water. Lightweight fireproof coating 4: comprises 110g of composite resin emulsion, 103g of lightweight composite powder, 107g of curing aid, and 35g of nano-alumina dispersion; wherein, 80g of the organosilicon acrylate hybrid epoxy resin prepared in Preparation Example 1 and 30g of organosilicon emulsion; the lightweight composite powder consists of 25g of high-alumina cement, 7g of glass powder, 5g of hollow glass beads, 4g of barium sulfate, 10g of aluminum hydroxide, 1g of silica fume, 0.2g of cellulose ether, and 34.7g of light sand; the curing aid includes 9g of curing agent, 0.3g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.5g of film-forming aid, and 23.4g of deionized water; The weather-resistant decorative layer 5 comprises 65g of waterborne silicone acrylate hybrid epoxy resin, 36g of FEVE emulsion, 34g of curing aid, 0.2g of leveling agent, 6g of nano-calcium carbonate, and 4g of color paste; wherein the curing aid includes 9g of curing agent, 0.3g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.5g of film-forming aid, and 23.7g of deionized water; First, mix the composite resin modified zinc-rich primer 2 evenly according to the specified ratio, and apply it evenly to the surface of the steel substrate 1 by roller coating, ensuring a thickness of 2mm. Then, mix the heat insulation and anti-corrosion coating 3 evenly and spray it onto the surface of the composite resin modified zinc-rich primer 2 after drying and curing, ensuring a thickness of 18mm. Next, mix the lightweight fireproof coating 4 evenly and spray it onto the surface of the heat insulation and anti-corrosion coating 3 after drying and curing, ensuring a thickness of 10mm. Finally, mix the finishing weather-resistant layer 5 evenly and spray it onto the surface of the cured lightweight fireproof coating 4, ensuring a thickness of 1mm.

[0033] Example 2 The difference between this embodiment and Embodiment 1 is that the thickness of the composite resin modified zinc-rich primer 2 coating on the surface of the steel substrate 1 is 2mm; the heat insulation and anti-corrosion coating 3 coating is uniformly mixed and sprayed onto the surface of the composite resin modified zinc-rich primer 2 after drying and curing, with a thickness of 18mm; the lightweight fireproof coating 4 coating is uniformly mixed and sprayed onto the surface of the heat insulation and anti-corrosion coating 3 after drying and curing, ensuring a thickness of 20mm; the finishing weather-resistant layer 5 coating is uniformly mixed and sprayed onto the surface of the cured lightweight fireproof coating 4, ensuring a thickness of 1mm.

[0034] Example 3 The difference between this embodiment and Embodiment 1 is that the active enhancement powder also includes 33.5g of quartz sand.

[0035] Example 4 The difference between this embodiment and Embodiment 1 is that the zinc-rich reinforcing powder is slag powder, sodium silicate and zinc powder in a mass ratio of 4:1:11.

[0036] Example 5 The difference between this embodiment and Embodiment 1 is that the zinc-rich reinforcing powder is slag powder, sodium silicate and zinc powder in a mass ratio of 4:1:6.8.

[0037] Example 6 The difference between this embodiment and Example 1 is that the composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 3:1.

[0038] Example 7 The difference between this embodiment and Example 1 is that the composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 1:1.

[0039] Example 8 The difference between this embodiment and Embodiment 1 is that the composite resin emulsion is an organosilicon acrylate resin and an organosilicon emulsion.

[0040] Example 9 The difference between this embodiment and Example 1 is that the heat-insulating and anti-corrosion coating 3 has the following mass components: 72g of composite resin emulsion, 53.4g of curing aid, 40g of nano-alumina dispersion, 72.2g of active reinforcing powder, 0.5g of anti-settling agent, and 0.5g of cellulose ether; wherein, the composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 1.5:1; the active reinforcing powder includes 20g of slag powder, 10g of steel slag powder, 2g of sodium silicate, 15.2g of basalt flakes, and 25g of quartz powder; the mass ratio of composite resin emulsion, nano-alumina dispersion, and basalt flakes is 1.8:1:0.38; the curing aid is 10g of curing agent, 0.3g of wetting agent, 0.4g of dispersant, 0.3g of defoamer, 0.6g of film-forming aid, and 41.8g of deionized water.

[0041] Example 10 The difference between this embodiment and Example 1 is that the heat-insulating and anti-corrosion coating 3 has the following mass components: 100g of composite resin emulsion, 53.4g of curing aid, 24g of nano-alumina dispersion, 72g of active reinforcing powder, 0.5g of anti-settling agent, and 0.5g of cellulose ether; wherein, the composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 1.5:1; the active reinforcing powder includes 20g of slag powder, 10g of steel slag powder, 2g of sodium silicate, 15.2g of basalt flakes, and 25g of quartz powder; the mass ratio of composite resin emulsion, nano-alumina dispersion, and basalt flakes is 2.5:0.6:0.38; the curing aid is 10g of curing agent, 0.3g of wetting agent, 0.4g of dispersant, 0.3g of defoamer, 0.6g of film-forming aid, and 41.8g of deionized water.

[0042] Example 11 The difference between this embodiment and Embodiment 1 is that the weather-resistant decorative layer 5 comprises 65g of waterborne silicone acrylate hybrid epoxy resin, 37.8g of FEVE emulsion, 34g of curing aid, 0.2g of leveling agent, 4.2g of nano-calcium carbonate, and 4g of color paste; wherein the curing aid comprises 9g of curing agent, 0.3g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.5g of film-forming aid, and 23.7g of deionized water.

[0043] Comparative Example 1 The comparative example differs from Example 1 in that the composite resin emulsion is an organosilicon emulsion; Comparative Example 2 The difference between this comparative example and Example 1 is that the heat-insulating and anti-corrosion coating 3 has the following mass components: 100g of composite resin emulsion, 53.4g of curing aid, 72g of active reinforcing powder, 0.5g of anti-settling agent, and 0.5g of cellulose ether; wherein, the composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 1.5:1; the active reinforcing powder includes 20g of slag powder, 10g of steel slag powder, 2g of sodium silicate, 15g of basalt flakes, and 25g of quartz powder; the mass ratio of composite resin emulsion to basalt flakes is 2.5:0.38; the curing aid is 10g of curing agent, 0.3g of wetting agent, 0.4g of dispersant, 0.3g of defoamer, 0.6g of film-forming aid, and 41.8g of deionized water.

[0044] Comparative Example 3 The difference between this comparative example and Example 1 is that the heat-insulating and anti-corrosion coating 3 has the following mass components: 100g of composite resin emulsion, 53.4g of curing aid, 40g of nano-alumina dispersion, 72g of active reinforcing powder, 0.5g of anti-settling agent, and 0.5g of cellulose ether; wherein, the composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 1.5:1; the active reinforcing powder includes 35g of slag powder, 10g of steel slag powder, 2g of sodium silicate, and 25g of quartz powder; the mass ratio of composite resin emulsion to nano-alumina dispersion is 2.5:1; the curing aid is 10g of curing agent, 0.3g of wetting agent, 0.4g of dispersant, 0.3g of defoamer, 0.6g of film-forming aid, and 41.8g of deionized water.

[0045] Comparative Example 4 A thick coating for steel structures with corrosion resistance and fire resistance comprises the following components: a heat-insulating and anti-corrosion coating 3, a lightweight fire-retardant coating 4, and a decorative weather-resistant layer 5 sequentially disposed on the surface of a steel substrate 1. The heat-insulating and anti-corrosion coating 3 comprises the following components by mass: 100g of composite resin emulsion, 53.4g of curing aid, 50g of nano-alumina dispersion, 72g of active reinforcing powder, 0.5g of anti-settling agent, and 0.5g of cellulose ether; wherein the composite resin emulsion has a mass ratio of 1.5: Preparation Example 1: The organosilicon acrylate hybrid epoxy resin and organosilicon emulsion were prepared; the active reinforcing powder included 20g slag powder, 10g steel slag powder, 2g sodium silicate, 15g basalt flakes and 25g quartz powder; the mass ratio of composite resin emulsion, nano alumina dispersion and basalt flakes was 2:1:0.3; the curing aid consisted of 10g curing agent, 0.3g wetting agent, 0.4g dispersant, 0.3g defoamer, 0.6g film-forming aid and 41.8g deionized water; Lightweight fireproof coating 4: comprises 110g of composite resin emulsion, 103g of lightweight composite powder, 107g of curing aid, and 35g of nano-alumina dispersion; wherein, 80g of the organosilicon acrylate hybrid epoxy resin prepared in Preparation Example 1 and 30g of organosilicon emulsion; the lightweight composite powder consists of 25g of high-alumina cement, 7g of glass powder, 5g of hollow glass beads, 4g of barium sulfate, 10g of aluminum hydroxide, 1g of silica fume, 0.2g of cellulose ether, and 34.7g of light sand; the curing aid includes 9g of curing agent, 0.3g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.5g of film-forming aid, and 23.4g of deionized water; The weather-resistant decorative layer 5 comprises 65g of waterborne silicone acrylate hybrid epoxy resin, 36g of FEVE emulsion, 34g of curing aid, 0.2g of leveling agent, 6g of nano-calcium carbonate, and 4g of color paste; wherein the curing aid includes 9g of curing agent, 0.3g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.5g of film-forming aid, and 23.7g of deionized water; Mix the heat-insulating and anti-corrosion coating 3 evenly and spray it onto the surface of the steel substrate 1, ensuring a thickness of 18mm; mix the lightweight fireproof coating 4 evenly and spray it onto the surface of the heat-insulating and anti-corrosion coating 3 after drying and curing, ensuring a thickness of 10mm; mix the finishing and weather-resistant layer 5 evenly and spray it onto the surface of the cured lightweight fireproof coating 4, ensuring a thickness of 1mm.

[0046] Comparative Example 5 A thick coating for steel structures with corrosion resistance and fire resistance comprises the following components: a composite resin-modified zinc-rich primer 2, a heat-insulating and anti-corrosion coating 3, and a lightweight fire-retardant coating 4 sequentially disposed on the surface of a steel substrate 1. The composite resin-modified zinc-rich primer 2 comprises the following components by weight: 100g of composite resin emulsion, 108g of zinc-rich reinforcing powder, 40.9g of curing aid, and 5g of nano-alumina dispersion; wherein the composite resin emulsion is 70g of the organosilicon acrylate hybrid epoxy resin prepared in Preparation Example 1 and 30g of organosilicon emulsion; the zinc-rich reinforcing powder is slag powder, sodium silicate, and zinc powder in a mass ratio of 1.8:1:9; the curing aid is 10g of curing agent, 0.1g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.6g of film-forming aid, and 29.7g of deionized water; The heat-insulating and anti-corrosion coating 3 comprises the following components by mass: 100g of composite resin emulsion, 53.4g of curing aid, 50g of nano-alumina dispersion, 72g of active reinforcing powder, 0.5g of anti-settling agent, and 0.5g of cellulose ether; wherein, the composite resin emulsion is the organosilicon acrylate hybrid epoxy resin and organosilicon emulsion prepared in Preparation Example 1 with a mass ratio of 1.5:1; the active reinforcing powder includes 20g of slag powder, 10g of steel slag powder, 2g of sodium silicate, 15g of basalt flakes, and 25g of quartz powder; the mass ratio of composite resin emulsion, nano-alumina dispersion, and basalt flakes is 2:1:0.3; the curing aid consists of 10g of curing agent, 0.3g of wetting agent, 0.4g of dispersant, 0.3g of defoamer, 0.6g of film-forming aid, and 41.8g of deionized water; Lightweight fireproof coating 4: comprises 110g of composite resin emulsion, 103g of lightweight composite powder, 107g of curing aid, and 35g of nano-alumina dispersion; wherein, 80g of the organosilicon acrylate hybrid epoxy resin prepared in Preparation Example 1 and 30g of organosilicon emulsion; the lightweight composite powder consists of 25g of high-alumina cement, 7g of glass powder, 5g of hollow glass beads, 4g of barium sulfate, 10g of aluminum hydroxide, 1g of silica fume, 0.2g of cellulose ether, and 34.7g of light sand; the curing aid includes 9g of curing agent, 0.3g of wetting agent, 0.3g of dispersant, 0.2g of defoamer, 0.5g of film-forming aid, and 23.4g of deionized water; First, mix the composite resin modified zinc-rich primer 2 evenly according to the specified ratio, and apply it evenly to the surface of the steel substrate 1 by roller coating, ensuring a thickness of 2mm; mix the heat insulation and anti-corrosion coating 3 evenly, and spray it onto the surface of the composite resin modified zinc-rich primer 2 after drying and curing, ensuring a thickness of 18mm; mix the lightweight fireproof coating 4 evenly, and spray it onto the surface of the heat insulation and anti-corrosion coating 3 after drying and curing, ensuring a thickness of 10mm.

[0047] Performance testing The performance tests of the thick coatings with corrosion resistance and fire resistance for steel structures prepared in the examples and comparative examples were conducted using the following methods: Physical and chemical properties, fire resistance, and weather resistance were tested according to GB / T14907-2018; salt spray resistance was tested according to JG / T224-2007 "Anti-corrosion Coatings for Steel Structures in Buildings"; and the bond strength was tested between the composite resin-modified zinc-rich primer and the steel substrate (1) and between the heat-insulating and anti-corrosion coating and the lightweight fire-retardant coating (2). The overall salt spray resistance of the coating (3), and the salt spray resistance of the heat insulation and anti-corrosion coating and the lightweight fireproof coating (4) did not show peeling, bulging, peeling, cracking, red rust and other prolonged effects; Weather resistance test of the finishing weatherproof layer: artificial aging test under xenon lamp for more than 1500 hours; The test results are as follows; The lightweight fireproof coating in Example 1 was burned under a flame of 1200 degrees for 3 hours, and the temperature on the back of the steel plate was 380 degrees; The lightweight fireproof coating in Example 2 was burned under a flame of 1200 degrees for 3 hours, and the temperature on the back of the steel plate was 260 degrees; Table 1 Performance Test Results As shown in Table 1, the thick coating for steel structures obtained in the above embodiments, which has corrosion resistance and fire resistance, not only has excellent fire resistance but also has extremely high salt spray resistance. The coatings have good adhesion and density, and good long-term performance.

[0048] Compared with Examples 6-10 and Example 1, and Comparative Examples 1-3, it is evident that organosilicon acrylate hybrid epoxy resin and organosilicon emulsion exhibit excellent adhesion to various materials and improve the density and impact resistance of resin materials, thereby enhancing the coating's salt spray resistance, acid and alkali resistance, and temperature resistance, ultimately improving the coating's strength and overall corrosion resistance. A certain proportion of composite resin emulsion, nano-alumina dispersion, and basalt flakes ensures that the heat-insulating and anti-corrosion coating maintains good interlayer adhesion and density, forming a barrier layer that can efficiently isolate corrosive media, significantly increasing the difficulty for corrosive media to enter the coating film and improving the heat resistance of the intermediate coating layer. However, if the content of composite resin emulsion is too low, the adhesion performance is insufficient and the strength is poor. If the content of nano-alumina dispersion is too low, the heat resistance is insufficient, and the dispersion of basalt flakes is weak, resulting in poor interfacial interaction with the resin and making it difficult to control the arrangement of basalt flakes, thus affecting the corrosion resistance of the anti-corrosion coating.

[0049] Comparing Examples 1 and 11 with Comparative Example 5, it is evident that adding organosilicon acrylate hybrid epoxy resin to FEVE resin further improves the chemical inertness of the coating surface and introduces a large number of FC bonds, resulting in stronger stability. The introduction of nano-calcium carbonate significantly enhances the density of the cured paint film, preventing chalking and fading, strengthening the weather resistance and color retention of the protective layer, and improving its resistance to various corrosive media. This ensures the entire fireproof system has excellent durability, maintaining its fireproof capability for a long time and extending its service life. Excessive FEVE emulsion content leads to excessive coating rigidity, poor elasticity, unstable performance, insufficient weather resistance, and in severe cases, cracking, peeling, and chalking.

[0050] Comparing Examples 1 and 4-5 with Comparative Example 4, it is evident that the interaction between the inorganic nanomaterial slag powder and sodium silicate in the proportions within the scope of this application cuts off the channels formed by moisture evaporation after resin film formation, significantly improving the sealing effect of the water-based resin coating. Combined with zinc powder, this results in high corrosion resistance to metal surfaces, exhibiting strong adhesion to metal substrates and excellent resistance to salt spray and damp heat. However, insufficient zinc powder content may affect the salt spray resistance of the primer and the overall salt spray resistance of the material.

[0051] The above are all preferred embodiments of this application and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made to the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A thick coating for steel structures with corrosion resistance and fire resistance, characterized in that: The coating comprises a composite resin modified zinc-rich primer (2), a heat-insulating and anti-corrosion coating (3), a lightweight fireproof coating (4), and a decorative weather-resistant layer (5) sequentially disposed on the surface of a steel substrate (1). By weight, the heat-insulating and anti-corrosion coating (3) comprises 80-120 parts of composite resin emulsion, 52.5-76.7 parts of curing aid, 30-40 parts of nano alumina dispersion, 66.5-133.5 parts of active reinforcing powder, 0.3-0.6 parts of anti-settling agent, and 0.3-0.6 parts of cellulose ether. The active reinforcing powder comprises slag powder, steel slag powder, sodium silicate, basalt flakes, and quartz powder. The composite resin modified zinc-rich primer (2) comprises, by weight, 80-120 parts of composite resin emulsion, 92-108 parts of zinc-rich reinforcing powder, 39.3-47.7 parts of curing aid, and 5-8 parts of nano-alumina dispersion; the zinc-rich reinforcing powder comprises slag powder, sodium silicate, and zinc powder. The composite resin emulsion comprises an organosilicon acrylate hybrid epoxy resin and an organosilicon emulsion; The preparation method of the organosilicon acrylate hybrid epoxy resin is as follows: 12g of butyl acrylate, 5g of ethylene glycol dimethacrylate, 1.8g of maleic anhydride and 0.3g of γ-aminopropyltriethoxysilane are added to 38ml of ethyl acetate for reaction. Under the action of azobisisobutyronitrile, the reaction is carried out at 70℃ for 2h, and the copolymer is discharged. At room temperature, 5g of SiO2 sol formed by partial hydrolysis of tetraethyl orthosilicate is added, followed by 10g of E-44 epoxy resin with a mass fraction of 12% and 3g of γ-aminopropyltriethoxysilane with a mass fraction of 4%. The mixture is stirred at room temperature, and the organosilicon acrylate hybrid epoxy resin is obtained after the solvent evaporates.

2. The thick coating with corrosion resistance and fire resistance for steel structures according to claim 1, characterized in that: In the heat-insulating and anti-corrosion coating (3), the mass ratio of organosilicon acrylate hybrid epoxy resin to organosilicon emulsion is (1.5-4):

1.

3. The thick coating with corrosion resistance and fire resistance for steel structures according to claim 1, characterized in that: In the heat-insulating and anti-corrosion coating (3), the mass ratio of the composite resin emulsion, nano alumina dispersion, and basalt flakes is (2-4):1:(0.2-0.45).

4. The thick coating with corrosion resistance and fire resistance for steel structures according to claim 1, characterized in that: The weather-resistant decorative layer (5) comprises 60-70 parts by weight of waterborne silicone acrylate hybrid epoxy resin, 30-40 parts by weight of FEVE emulsion, 33.7-44.7 parts by weight of curing aid, 0.2-0.4 parts by weight of leveling agent, 5-8 parts by weight of nano calcium carbonate, and 3-6 parts by weight of color paste.

5. The thick coating with corrosion resistance and fire resistance for steel structures according to claim 4, characterized in that: The mass ratio of the FEVE emulsion to nano-calcium carbonate is (4-8):

1.

6. The thick coating with corrosion resistance and fire resistance for steel structures according to claim 1, characterized in that: In the composite resin modified zinc-rich primer (2), the mass ratio of slag powder, sodium silicate and zinc powder is (1.8-4):1:(9-16).

Citation Information

Patent Citations

  • Petrochemical water-based high-temperature-resistant, anticorrosive and abrasion-resistant coating and method for preparing same

    CN105885620A

  • Modified water-based organosiloxane-acrylate hybrid resin as well as preparation and application thereof

    CN114133688A