A method for preparing a cell for enhancing the durability of proton ceramic fuel cell for ethylene production by ethane electrolysis and application thereof

By brushing a BZCYYBNRu and NiO catalyst layers onto the anode surface of a proton ceramic fuel cell, the problems of high energy consumption and carbon buildup in ethylene production processes were solved, achieving efficient and stable operation of the battery and high selectivity in the conversion of ethane to ethylene.

CN119776900BActive Publication Date: 2026-11-20NANJING TECH UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411667973.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-20
Publication Date
2026-11-20
Estimated Expiration
2044-11-20

AI Technical Summary

Technical Problem

Traditional ethylene production processes are energy-intensive and difficult to replace, and the problem of carbon buildup in proton ceramic electrochemical cells during the conversion of ethane to ethylene has not been effectively solved.

Method used

A catalyst layer of BZCYYBNRu and NiO was brushed onto the anode surface of a proton ceramic fuel cell using screen printing to form a dense catalyst layer. The anti-carbon deposition performance of the battery was improved by tape casting and sintering treatment.

Benefits of technology

It improves the battery's resistance to carbon buildup and durability, enhances the contact density between the catalyst layer and the anode, and improves the conversion rate and selectivity of ethane electrolysis to ethylene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119776900B_ABST
    Figure CN119776900B_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing and applying a proton ceramic fuel cell to enhance the durability of ethane electrolysis for ethylene production, specifically, a method for brushing a layer of Ba(Zr) onto the anode surface of a proton conductor half-cell obtained by casting and screen printing. 0.1 Ce 0.7 Y 0.1 Yb 0.1 ) 0.9 Ni 0.05 Ru 0.05 O 3‑δ (BZCYYbNRu) is composited with NiO in a certain proportion as a catalyst layer, and co-fired with the half-cell at high temperature. The cathode is a perovskite material, with BaCo as the cathode. 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3‑δ Taking (BCFZY) as an example, by changing the contact method between the catalyst layer and the anode, the density of the catalyst layer is enhanced, thereby improving the battery's resistance to carbon buildup and its durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing and applying a proton ceramic fuel cell for enhancing the durability of ethylene production via ethane electrolysis. Background Technology

[0002] Traditional steam cracking for ethylene production is the most energy-intensive process in the chemical industry, estimated to account for 60% of production costs and two-thirds of the carbon footprint. It is recognized that the optimized methods for ethylene production from ethane or naphtha steam cracking over the past few decades are difficult to replace without significant breakthroughs in process intensification or catalyst science. Among various alternatives, proton ceramic electrochemical cells (PCECs) have emerged as a highly efficient and environmentally friendly method, enabling direct chemical production and energy conversion at intermediate temperatures (400-700°C). In PCECs, during the conversion of ethane to ethylene, hydrogen produced by the dehydrogenation reaction is selectively removed from the product stream via a hydrogen oxidation reaction, forming protons at the anode, which are then transported to the cathode via a proton-conducting electrolyte. Developing cells with high activity, selectivity, and resistance to carbon buildup is crucial for achieving efficient and stable ethylene production via PCECs. Summary of the Invention

[0003] The purpose of this invention is to provide a method for preparing a proton ceramic fuel cell for ethane electrolysis to ethylene that enhances the durability of the fuel cell. The method involves screen printing a catalyst layer BZCYYBNRu onto the anode surface of the fuel cell (prepared by casting method), and then co-firing the two layers to form a dense catalyst layer, thereby improving the battery's resistance to carbon buildup.

[0004] A proton ceramic fuel cell anode includes an anode and a catalyst supported on the surface of the anode, said catalyst being used to convert alkanes into olefins.

[0005] The catalyst is made of Ba(Zr) 0.1 Ce 0.7 Y 0.1 Yb 0.1 ) 0.9 Ni 0.05 Ru 0.05 O 3-δ The composite material is composed of (BZCYYbNRu) and NiO, with a weight ratio ranging from 5 to 10:1.

[0006] The anode material is Ni-BZCYYb.

[0007] A proton ceramic fuel cell includes the aforementioned anode, electrolyte, and cathode.

[0008] The above-mentioned method for preparing the proton ceramic fuel cell anode includes the following steps:

[0009] Step 1: Obtain the anode layer using the tape casting method;

[0010] Step 2: Apply electrolyte to the surface of the anode blank obtained by the casting method using screen printing.

[0011] Step 3: Apply a slurry containing the catalyst to the anode surface by screen printing.

[0012] Step 4: Sintering treatment to densify the anode layer and catalyst layer.

[0013] The slurry also contains NiO powder, and the weight ratio of catalyst to NiO powder is in the range of 5-10:1, and the total mass of catalyst and NiO powder in the slurry is 25-65% by mass.

[0014] The solvent in the slurry is an alcohol solvent, and it also contains dispersants and thickeners.

[0015] Sintering treatment at 1450-1500℃ for 5-15 hours, with a heating rate of 0.5-5℃ / min.

[0016] The screen printing process is repeated 3-5 times.

[0017] The method for producing ethylene by ethane electrolysis includes the following steps:

[0018] Using the above-mentioned proton ceramic fuel cell, a reduction treatment is first performed under H2 atmosphere;

[0019] The anode comes into contact with a carrier gas containing C2H6, N2 and H2O to carry out a catalytic reaction and obtain a product gas containing C2H4.

[0020] The temperature conditions for the catalytic reaction are 650-750℃.

[0021] Beneficial effects

[0022] This invention relates to a method and its application for changing the contact mode between the battery catalyst layer and the anode, enhancing the density of the catalyst layer, and improving the battery's resistance to carbon buildup and durability. Attached Figure Description

[0023] Figure 1 This is a comparison curve of IVP at 650℃-750℃ for batteries with catalyst layers prepared under hydrogen atmosphere and under C2H6 fuel gas atmosphere.

[0024] Figure 2 (a) is a bar chart showing the conversion rate of C2H6 versus the selectivity of C2H4 under OCV conditions. Figure 2 (b) To ensure stable battery operation, add 300-500 mA / cm 2The current is used to ensure that the voltage is around 0.6V at each temperature point, and the bar chart shows the conversion rate of C2H6 and the selectivity of C2H4.

[0025] Figure 3 For comparison, the IVP curves of the catalytic-free battery were tested at 650℃-750℃ in an atmosphere with C2H6 as fuel gas.

[0026] Figure 4 The comparison between cells with and without a catalytic layer at 750℃ and 300 mA / cm 2 The IV stability curve obtained under the current.

[0027] Figure 5 The images show cross-sectional SEM images of the anode and electrolyte before and after testing of the battery with a catalyst layer.

[0028] Figure 6 This is a SEM image of the anode surface after testing the battery with and without a catalyst layer.

[0029] Figure 7 This is a cross-sectional SEM image after the catalyst was sprayed and tested. Detailed Implementation

[0030] Example 1: Preparation of catalyst powder

[0031] This embodiment provides a bimetallic synergistic anode catalyst material, Ba(Zr), for medium- and high-temperature solid oxide fuel cells. 0.1 Ce 0.7 Y 0.1 Yb 0.1 ) 0.9 Ni 0.05 Ru 0.05 O 3-δThe preparation method is as follows: Weigh 5.2268g of barium nitrate, 0.7728g of zirconium nitrate, 5.4712g of cerium nitrate, 0.6894g of yttrium nitrate, 0.8084g of ytterbium nitrate, 0.2908g of nickel nitrate, and 0.26145g of ruthenium chloride, and dissolve them in a small amount of deionized water. Weigh 11.69g of ethylenediaminetetraacetic acid and 16.81g of hydrated citric acid as complexing agents in deionized water according to a molar ratio of ethylenediaminetetraacetic acid: hydrated citric acid: total metal ions of 1:2:1. Add the solution containing the complexing agent to the solution containing the metal ions, and add an appropriate amount of ammonia water dropwise until the pH of the solution reaches 7. Then, stir under magnetic stirring until the water is completely evaporated to obtain a gel-like substance. Place the gel-like substance in an oven and calcine it at 250℃ for 5 hours to obtain the desired foam-like precursor. The precursor was calcined in a high-temperature muffle furnace at 1100℃ for 10 hours to obtain the desired powder. 1.76 g of the obtained powder was mixed with 0.23 g of NiO powder in a high-energy ball mill with ethanol as a solvent, and then dried in an oven at 60℃ to obtain the desired catalyst powder.

[0032] Example 2: Preparation of screen printing paste

[0033] First, prepare the solvent for the paste. Take 50g of terpineol and add 4% ethyl cellulose. Heat and stir at low temperature for 24 hours to obtain the required solvent. Then, take 2g of powder, add 2.4g of solvent and 0.2g of dispersant fish oil to a mortar, and grind by hand for 2-3 hours to obtain the paste required for screen printing.

[0034] Preparation of low-temperature proton ceramic fuel cell cathode material and preparation of single cells in Example 3

[0035] Take 9.8670g Ba(NO3)2, 8.0800g Fe(NO3)3·9H2O, 5.8206g Co(NO3)2·6H2O, 2.1466g Zr(NO3)4·5H2O and 1.9151g Y(NO3)3·6H2O, add an appropriate amount of deionized water to dissolve, stir and heat to dissolve, and after the solution is clear and transparent, add a complexing agent; the complexing agent is 23g EDTA, 43g citric acid CA and 100mL ammonia water. Stir until a clear and dissolved solution is obtained, and use a glass rod to introduce it into a beaker and stir until the solution becomes clear and transparent. The pH of the solution was adjusted to approximately 7 by adding ammonia to the beaker. The solution was then stirred magnetically until all water evaporated, yielding a gel-like substance. The gel was placed in a forced-air drying oven and dried at a constant temperature of 180°C for at least 5 hours to obtain the precursor. The precursor was then calcined at 1000°C for 5 hours at a heating rate of 5°C / min. -1 The desired cathode material powder is obtained.

[0036] The anode preform for the battery was obtained using a casting method. First, 120g of NiO and 80g of BZCYYb were weighed and placed in a pre-prepared ball mill jar. Then, 70g of xylene, 50g of ethanol, and 6g of fish oil were added, and the mixture was ball-milled at high speed in a planetary ball mill for 12 hours. After the first ball milling, 10g of polyethylene glycol-400, 13g of dioctyl phthalate, 2g of cyclohexanone, and 11.5g of polyvinyl butyral were weighed and added to the ball mill jar, and the mixture was ball-milled again in a planetary ball mill for 24 hours. Subsequently, the viscous slurry was transferred to a vacuum defoamer for 5 minutes to remove bubbles. Then, casting was performed, with a casting height of 2mm. Part of the cast tape was allowed to air dry naturally, while the other part was conveyed into a water-filled container for phase transformation treatment for 24 hours. After that, it was dried in an oven at 60℃ to obtain the Ni-BZCYYb cast sheet.

[0037] An electrolyte layer was applied to one side of the obtained anode blank using the formulation of Example 2 via screen printing, and a catalytic coating was applied to the other side to obtain a half-cell. The half-cell was first sintered at 1000°C for 5-10 hours to remove the binder, with a heating rate of 0.5-5°C / min. Then, it was sintered at 1450-1500°C for 5-15 hours, with a heating rate of 0.5-5°C / min, to sinter the cell to a dense state.

[0038] The single cell adopts a BZCYYbNRu+NiO||Ni-BZCYYb||BZCYYb||BCFZY structure for electrochemical testing. The porous BCFZY cathode is prepared by spraying. A certain amount of cathode powder is dissolved in a mixed solution of isopropanol, ethylene glycol, and glycerol, and uniform dispersion is ensured with the aid of a high-energy ball mill. The resulting BCFZY cathode slurry is uniformly sprayed onto the electrolyte side of a preheated bilayer sheet at 200℃ under the impingement of an inert gas. After eight coats of spraying, the cell is calcined at 1000℃ for 2 hours to obtain a single cell. The heating rate is 5℃·min. -1 It is used for electrochemical testing in the temperature range of 650 to 750°C.

[0039] Comparative Example 1

[0040] The difference from Example 3 is that no catalyst layer was printed on the anode side, but all other parameters are the same.

[0041] Comparative Example 2

[0042] The difference from Example 3 is that no catalyst layer was printed on the anode side, while the other parameters were the same. The catalyst layer slurry was obtained by spraying on the anode side. The catalyst layer was made by dissolving a certain amount of BZCYYbNRu catalyst powder in a suitable amount of mixed solution of isopropanol, ethylene glycol and glycerol, and ensuring uniform dispersion with the help of a high-energy ball mill.

[0043] Electrochemical testing

[0044] The prepared single cells were tested using a self-made fuel cell device at 650℃ to 750℃, with tests conducted at 50℃ intervals. The initial test was performed at a rate of 80 mL / min. -1 Hydrogen gas is introduced into the anode side, and the cathode is fed at a rate of 80 mL / min. -1 High-purity air was introduced for reduction. After reduction, the battery was tested using a Digital Source Meter (Keithley 2420) in four-probe mode to collect IV polarization curves. Then, the anode inlet gas was switched to 20% C2H6, 60% N2, and 20% water vapor, and the same Digital Source Meter (Keithley 2420) was used for testing.

[0045] Conversion rate test

[0046] When the anode inlet gas was switched to 20% C2H6, 60% N2, and 20% water vapor, the water vapor was liquid water pumped in quantitatively via a vaporization pump, then sent through a carrier gas into a heated and insulated gas pipeline, and finally into the reaction apparatus. The product measured at the anode was condensed to remove water before being introduced into a chromatograph for quantitative analysis of its composition. The gas flow rate of the product was measured using a soap bubble flow meter.

[0047] Stability test

[0048] The cells with and without the catalyst layer were heated to 750℃ using H2 at a flow rate of 80 ml / min. After cell reduction, the anode atmosphere was switched to 20% C2H6, 60% N2, and 20% water vapor, respectively. A current of 300 mA / cm² was applied to each cell. 2 The rated current is recorded, and the voltage change curve IV is recorded.

[0049] Characterization results

[0050] Output power characterization

[0051] Figure 1 The image shows the IVP (Input Power Output) curves of the prepared catalytic layer battery at 650℃-750℃, tested in a hydrogen atmosphere and an atmosphere using C2H6 as fuel gas. At 750℃, the battery output power in hydrogen atmosphere is 985 mW·cm⁻¹. -2 It achieves the general performance of a conventional anode-supported single cell without a catalyst layer under H2 conditions. After switching the anode inlet gas to 20% C2H6, 60% N2, and 20% water vapor, the power at 750℃ was measured to be 449 mW·cm⁻¹. -2 303 mW·cm at 700℃·h -2 200mW·cm at 650℃·h -2 ,and Figure 3 The performance of the uncatalyzed solar cell, measured with an anode inlet gas of 20% C2H6, 60% N2, and 20% water vapor (i.e., 750℃), was 369 mW·cm⁻¹. -2 294 mW·cm at 700℃·h -2 At 650℃·hour, the value is 120mW·cm. -2 Compared to conventional electrolyte-supported batteries, there is a slight improvement, while compared to conventional electrolyte-supported batteries, there is a significant improvement.

[0052] Conversion rate testing characterization

[0053] The battery was measured under OCV operation conditions. Figure 2 The (a)C2H6 conversion at 750 °C was 35.1%, and the selectivity for C2H4 was 78.4%, which is consistent with the increase of 450 mA / cm measured in the same cell. 2 The current was measured when the battery voltage was around 0.6. Figure 2 (b) Compared to the C2H6 conversion rate of 37.6% and the C2H4 selectivity of 95.4%, both showed a certain degree of improvement after the addition of current, and the same situation was observed at other temperature points.

[0054] Stability testing characterization

[0055] Figure 4 Tests show that the battery without a catalyst layer rapidly decreases from 0.7V within 10 hours after the current is applied and the battery starts working, while the battery with a catalyst layer maintains a voltage of around 0.73V within 80 hours. The battery's stability is greatly improved, which proves that the addition of a catalyst layer can change the contact mode between the catalyst layer and the anode, enhance the density of the catalyst layer, and improve the battery's resistance to carbon buildup and durability.

[0056] SEM characterization

[0057] Figure 5 Figure 'ab' shows cross-sectional views of the catalyst layer and electrolyte side before and after the battery test, and Figure 'cd' shows SEM images of the cross-sections on both sides after the test. The images show that the catalyst layer is about 13μm thick after three coats of brushing. After the test, a certain amount of porosity was restored to ensure the passage of hydrogen gas, and there was no sign of the catalyst layer peeling off after the test.

[0058] Figure 6 Image 'a' is a SEM image of the anode surface after testing the catalyst-free battery. The image shows agglomeration of many black substances on the surface, indicating carbon deposition in the battery. Figure 6 Image b is an SEM image of the catalyst layer surface after the catalytic cell test. It can be seen that the catalyst layer surface is intact and no serious carbon deposition was found.

[0059] Figure 7The image shows a cross-sectional SEM image after the catalyst was sprayed. The battery was completely pulverized, and the boundary of the cross-section was no longer visible. It can be seen that the battery obtained by the spraying method is basically consistent with the test results without catalyst, and the blocking effect on C2H6 gas is too weak.

Claims

1. A method for producing ethylene by electrolysis of ethane, characterized in that, Includes the following steps: (1) Preparation of proton ceramic fuel cells: NiO powder and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The powders are mixed and then cast to obtain a NiO-BZCYYb anode blank. A BZCYYb electrolyte layer is screen-printed onto one side of the anode preform, and a catalyst slurry containing Ba(Zr) is screen-printed onto the other side of the anode preform. 0.1 Ce 0.7 Y 0.1 Yb 0.1 ) 0.9 Ni 0.05 Ru 0.05 O 3-δ and NiO, and Ba(Zr 0.1 Ce 0.7 Y 0.1 Yb 0.1 ) 0.9 Ni 0.05 Ru 0.05 O 3-δ The weight ratio of NiO to NiO is 5-10:1; The anode blank coated with the electrolyte layer and catalyst slurry is subjected to a debinding treatment at 1000℃ for 5-10 h, and then sintered at 1450-1500℃ for 5-15 h, so that the catalyst slurry forms a catalyst layer loaded on the surface of the anode support layer and co-fired and bonded to the anode support layer. The heating rates of the debinding treatment and sintering treatment are 0.5-5℃ / min, respectively. A cathode is disposed on the side of the electrolyte layer away from the anode support layer, thereby obtaining a proton ceramic fuel cell comprising a catalyst layer, an anode support layer, an electrolyte layer, and a cathode in sequence; (2) The proton ceramic fuel cell is subjected to reduction treatment in H2 atmosphere to reduce NiO in the anode support layer to Ni; (3) The catalyst layer of the reduced proton ceramic fuel cell is brought into contact with a mixed gas containing C2H6, N2 and H2O, and an electric current is applied to the proton ceramic fuel cell at 650-750°C to carry out an electrochemical catalytic reaction to obtain gas containing C2H4.

2. The method for producing ethylene by ethane electrolysis according to claim 1, characterized in that, The Ba(Zr) 0.1 Ce 0.7 Y 0.1 Yb 0.1 0.9Ni 0.05 Ru 0.05 O 3-δ The total mass of NiO accounts for 25-65% of the mass of the catalyst slurry.

3. The method for producing ethylene by ethane electrolysis according to claim 1, characterized in that, The catalyst slurry uses terpineol as a solvent, fish oil as a dispersant, and contains ethyl cellulose as a thickener.

4. The method for producing ethylene by ethane electrolysis according to claim 1, characterized in that, The catalyst slurry is screen-printed on the surface of the anode preform 3-5 times.

5. The method for producing ethylene by ethane electrolysis according to claim 1, characterized in that, The cathode is BaCo. 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ Porous cathode.

6. The method for producing ethylene by ethane electrolysis according to claim 1, characterized in that, The mixed gas comprises 20% C2H6, 60% N2 and 20% water vapor by volume.

7. The method for producing ethylene by ethane electrolysis according to claim 1, characterized in that, The current density applied to the proton ceramic fuel cell is 300-500 mA / cm². 2 And maintain the voltage of the proton ceramic fuel cell at 0.6 V.

Citation Information

Patent Citations

  • Ethylene and electric energy symbiotic solid oxide fuel cell and preparation method thereof

    CN113299960A