Electrolytic cell and method for the production of aluminum alloys by low temperature molten salt electrolysis

By using low-temperature molten salt electrolysis, an electrolysis process based on chloride salts, the problems of cumbersome and energy-intensive aluminum alloy production have been solved, achieving efficient and low-cost aluminum alloy preparation. The content of alloying elements can be controlled, and it is suitable for the production of various types of aluminum alloys.

CN119776911BActive Publication Date: 2026-11-20NORTHEASTERN UNIV CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510128224.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-02-05
Publication Date
2026-11-20
Estimated Expiration
2045-02-05

AI Technical Summary

Technical Problem

Existing aluminum alloy production processes are cumbersome, energy-intensive, costly, and cause serious environmental pollution. Traditional molten salt electrolysis methods suffer from problems such as low current efficiency, low alloy element content, and unstable electrolysis.

Method used

A low-temperature molten salt electrolysis method was adopted, using chloride salts as the molten salt system, chlorides of alloying elements as raw materials, and solid aluminum as a consumable cathode. Aluminum alloys with different compositions were prepared by controlling the electrolysis temperature and the composition of the molten salt system.

Benefits of technology

It achieves low-energy consumption and high-efficiency aluminum alloy preparation, with controllable alloy element content, low cost, and uniform alloy composition, and is suitable for the production of various types of aluminum alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119776911B_ABST
    Figure CN119776911B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of fused salt electrolysis, and particularly relates to an electrolytic cell and a method for preparing aluminum alloy by low-temperature fused salt electrolysis. The electrolytic cell comprises a cell shell, a cover plate, a heat preservation layer, a bottom insulation layer, an auxiliary heating device, a gas recovery device, a cathode guide rod, an anode guide rod, a consumable cathode and an anode lining. The method uses chlorinated salt as a fused salt system, chlorides of alloying elements as raw materials, and solid aluminum as a consumable cathode to perform electrolysis. During the electrolysis process, alloying elements are deposited on the surface of the solid aluminum at the cathode and are alloyed with the aluminum matrix to form aluminum alloy. Different components of aluminum alloy can be prepared by controlling the electrolysis temperature and the components of the fused salt system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of molten salt electrolysis technology, specifically relating to an electrolytic cell and method for preparing aluminum alloys by low-temperature molten salt electrolysis. Background Technology

[0002] Aluminum alloys have excellent material properties such as light weight, good shock absorption, high specific strength, high machinability, good biocompatibility, and corrosion resistance. They are widely used in automobiles, aerospace, defense, biomedicine, and electronic components. Currently, aluminum alloys are mainly produced by blending aluminum with other elements in a certain proportion in the molten state. The production of aluminum alloys using this method has advantages such as simple equipment, mature technology, and easy operation, but there are also many problems: (1) The production process is complicated: Before production, both aluminum and alloying elements need to go through their respective metallurgical processes, and then the target alloy is obtained through secondary or even multiple smelting; (2) The metal burn-off rate is high: Oxidation burn-off is serious during the heating and smelting process; especially for some highly active alloying elements, such as magnesium and lithium, the production cost of aluminum alloys is high; (3) High energy consumption and large environmental pollution.

[0003] Many aluminum alloys, such as aluminum-magnesium and aluminum-lithium alloys, can also be produced using molten salt electrolysis. However, the traditional molten salt electrolysis method for producing aluminum-magnesium alloys uses fluoride as the molten salt system, magnesium oxide as the raw material, and molten aluminum as the cathode. Although magnesium oxide is inexpensive and has a low-cost advantage, its low solubility in fluoride salts results in low magnesium content in the produced aluminum-magnesium alloys. It also easily leads to anodic effects during electrolysis, resulting in low current efficiency and high energy consumption. Molten salt electrolysis for producing aluminum-lithium alloys uses chloride as the molten salt system, lithium chloride or lithium carbonate as the raw material, and molten aluminum as the cathode. Using lithium carbonate as the raw material can significantly reduce the cell voltage, but lithium carbonate has poor solubility in chloride molten salts and easily produces elemental carbon after prolonged electrolysis, affecting continuous operation. Given these drawbacks, researchers have been exploring more economical and environmentally friendly methods for producing aluminum alloys. Summary of the Invention

[0004] To address the aforementioned problems, this invention proposes an electrolytic cell and method for preparing aluminum alloys via low-temperature molten salt electrolysis. This method uses chloride salts as the molten salt system, chlorides of alloying elements as raw materials, and solid aluminum as the consumable cathode for electrolysis. During electrolysis, alloying elements precipitate on the surface of the solid aluminum cathode and alloy with the aluminum matrix to form aluminum alloys. By controlling the electrolysis temperature and the composition of the molten salt system, aluminum alloys with different compositions can be prepared.

[0005] The technical solution of this invention is: An electrolytic cell for preparing aluminum alloys by low-temperature molten salt electrolysis is disclosed. The electrolytic cell includes a tank shell, a cover plate, a heat insulation layer, a bottom insulation layer, an auxiliary heating device, a gas recovery device, a cathode guide rod, an anode guide rod, a consumable cathode, and an anode liner. The outermost part of the electrolytic cell is the tank shell, and a heat insulation layer is provided close to the inner wall of the tank shell. A cover plate is provided on the top of the tank shell, with outlets for liquid aluminum alloy, cathode guide rods, and gas recovery devices. The bottom insulation layer and the anode liner are provided inside the heat insulation layer. The anode liner is attached to the side wall of the heat insulation layer. The bottom of the anode liner is connected to the bottom insulation layer and sealed. The anode guide rod is connected to the anode liner. The consumable cathode is connected to the cathode guide rod by threads. The gas recovery device is located at the gas recovery device outlet of the cover plate, and a liquid aluminum alloy outlet cover plate is provided at the liquid aluminum alloy outlet. The electrolytic cell contains molten electrolyte with a height of 50-100 cm. An auxiliary heating device is provided on the side of the electrolytic cell 30-60 cm away from the cover plate to control the electrolysis temperature.

[0006] Furthermore, in the aforementioned low-temperature molten salt electrolysis method for preparing aluminum alloys, the electrolytic cell is cylindrical or cuboid in shape; the cell shell is made of steel plate with a thickness of 5-10 mm; the insulation layer is constructed from one or more of mullite bricks, clay bricks, alumina bricks, and calcium silicate boards, with a thickness of 20-40 cm; the cover plate has an upper layer of steel plate and a lower layer of insulation material, the insulation material being one of alumina, mullite, calcium silicate, and clay, with a cover plate thickness of 10-20 cm.

[0007] Furthermore, in the aforementioned electrolytic cell for preparing aluminum alloys by low-temperature molten salt electrolysis, the cover plate is in a closed state when liquid aluminum alloy is not discharged or when the consumable cathode does not need to be replaced, and can be opened to perform the operations of discharging liquid aluminum alloy and replacing the consumable cathode when liquid aluminum alloy is discharged or when the consumable cathode needs to be replaced.

[0008] Furthermore, in the aforementioned electrolytic cell for preparing aluminum alloys by low-temperature molten salt electrolysis, the anode liner is made of carbonaceous material, with a height of 30-100 cm and a thickness of 5-10 cm. The carbonaceous material is petroleum coke, graphite, or calcined anthracite. The bottom insulating layer connected to the anode liner is made of one of corundum, silicon nitride combined with silicon carbide, or aluminum oxide, with a thickness of 5-10 cm and a height of 10-40 cm. The consumable cathode is made of pure aluminum, in the shape of a cylinder or cuboid, and is connected to the cathode guide rod by a thread. The pure aluminum is primary aluminum obtained by electrolysis. The anode guide rod is connected to the anode liner by a thread or by casting with phosphorus iron. After the connection is completed, the anode guide rod opening is sealed and insulated.

[0009] Furthermore, in the aforementioned low-temperature molten salt electrolysis method for preparing aluminum alloys, during electrolysis, the metal electrochemically generated by the consumable cathode first forms on the aluminum consumable cathode and reacts with the aluminum to form an alloy of the metal and aluminum. As electrolysis proceeds, the content of this element in the aluminum alloy increases. When the melting point of the alloy is reached, the alloy melts and drips from the surface of the aluminum consumable cathode to the bottom of the electrolysis cell, forming an aluminum alloy molten pool. When the aluminum consumable cathode is consumed to a certain extent, the consumable cathode is replaced. When the amount of aluminum alloy molten pool at the bottom reaches a certain level, a portion of the aluminum alloy melt is extracted from the bottom of the electrolysis cell using a vacuum ladle. The extracted aluminum alloy is then simply refined and cast into ingots for use as the master alloy for aluminum alloy production. During electrolysis, the electrolysis temperature in the electrolysis cell is controlled by an auxiliary heating device, thereby controlling the content of alloying elements in the generated aluminum alloy.

[0010] A method for preparing aluminum alloys by low-temperature molten salt electrolysis is disclosed. After the electrolytic cell is constructed, it is first heated to above 600°C using gas. Then, the electrolyte is heated to its electrolysis temperature outside the cell and melted before being poured into the cell. A consumable cathode, either an aluminum ingot or a plate, is installed on the cell, which is then sealed. Electrolysis is then carried out. During electrolysis, raw materials are added to the molten electrolyte in molten or solid form every 0.5 hours, depending on the current intensity of the cell. The consumable cathode is replaced every 10-48 hours. Every 5-36 hours, aluminum alloy is vacuum-lifted from the bottom of the cell, ensuring the liquid aluminum alloy level is 2-5 cm below the anode substrate. The main components of the cathode residue are aluminum and alloying elements. This cathode residue is remelted and recast into a consumable cathode for reuse. The electrolyte composition and electrolysis process vary depending on the type of aluminum alloy being prepared during electrolysis.

[0011] Furthermore, in the aforementioned method for preparing aluminum alloys via low-temperature molten salt electrolysis, magnesium chloride is used as the raw material for preparing aluminum-magnesium alloys. The molten salt electrolyte used for electrolysis is a chloride molten salt system mainly composed of NaCl-KCl-MgCl2, MgCl2-KCl, and MgCl2-NaCl. Alkali metal or alkaline earth metal chlorides CaCl2 and LiCl can also be added. The molar percentage of each substance in the electrolyte is: NaCl: 20-80%, KCl: 20-80%, MgCl2: 0-40%, CaCl2: 0-20%, LiCl: 0-20%. The initial crystallization temperature of the electrolyte is controlled at 400-600℃, the electrolysis temperature is 450-640℃ during electrolysis, and the current density of the anode liner is 0.2-0.7 A / cm². 2During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Magnesium chloride is electrolyzed into metallic magnesium, which precipitates on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-magnesium alloy. When the magnesium content in the aluminum-magnesium alloy is 0-70 wt.%, the aluminum-magnesium alloy drips to the bottom of the electrolytic cell in a liquid state. During electrolysis, by adjusting the electrolyte composition and electrolysis temperature, aluminum-magnesium alloys with a magnesium content of 0-70 wt.% are prepared. The aluminum-magnesium alloy melt obtained at the bottom of the electrolytic cell is taken out of the electrolytic cell by vacuum lifting. The aluminum-magnesium alloy taken out of the electrolytic cell is poured into a mixing furnace for refining to obtain an aluminum-magnesium master alloy. After dilution with aluminum and addition of alloying elements, various types of aluminum alloys can be prepared from this aluminum-magnesium master alloy.

[0012] Furthermore, in the aforementioned method for preparing aluminum-lithium alloys via low-temperature molten salt electrolysis, lithium chloride is used as the raw material. The molten salt electrolyte used for electrolysis is an alkali metal chloride molten salt system mainly composed of NaCl-KCl-LiCl, LiCl-KCl, and LiCl-NaCl. The molar percentages of each substance in the electrolyte are: NaCl: 20-80%, KCl: 10-80%, and LiCl: 20-50%. The initial crystallization temperature of the electrolyte is controlled at 550-600℃. During electrolysis, the electrolysis temperature is 590-650℃, and the current density in the anode liner is 0.2-0.7 A / cm². 2 During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Lithium chloride is electrolyzed into metallic lithium, which precipitates on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-lithium alloy. When the lithium content in the aluminum-lithium alloy is 0-10 wt.%, the aluminum-lithium alloy drips to the bottom of the electrolytic cell in a liquid state. During electrolysis, by adjusting the electrolyte composition and electrolysis temperature, an aluminum-lithium alloy with a lithium content of 0-10 wt.% is prepared. The aluminum-lithium alloy melt obtained at the bottom of the electrolytic cell is taken out of the electrolytic cell by vacuum lifting. The aluminum-lithium alloy taken out of the electrolytic cell is poured into a mixing furnace for refining to obtain an aluminum-lithium intermediate alloy. This aluminum-lithium intermediate alloy can be diluted with aluminum and alloying elements to prepare various types of aluminum alloys.

[0013] Furthermore, in the aforementioned method for preparing aluminum alloys via low-temperature molten salt electrolysis, zinc chloride is used as the raw material for preparing aluminum-zinc alloys. The molten salt electrolyte used for electrolysis is a chloride molten salt system mainly composed of NaCl-KCl-ZnCl2, ZnCl2-NaCl, and ZnCl2-KCl. The molar percentages of each substance in the electrolyte are: NaCl: 20-80%, KCl: 10-80%, and ZnCl2: 10-25%. The initial crystallization temperature of the electrolyte is controlled at 350-550℃. During electrolysis, the electrolysis temperature is 350-550℃, and the current density in the anode liner is 0.2-0.7 A / cm². 2During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Zinc chloride is electrolyzed into metallic zinc, which is deposited on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-zinc alloy. When the zinc content in the aluminum-zinc alloy is 0-80 wt.%, the aluminum-zinc alloy drips to the bottom of the electrolytic cell in liquid form. During the electrolysis process, by adjusting the electrolyte composition and electrolysis temperature, an aluminum-zinc alloy with a zinc content of 0-80 wt.% can be prepared.

[0014] Furthermore, in the aforementioned method for preparing aluminum alloys via low-temperature molten salt electrolysis, calcium oxide is used as the raw material for preparing aluminum-calcium alloys. The molten salt electrolyte used for electrolysis is a chloride molten salt system mainly composed of NaCl-KCl-CaCl2, CaCl2-NaCl, and CaCl2-KCl. The molar percentages of each substance in the electrolyte are: NaCl: 20-70%, KCl: 10-70%, CaCl2: 20-70%, and CaO: 1-10%. The initial crystallization temperature of the electrolyte is controlled at 450-550℃, and during electrolysis, the electrolysis temperature is 550-590℃, and the current density in the anode liner is 0.2-0.7 A / cm². 2 During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Calcium oxide is electrolyzed into metallic calcium, which precipitates on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-calcium alloy. When the calcium content in the aluminum-calcium alloy reaches more than 40%, the aluminum-calcium alloy drips into the bottom of the electrolytic cell in a liquid state. During the electrolysis process, by adjusting the electrolyte composition and electrolysis temperature, an aluminum-calcium alloy with a calcium content of more than 40 wt.% can be prepared.

[0015] Advantages and beneficial effects of the present invention: The method for preparing aluminum-magnesium, aluminum-lithium, aluminum-zinc, and aluminum-calcium alloys offers advantages such as low energy consumption, high and controllable magnesium / lithium content, minimal magnesium / lithium loss, uniform composition, and low cost. Furthermore, the produced alloys, after simple refining and the addition of alloying elements, can be used to prepare various types of aluminum alloy products. In addition, this method can also be applied to the production of other aluminum alloys, and the low-temperature molten salt electrolysis method used in this project shows promising application prospects. Attached Figure Description

[0016] Figure 1 This is a front view of the rectangular electrolytic cell structure of the present invention; Figure 2 This is a top view (AA) of the rectangular electrolytic cell structure of the present invention. Figure 3 This is a top view (BB) of the rectangular electrolytic cell structure of the present invention. Figure 4 This is a front view of the cylindrical electrolytic cell structure of the present invention; Figure 5This is a top view (AA) of the cylindrical electrolytic cell structure of the present invention. Figure 6 This is a top view (BB) of the cylindrical electrolytic cell structure of the present invention. In the figure, 1-liquid aluminum alloy outlet cover; 2-cathode guide rod; 3-gas collection device; 4-anode liner; 5-cover plate; 6-insulation layer; 7-auxiliary heating device; 8-electrolyte; 9-liquid aluminum alloy; 10-bottom insulation layer; 11-tank shell; 12-anode guide rod; 13-consumable cathode. Detailed Implementation

[0017] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The purity of LiCl, NaCl, KCl, and MgCl2 used in the following examples is ≥98%. The following examples are for illustrative purposes only and should not be used to limit the scope of the present invention.

[0018] Example 1

[0019] This embodiment describes an electrolytic cell for the low-temperature molten salt electrolysis preparation of aluminum alloys, such as... Figure 1-3 As shown, the electrolytic cell includes a shell 11, a cover plate 5, a heat insulation layer 6, a bottom insulation layer 10, an auxiliary heating device 7, a gas recovery device 3, a cathode guide rod 2, an anode guide rod 12, a consumable cathode 13, and an anode liner 4. The electrolytic cell is rectangular in shape, with the outermost part being the shell 11. The heat insulation layer 6 is provided close to the inner wall of the shell 11. The top of the shell 11 is provided with a cover plate 5, which has outlets for liquid aluminum alloy, cathode guide rods, and the gas recovery device. The insulation layer 6 contains a bottom insulation layer 10 and an anode liner 4. The anode liner 4 is attached to the side wall of the insulation layer 6. The bottom of the anode liner 4 is connected to the bottom insulation layer 10 and sealed. The anode guide rod 12 is connected to the anode liner 4. The consumable cathode 13 is connected to the cathode guide rod 12 by a thread. The gas recovery device 3 is located at the gas recovery device port of the cover plate 5. The liquid aluminum alloy outlet is provided with a liquid aluminum alloy outlet cover 1 plate. The electrolytic cell contains molten electrolyte with a height of 50 cm. An auxiliary heating device 7 is provided on the side of the electrolytic cell 30 cm below the cover plate 5 to control the electrolysis temperature. The trough shell 11 is made of steel plate with a thickness of 5 mm; the insulation layer is made of mullite bricks with a thickness of 20 cm; the cover plate 5 has a steel plate on the upper layer and an insulation material on the lower layer, the insulation material is alumina, and the cover plate 5 has a thickness of 10 cm. The cover plate 5 is in a closed state when liquid aluminum alloy is not discharged or when the consumable cathode 13 does not need to be replaced. It can be opened to discharge liquid aluminum alloy or replace the consumable cathode 13 when liquid aluminum alloy is discharged or when the consumable cathode 13 needs to be replaced. The anode liner 4 is made of carbonaceous material, with a height of 30 cm and a thickness of 5 cm. The carbonaceous material is petroleum coke. The bottom insulating layer 10 connected to the anode liner 4 is made of corundum, with a thickness of 5 cm and a height of 10 cm. The consumable cathode 13 is made of pure aluminum, in the shape of a cuboid, and is connected to the cathode guide rod 2 by a thread. The pure aluminum is primary aluminum obtained by electrolysis. The anode guide rod 12 is connected to the anode liner 4 by a thread. After the connection is completed, the anode guide rod opening is sealed and insulated.

[0020] Example 2

[0021] This embodiment describes an electrolytic cell for the low-temperature molten salt electrolysis preparation of aluminum alloys, such as... Figure 4-6 As shown, the electrolytic cell includes a shell 11, a cover plate 5, a heat insulation layer 6, a bottom insulation layer 10, an auxiliary heating device 7, a gas recovery device 3, a cathode guide rod 2, an anode guide rod 12, a consumable cathode 13, and an anode liner 4. The electrolytic cell is cylindrical in shape, with the outermost part being the shell 11. A heat insulation layer 6 is provided close to the inner wall of the shell 11. A cover plate 5 is provided on the top of the shell 11, and the cover plate 5 has a liquid aluminum alloy outlet, a cathode guide rod outlet, and a gas recovery device outlet. The insulation layer 6 contains a bottom insulation layer 10 and an anode liner 4. The anode liner 4 is attached to the side wall of the insulation layer 6. The bottom of the anode liner 4 is connected to the bottom insulation layer 10 and sealed. The anode guide rod 12 is connected to the anode liner 4. The consumable cathode 13 is connected to the cathode guide rod 12 by a thread. The gas recovery device 3 is located at the gas recovery device port of the cover plate 5. The liquid aluminum alloy outlet is provided with a liquid aluminum alloy outlet cover 1 plate. The electrolytic cell contains molten electrolyte with a height of 50 cm. An auxiliary heating device 7 is provided on the side of the electrolytic cell 30 cm below the cover plate 5 to control the electrolysis temperature. The trough shell 11 is made of steel plate with a thickness of 5 mm; the insulation layer is made of clay bricks with a thickness of 20 cm; the cover plate 5 has a steel plate on the upper layer and an insulation material on the lower layer, the insulation material being mullite, and the cover plate 5 having a thickness of 10 cm. The cover plate 5 is in a closed state when liquid aluminum alloy is not discharged or when the consumable cathode 13 does not need to be replaced. It can be opened to discharge liquid aluminum alloy or replace the consumable cathode 13 when liquid aluminum alloy is discharged or when the consumable cathode 13 needs to be replaced. The anode liner 4 is made of carbonaceous material, with a height of 30 cm and a thickness of 5 cm. The carbonaceous material is graphite. The bottom insulating layer 10 connected to the anode liner 4 is made of corundum, with a thickness of 5 cm and a height of 10 cm. The consumable cathode 13 is made of pure aluminum, is cylindrical in shape, and is connected to the cathode guide rod 2 by a thread. The pure aluminum is primary aluminum obtained by electrolysis. The anode guide rod 12 is connected to the anode liner 4 by casting with phosphorus iron. After the connection is completed, the anode guide rod opening is sealed and insulated.

[0022] Example 3

[0023] This embodiment describes a method for preparing aluminum-magnesium alloys using the electrolytic cell of Example 1. The specific steps of this method are as follows: A molten salt system was prepared with 40 MgCl2-32.5 KCl-27.5 NaCl (mol %), and a 5 mm thick aluminum plate was used as the consumable cathode. After the electrolytic cell is constructed, it is first heated to 600℃ using gas. Then, the electrolyte is heated to its electrolysis temperature outside the cell and melted before being poured into the cell. The consumable cathode is then installed on the cell, which is sealed. Electrolysis is then initiated by applying electricity. During electrolysis, the initial crystallization temperature of the electrolyte is controlled at 450℃, the electrolysis temperature is controlled at 475℃, and the current density inside the anode lining is 0.2 A / cm². 2 The electrolysis time is 3 h. MgCl2 raw material is added to the molten electrolyte in molten form every 0.5 h. The consumable cathode is replaced every 10 h. The aluminum alloy is lifted out from the bottom of the electrolytic cell by vacuum every 5 h to ensure that the liquid surface of the liquid aluminum alloy is 2 cm away from the bottom of the anode substrate. After electrolysis, the aluminum-magnesium alloy at the bottom of the electrolytic cell was removed, and after ultrasonic cleaning, the weight percentage of magnesium was measured to be 34.1%.

[0024] Example 4

[0025] This embodiment describes a method for preparing aluminum-magnesium alloys using the electrolytic cell of Example 1. The specific steps of this method are as follows: A molten salt system was prepared with 25 MgCl2-55 KCl-20 NaCl (mol %), and an aluminum plate with a thickness of 5 mm was used as the consumable cathode. After the electrolytic cell is constructed, it is first heated to 600℃ using gas. Then, the electrolyte is heated to its electrolysis temperature outside the cell and melted before being poured into the cell. The consumable cathode is then installed on the cell, which is sealed. Electrolysis is then initiated by applying electricity. During electrolysis, the initial crystallization temperature of the electrolyte is controlled at 530℃, the electrolysis temperature is controlled at 550℃, and the current density inside the anode lining is 0.2 A / cm². 2 The electrolysis time is 3 h. MgCl2 raw material is added to the molten electrolyte in molten or solid form every 0.5 h. The consumable cathode is replaced every 10 h. The aluminum alloy is lifted out from the bottom of the electrolytic cell by vacuum every 5 h to ensure that the liquid surface of the liquid aluminum alloy is 2 cm away from the bottom of the anode substrate. After electrolysis, the aluminum-magnesium alloy at the bottom of the electrolytic cell was removed, and after ultrasonic cleaning, the weight percentage of magnesium was measured to be 19.8%.

[0026] Example 5

[0027] This embodiment describes a method for preparing aluminum-lithium alloy using the electrolytic cell of Example 1. The specific steps of this method are as follows: A molten salt system was prepared with 40LiCl-60KCl (mol%), and an aluminum plate with a thickness of 5 mm was used as the consumable cathode. After the electrolytic cell is constructed, it is first heated to 600℃ using gas. Then, the electrolyte is heated to its electrolysis temperature outside the cell and poured into the cell. The consumable cathode is installed on the cell, which is then sealed. Electrolysis is then carried out by applying electricity. During electrolysis, the initial crystallization temperature of the electrolyte is controlled at 580℃, the electrolysis temperature is controlled at 600℃, and the current density inside the anode lining is 0.3 A / cm². 2 The electrolysis time is 3 h. LiCl raw material is added to the molten electrolyte in molten form every 0.5 h. The consumable cathode is replaced every 10 h. The aluminum alloy is lifted out from the bottom of the electrolytic cell by vacuum every 5 h to ensure that the liquid surface of the liquid aluminum alloy is 2 cm away from the bottom of the anode substrate. After electrolysis, the aluminum-lithium alloy at the bottom of the electrolytic cell was removed, and after ultrasonic cleaning, the weight percentage of lithium was measured to be 9.3%.

[0028] Example 6

[0029] This embodiment describes a method for preparing aluminum-lithium alloy using the electrolytic cell of Example 1. The specific steps of this method are as follows: A molten salt system was prepared with 30 LiCl-70 NaCl (mol %), and an aluminum plate with a thickness of 5 mm was used as the consumable cathode. After the electrolytic cell is constructed, it is first heated to 600℃ using gas. Then, the electrolyte is heated to its electrolysis temperature outside the cell and melted before being poured into the cell. The consumable cathode is then installed on the cell, which is sealed. Electrolysis is then carried out by applying electricity. During electrolysis, the initial crystallization temperature of the electrolyte is controlled at 620℃, the electrolysis temperature is controlled at 640℃, and the current density inside the anode lining is 0.3 A / cm². 2 The electrolysis time is 3 h. LiCl raw material is added to the molten electrolyte in molten form every 0.5 h. The consumable cathode is replaced every 10 h. The aluminum alloy is lifted out from the bottom of the electrolytic cell by vacuum every 5 h to ensure that the liquid surface of the liquid aluminum alloy is 2 cm away from the bottom of the anode substrate. After electrolysis, the aluminum-lithium alloy at the bottom of the electrolytic cell was removed, and after ultrasonic cleaning, the weight percentage of lithium was measured to be 3.8%.

[0030] Example 7

[0031] This embodiment describes a method for preparing aluminum-zinc alloy using the electrolytic cell of Example 1. The specific steps of this method are as follows: A molten salt system was prepared using 20 ZnCl2 - 40 NaCl - 40 KCl (mol %), and a 5 mm thick aluminum plate was used as the consumable cathode. After the electrolytic cell is constructed, it is first heated to 600℃ using gas. Then, the electrolyte is heated to its electrolysis temperature outside the cell and melted before being poured into the cell. The consumable cathode is then installed on the cell, which is sealed. Electrolysis is then carried out by applying electricity. During electrolysis, the initial crystallization temperature of the electrolyte is controlled at 520℃, the electrolysis temperature is controlled at 550℃, and the current density inside the anode lining is 0.3 A / cm². 2 The electrolysis time is 3 h. Every 0.5 h, raw material ZnCl2 is added to the molten electrolyte in molten form. The consumable cathode is replaced every 10 h. Every 5 h, aluminum alloy is lifted out from the bottom of the electrolytic cell by vacuum to ensure that the liquid surface of the liquid aluminum alloy is 2 cm away from the bottom of the anode substrate. After electrolysis, the aluminum-zinc alloy at the bottom of the electrolytic cell was removed, and after ultrasonic cleaning, the weight percentage of zinc was measured to be 74.6%.

[0032] Example 8

[0033] This embodiment describes a method for preparing aluminum-calcium alloy using the electrolytic cell of Example 1. The specific steps of this method are as follows: A molten salt system was prepared with 48 CaCl2 - 50 NaCl - 2CaO (mol %), and an aluminum plate with a thickness of 5 mm was used as the consumable cathode. After the electrolytic cell is constructed, it is first heated to 600℃ using gas. Then, the electrolyte is heated to its electrolysis temperature outside the cell and melted before being poured into the cell. The consumable cathode is then installed on the cell, which is sealed. Electrolysis is then carried out by applying electricity. During electrolysis, the initial crystallization temperature of the electrolyte is controlled at 510℃, the electrolysis temperature is controlled at 550℃, and the current density inside the anode lining is 0.3 A / cm². 2 The electrolysis time is 3 h. CaCl2 is added to the molten electrolyte in molten form every 0.5 h. The consumable cathode is replaced every 10 h. The aluminum alloy is lifted out from the bottom of the electrolytic cell by vacuum every 5 h to ensure that the liquid surface of the liquid aluminum alloy is 2 cm away from the bottom of the anode substrate. After electrolysis, the aluminum-calcium alloy at the bottom of the electrolytic cell was removed, and after ultrasonic cleaning, the weight percentage of calcium was measured to be 62.7%.

Claims

1. An electrolytic cell for preparing aluminum alloys by low-temperature molten salt electrolysis, characterized in that, The electrolytic cell includes a shell, a cover plate, an insulation layer, a bottom insulation layer, an auxiliary heating device, a gas recovery device, a cathode guide rod, an anode guide rod, a consumable cathode, and an anode liner. The outermost part of the electrolytic cell is the shell, with an insulation layer located close to the inner wall of the shell. A cover plate is installed on the top of the shell, with outlets for liquid aluminum alloy, cathode guide rods, and the gas recovery device. Inside the insulation layer are the bottom insulation layer and the anode liner. The anode liner is fitted to the side wall of the insulation layer, and the bottom of the anode liner is connected to the bottom insulation layer and sealed. The anode guide rod is connected to the anode liner, and the consumable cathode is connected to the cathode guide rod via threads. The gas recovery device is located at the gas recovery device outlet on the cover plate, and a liquid aluminum alloy outlet cover plate is provided at the liquid aluminum alloy outlet. The electrolytic cell contains molten electrolyte with a height of 50-100 cm. An auxiliary heating device is located on the side of the electrolytic cell 30-60 cm from the cover plate to control the electrolysis temperature. The anode liner is made of carbonaceous material, with a height of 30-100 cm and a thickness of 5-10 cm. The carbonaceous material is petroleum coke, graphite, or calcined anthracite. The bottom insulating layer connected to the anode liner is made of one of corundum, silicon nitride combined with silicon carbide, or aluminum oxide, with a thickness of 5-10 cm and a height of 10-40 cm. The consumable cathode is made of pure aluminum, in the shape of a cylinder or cuboid, and is connected to the cathode guide rod by a thread. The pure aluminum is primary aluminum obtained by electrolysis. The anode guide rod is connected to the anode liner by a thread or by casting with phosphorus iron. After the connection is completed, the anode guide rod opening is sealed and insulated.

2. The electrolytic cell for preparing aluminum alloys by low-temperature molten salt electrolysis according to claim 1, characterized in that, The electrolytic cell is cylindrical or cuboid in shape; the cell shell is made of steel plate with a thickness of 5-10 mm; the insulation layer is constructed of one or more of mullite bricks, clay bricks, alumina bricks, and calcium silicate boards, with a thickness of 20-40 cm; the cover plate has a steel plate as the upper layer and an insulation material as the lower layer, which is made of one of alumina, mullite, calcium silicate, and clay, with a thickness of 10-20 cm.

3. The electrolytic cell for preparing aluminum alloys by low-temperature molten salt electrolysis according to claim 2, characterized in that, The cover plate is in a closed state when liquid aluminum alloy is not discharged or when the consumable cathode does not need to be replaced, and can be opened to discharge liquid aluminum alloy or replace the consumable cathode.

4. The electrolytic cell for preparing aluminum alloys by low-temperature molten salt electrolysis according to claim 1, characterized in that, During electrolysis, the metal electrochemically generated by the consumable cathode first forms on the aluminum consumable cathode and reacts with the aluminum to form an alloy of the metal and aluminum. As electrolysis proceeds, the content of this element in the aluminum alloy increases. When the melting point of the alloy is reached, the alloy melts and drips from the surface of the aluminum consumable cathode to the bottom of the electrolytic cell to form an aluminum alloy molten pool. When the aluminum consumable cathode is consumed to a certain extent, the consumable cathode is replaced. When the amount of molten aluminum alloy in the bottom pool reaches a certain level, a portion of the molten aluminum alloy is extracted from the bottom of the electrolytic cell using a vacuum ladle. The extracted aluminum alloy is then cast into ingots after simple refining and used as the master alloy for aluminum alloy production. During the electrolysis process, the electrolysis temperature in the electrolytic cell is controlled by an auxiliary heating device, thereby controlling the content of alloying elements in the generated aluminum alloy.

5. A method for preparing aluminum alloys by low-temperature molten salt electrolysis, characterized in that, After the electrolytic cell is constructed, it is first heated to over 600℃ using gas. Then, the electrolyte is heated to the electrolysis temperature outside the cell and melted before being poured into the cell. The consumable cathode aluminum ingot or plate is then installed on the cell, which is sealed, and electrolysis is initiated by energizing the cells. During electrolysis, raw materials are added to the molten electrolyte in molten or solid form every 0.5 hours, depending on the current intensity of the cell. The consumable cathode is replaced every 10-48 hours, and the aluminum alloy is vacuum-lifted from the bottom of the cell every 5-36 hours, ensuring that the liquid aluminum alloy level is 2-5 cm below the anode substrate. The main components of the cathode residue are aluminum and alloying elements. This cathode residue is remelted and recast into a consumable cathode for reuse. The electrolyte composition and electrolysis process vary depending on the type of aluminum alloy being prepared during electrolysis.

6. The method for preparing aluminum alloys by low-temperature molten salt electrolysis according to claim 5, characterized in that, In the preparation of aluminum-magnesium alloys, magnesium chloride is used as the raw material. The molten salt electrolyte used for electrolysis is a chloride molten salt system mainly composed of NaCl-KCl-MgCl2, MgCl2-KCl, and MgCl2-NaCl. Alkali metal or alkaline earth metal chlorides CaCl2 and LiCl can also be added. The molar percentage of each substance in the electrolyte is: NaCl: 20-80%, KCl: 20-80%, MgCl2: 0-40%, CaCl2: 0-20%, LiCl: 0-20%. The initial crystallization temperature of the electrolyte is controlled at 400-600℃. During electrolysis, the electrolysis temperature is 450-640℃, and the current density in the anode liner is 0.2-0.7 A / cm². 2 During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Magnesium chloride is electrolyzed into metallic magnesium, which precipitates on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-magnesium alloy. When the magnesium content in the aluminum-magnesium alloy is 0-70 wt.%, the aluminum-magnesium alloy drips to the bottom of the electrolytic cell in a liquid state. During electrolysis, by adjusting the electrolyte composition and electrolysis temperature, aluminum-magnesium alloys with a magnesium content of 0-70 wt.% are prepared. The aluminum-magnesium alloy melt obtained at the bottom of the electrolytic cell is taken out of the electrolytic cell by vacuum lifting. The aluminum-magnesium alloy taken out of the electrolytic cell is poured into a mixing furnace for refining to obtain an aluminum-magnesium master alloy. After dilution with aluminum and addition of alloying elements, various types of aluminum alloys can be prepared from this aluminum-magnesium master alloy.

7. The method for preparing aluminum alloys by low-temperature molten salt electrolysis according to claim 5, characterized in that, In the preparation of aluminum-lithium alloys, lithium chloride is used as the raw material. The molten salt electrolyte used for electrolysis is an alkali metal chloride molten salt system mainly composed of NaCl-KCl-LiCl, LiCl-KCl, and LiCl-NaCl. The molar percentage of each substance in the electrolyte is NaCl: 20-80%, KCl: 10-80%, and LiCl: 20-50%. The initial crystallization temperature of the electrolyte is controlled at 550-600℃. During electrolysis, the electrolysis temperature is 590-650℃, and the current density in the anode liner is 0.2-0.7 A / cm². 2 During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Lithium chloride is electrolyzed into metallic lithium, which precipitates on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-lithium alloy. When the lithium content in the aluminum-lithium alloy is 0-10 wt.%, the aluminum-lithium alloy drips to the bottom of the electrolytic cell in a liquid state. During electrolysis, by adjusting the electrolyte composition and electrolysis temperature, an aluminum-lithium alloy with a lithium content of 0-10 wt.% is prepared. The aluminum-lithium alloy melt obtained at the bottom of the electrolytic cell is taken out of the electrolytic cell by vacuum lifting. The aluminum-lithium alloy taken out of the electrolytic cell is poured into a mixing furnace for refining to obtain an aluminum-lithium master alloy. This aluminum-lithium master alloy can be diluted with aluminum and alloying elements to prepare various types of aluminum alloys.

8. The method for preparing aluminum alloys by low-temperature molten salt electrolysis according to claim 5, characterized in that, In the preparation of aluminum-zinc alloys, zinc chloride is used as the raw material. The molten salt electrolyte used for electrolysis is a chloride molten salt system mainly composed of NaCl-KCl-ZnCl2, ZnCl2-NaCl, and ZnCl2-KCl. The molar percentages of each substance in the electrolyte are: NaCl: 20-80%, KCl: 10-80%, and ZnCl2: 10-25%. The initial crystallization temperature of the electrolyte is controlled at 350-550℃. During electrolysis, the electrolysis temperature is 350-550℃, and the current density in the anode liner is 0.2-0.7 A / cm². 2 During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Zinc chloride is electrolyzed into metallic zinc, which is deposited on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-zinc alloy. When the zinc content in the aluminum-zinc alloy is 0-80 wt.%, the aluminum-zinc alloy drips to the bottom of the electrolytic cell in liquid form. During the electrolysis process, by adjusting the electrolyte composition and electrolysis temperature, an aluminum-zinc alloy with a zinc content of 0-80 wt.% can be prepared.

9. The method for preparing aluminum alloys by low-temperature molten salt electrolysis according to claim 5, characterized in that, In the preparation of aluminum-calcium alloys, calcium oxide is used as the raw material. The molten salt electrolyte used for electrolysis is a chloride molten salt system mainly composed of CaO-NaCl-KCl-CaCl2, CaO-CaCl2-NaCl, and CaO-CaCl2-KCl. The molar percentages of each substance in the electrolyte are: NaCl: 20-70%, KCl: 10-70%, CaCl2: 20-50%, and CaO: 1-10%. The initial crystallization temperature of the electrolyte is controlled at 450-550℃, and during electrolysis, the electrolysis temperature is 550-590℃, and the current density in the anode liner is 0.2-0.7 A / cm². 2 During electrolysis, the consumable cathode aluminum is suspended in solid form in the molten salt electrolyte. Calcium oxide is electrolyzed into metallic calcium, which precipitates on the surface of the consumable cathode aluminum and combines with aluminum to form an aluminum-calcium alloy. When the calcium content in the aluminum-calcium alloy reaches more than 40%, the aluminum-calcium alloy drips into the bottom of the electrolytic cell in a liquid state. During the electrolysis process, by adjusting the electrolyte composition and electrolysis temperature, an aluminum-calcium alloy with a calcium content of more than 40 wt.% can be prepared.

Citation Information

Patent Citations

  • Method for producing aluminium-lithium alloy with high lithium content by low-temperature molten salt electrolysis

    CN101643921A

  • Aluminum-lithium-samarium alloy and fused salt electrolysis preparation method thereof

    CN101886197A

  • Device and method for preparing aluminum-rare earth alloy through floating special-shaped cathode molten salt electrolysis

    CN116516440A

  • Electrolytic cell for override recovery of pure aluminum from scrap aluminum and use method of electrolytic cell