Galena composite collector and preparation method and application thereof

The composite collector composed of alcohol black, methyl isoamyl xanthate and propanol has solved the problem of efficient lead recovery in lead-zinc ore, improved lead grade and recovery rate, and reduced zinc cross-contamination. It is highly adaptable and easy to operate.

CN119793709BActive Publication Date: 2026-11-24GUANGXI ZHONGJIN LINGNAN MINING CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411945259.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-27
Publication Date
2026-11-24
Estimated Expiration
2044-12-27

AI Technical Summary

Technical Problem

Existing technologies are insufficient for achieving efficient lead recovery in complex and difficult-to-process lead-zinc ores, and traditional collectors have shortcomings in terms of selectivity and collectability.

Method used

A composite collector for galena, composed of alcohol black, methyl isoamyl xanthate and propanol, is applied to the lead-zinc ore flotation process after being uniformly mixed. Combined with inhibitors and frothers, it forms small and stable bubbles to improve lead recovery.

Benefits of technology

It improves lead recovery and selectivity over a wide pH range, increasing lead grade by 0.15%-2.00% and recovery by 1.25%-7.69%, while reducing zinc inclusion in lead concentrate. The operation is simple and reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to a composite collector for galena, its preparation method, and its application. The composite collector, by weight, consists of 15-80 parts of alcohol black, 20-95 parts of methyl isopentyl xanthate, and 90-150 parts of propanol. By distributing alcohol black, methyl isopentyl xanthate, and propanol in a specific ratio, this invention can improve the collection efficiency and selectivity of lead through the synergistic effect between the components, effectively increasing the lead recovery rate while reducing the zinc content in lead concentrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of mineral processing technology, and more specifically, to a galena composite collector, its preparation method, and its application. Background Technology

[0002] Metallic lead is chemically stable, has good corrosion resistance, and is soft and easy to process. It has a wide range of industrial applications, primarily in the manufacture of lead-acid batteries, alloys, cable sheaths, corrosion-resistant linings, and radiation shields. Galena is the most important lead mineral in the industry, and it often occurs in association with sphalerite to form lead-zinc ore. Therefore, flotation of lead-zinc ore is usually required to enrich galena and obtain lead concentrate. The lead concentrate is then further smelted to produce metallic lead. The performance of the galena collector is crucial for achieving the goal of enriching galena.

[0003] Based on the characteristics and occurrence of galena, it is of great significance to achieve efficient lead recovery in complex and difficult-to-process lead-zinc ores by using simple and reasonable compound reagents to obtain synergistic collection effects and improve the flotation efficiency of minerals. Summary of the Invention

[0004] Based on this, the present invention provides a composite collector for galena, which can improve the separation effect of lean, fine and impure lead-zinc ores, with good selectivity for lead and high lead recovery rate.

[0005] To achieve the above objectives, the present invention provides the following solution:

[0006] A composite collector for galena, by weight, is composed of 15-80 parts of alcohol black, 20-95 parts of methyl isopentyl xanthate and 90-150 parts of propanol.

[0007] In some embodiments, the mass ratio of the alcohol black powder to the methyl isopentyl xanthate is 3:1-9.

[0008] In some embodiments, the galena composite collector is composed of 20-77 parts by weight of alcohol black, 25-80 parts by weight of methyl isopentyl xanthate, and 100-130 parts by weight of propanol.

[0009] In some embodiments, the alcohol black is di-sec-butyl dithiophosphate; more specifically, the alcohol black is sodium di-sec-butyl dithiophosphate.

[0010] This invention also provides a method for preparing the above-mentioned galena composite collector, the method comprising the following steps:

[0011] Alcohol black, methyl isopentyl xanthate, and propanol are mixed in a certain proportion and stirred evenly at a temperature of 25-35°C to obtain the galena composite collector.

[0012] This invention also provides the application of the above-mentioned galena composite collector in mineral processing, the application comprising the following steps:

[0013] After grinding the raw ore to a fineness of -0.074mm particle size of 75%, a slurry is prepared. Then, an inhibitor, a galena composite collector, and a frother are added, and the foam is scraped off to obtain a rough lead concentrate. Then, a galena composite collector is added to the slurry, and the foam is scraped off to obtain a lead concentrate and tailings. The rough lead concentrate and the lead concentrate are combined to obtain the final lead concentrate.

[0014] In some embodiments, the inhibitor is sodium sulfite, added at a rate of 250-300 g / t; the foaming agent is 2 # Oil, added at a rate of 25-40 g / t; the first collector added at a rate of 70-100 g / t, and the second collector added at a rate of 30-50 g / t.

[0015] In some embodiments, the Pb grade in the ore is below 1.0%, and the Zn grade is 3.0-5.0%; preferably, the Pb grade is 0.3-1.0%.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0017] This invention uses alcohol black, methyl isopentyl xanthate, and propanol as raw material components of a composite collector for galena. Through the synergistic effect between the components, the collection capacity and selectivity of galena are improved, resulting in good separation effect.

[0018] The galena composite collector of the present invention can float lead in a wide pH range (7-13), has strong adaptability to the on-site flotation environment, and can form small and stable bubbles during the flotation process, which is beneficial to improving the lead recovery rate.

[0019] The galena composite collector of the present invention can enhance the selectivity and collection of lead minerals with close intercalation relationship under the premise of similar or less dosage. Compared with the traditional galena collector, the lead grade is increased by 0.15%-2.00%, the recovery rate is increased by 1.25%-7.69%, and the zinc content in lead concentrate is reduced.

[0020] The raw materials for the galena composite collector of the present invention are readily available, the preparation is simple and reliable, the properties are stable, and the on-site operation is convenient. Detailed Implementation

[0021] Numerous specific details are set forth in the following description to provide a full understanding of the invention. However, the invention can be practiced in many other ways different from those described herein, and similar modifications can be made by those skilled in the art without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0023] Example 1

[0024] A composite collector for galena, by weight, is composed of 75 parts of sodium disec-butyl dithiophosphate, 25 parts of methyl isopentyl xanthate and 110 parts of propanol.

[0025] Its preparation includes the following steps:

[0026] Sodium disec-butyl dithiophosphate, methyl isopentyl xanthate, and propanol were weighed according to the stated weight proportions, mixed, and stirred at 30°C for 4.5 hours to ensure uniform mixing of the raw materials, thus obtaining the galena composite collector.

[0027] Example 2

[0028] A composite collector for galena, by weight, is composed of 50 parts of sodium disec-butyl dithiophosphate, 50 parts of methyl isopentyl xanthate and 110 parts of propanol.

[0029] Its preparation method is the same as that of Example 1.

[0030] Example 3

[0031] A composite collector for galena, by weight, is composed of 26 parts of sodium disec-butyl dithiophosphate, 75 parts of methyl isopentyl xanthate and 110 parts of propanol.

[0032] Its preparation method is the same as that of Example 1.

[0033] Application Example 1

[0034] The galena composite collectors obtained in Examples 1-3 were applied to the flotation of lead-zinc ore. The specific beneficiation process is as follows:

[0035] After grinding the raw ore to a fineness of -0.074 mm with 75% particle size, 300 g / t of sodium sulfite inhibitor, 80 g / t of the galena composite collector prepared in the example, and 2 g / t of frother were added. # 25-40 g / t of oil was used to scrape off the foam to obtain lead rough concentrate. Then, 40 g / t of the galena composite collector prepared in the example was added to the slurry. The foam was scraped off to obtain lead concentrate and tailings. The lead rough concentrate and lead concentrate were combined to obtain the final lead concentrate.

[0036] Application Example 2

[0037] The flotation process in this application example is the same as that in Application Example 1. The collector is the galena composite collector prepared in Example 2. The only difference is that the depressant in this application example is lime, and its dosage is 1.5-2 kg / t. The specific process flow is as follows:

[0038] After grinding the raw ore to a fineness of -0.074mm particle size of 75%, 1.5-2 kg / t of lime, 80 g / t of collector, and 2 # 25-40g / t of oil is added to the slurry, and the foam is scraped to obtain lead rough concentrate; then 40g / t of collector is added to the slurry, and the foam is scraped to obtain lead concentrate and tailings. The lead rough concentrate and lead concentrate are combined to obtain the final lead concentrate.

[0039] Comparative Example 1

[0040] The collector used in this comparative example is a conventional galena-based combined collector of butyl xanthate and ethyl thiocyanate. The flotation process is the same as that used in Application Example 2, the only difference being that the collector and its ratio in this comparative example is butyl xanthate + ethyl thiocyanate (1:1), with a total dosage of 140 g / t. The specific process flow is as follows:

[0041] After grinding the raw ore to a fineness of -0.074mm particle size of 75%, 1.5-2 kg / t of lime, 100 g / t of the collector described in Comparative Example 1, and 2 # 25-40 g / t of oil was added to the slurry, and the foam was scraped to obtain lead rough concentrate. Then, 40 g / t of the collector described in Comparative Example 1 was added to the slurry, and the foam was scraped to obtain lead concentrate and tailings. The lead rough concentrate and lead concentrate were combined to obtain the final lead concentrate.

[0042] Comparative Example 2

[0043] The collector used in this comparative example is a conventional galena-based combined collector of butanol black and ethyl xanthate. The flotation process is the same as that in Application Example 1, the only difference being that the collector and its ratio in this comparative example is butanol black + ethyl xanthate (2:1), with a total dosage of 140 g / t. The specific process flow is as follows:

[0044] After grinding the raw ore to a fineness of -0.074mm particle size of 75%, 300g / t of sodium sulfite inhibitor, 100g / t of the collector described in Comparative Example 2, and 2g / t of frother were added. # 25-40 g / t of oil is added to the slurry to obtain lead rough concentrate. Then, 40 g / t of the collector described in Comparative Example 2 is added to the slurry and the lead concentrate and tailings are obtained by scraping the foam. The lead rough concentrate and lead concentrate are combined to obtain the final lead concentrate.

[0045] The results of flotation tests using the collectors in the examples and the comparative examples are shown in Table 1.

[0046] Table 1. Lead capture effects of Examples 1-3 and Comparative Examples 1-2

[0047]

[0048] The data in Table 1 show that conventional galena composite collectors have poor selectivity, making it difficult to balance collectability and selectivity. However, the galena composite collector provided by this invention can improve the lead grade and recovery rate of lead concentrate under both natural pH and high alkaline conditions, while reducing the zinc content in lead concentrate. It also exhibits good selectivity and collectability for lead at lower dosages.

[0049] In summary, the beneficiation index of lead concentrate products can be further improved by adjusting the weight ratio of raw materials in the collector of this invention.

[0050] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0051] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. Use of a galena composite collector in the beneficiation of lead-zinc ores, characterized in that, It comprises the following steps: After grinding the raw ore to a fineness of-0.074mm particle size accounting for 75%, a slurry is prepared, then a depressant, a galena composite collector and a foaming agent are added, and a lead rough concentrate is obtained by scraping bubbles; then the galena composite collector is added to the slurry, and a lead concentrate and a tailing are obtained by scraping bubbles, and the lead rough concentrate and the lead concentrate are combined to obtain a final lead concentrate; The galena composite collector consists of 20-77 parts of alcohol black by weight, 25-80 parts of methyl isopentyl xanthate and 100-130 parts of propanol; The mass ratio of the alcohol black to the methyl isopentyl xanthate is 3:1-3; The alcohol black is sodium di-sec-butyl dithiophosphate; The inhibitor is sodium sulfite, added in an amount of 250-300 g / t; the frother is 2 # oil, added in an amount of 25-40 g / t; the first collector is added in an amount of 70-100 g / t, and the second collector is added in an amount of 30-50 g / t; The grade of Pb in the raw ore is below 1.0%, and the grade of Zn is 3.0-5.0%.

2. Use of the complex galena collector of claim 1 in the beneficiation of lead-zinc ores, characterized by, The alcohol black is sodium di-sec-butyl dithiophosphate.

3. Use of the complex galena collector of claim 1 in the beneficiation of lead-zinc ores, characterized by, The preparation method of the galena composite collector comprises the following steps: The alcohol black, the methyl isopentyl xanthate and the propanol are mixed in a proportion, and stirred uniformly at a temperature of 25-35℃ to obtain the galena composite collector.

Citation Information

Patent Citations

  • Method for recovering valuable elements in electrolytic manganese leaching residues

    CN115074541A