Aluminum alloy composite sheet and preparation method and application thereof
Aluminum alloy composite sheets processed with specific components and techniques have solved the problem of balancing aesthetics and strength, enabling the application of high-strength and aesthetically pleasing electronic product exterior components.
Patent Information
- Application Number
- CN202411933680.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-26
AI Technical Summary
Existing aluminum alloy sheets are difficult to balance aesthetics and strength in electronic products, especially 6-series and 7-series aluminum alloys, where aesthetics and strength conflict after oxidation.
A composite sheet is made up of a first aluminum alloy layer and a second aluminum alloy layer with specific component contents. Through extrusion, online quenching, stretching and artificial aging treatment, AlMgSi(Cu) phase and MgZn₂ phase are formed to improve the overall performance and peel strength of the material.
This technology enables aluminum alloy composite panels to maintain aesthetic appeal while possessing high mechanical strength and peel strength, making them suitable for electronic product exterior components.
Smart Images

Figure CN119795696B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy technology, and in particular to an aluminum alloy composite sheet, its preparation method, and its application. Background Technology
[0002] Aluminum alloys have relatively low density, are inexpensive, have moderate hardness, and possess a certain degree of corrosion resistance. Currently, aluminum alloy sheets are mainly used in the electronics industry as exterior casings (generally, 6-15mm thick sheets are CNC machined with grooves to protect the product, and electronic components are installed within these grooves). During application, the surface is anodized to improve corrosion resistance and aesthetics. Depending on the type of aluminum alloy used, there are generally 6-series aluminum alloys with a strength of 300-400MPa and a relatively aesthetically pleasing anodized finish, or 7-series aluminum alloys with higher strength of 400-500MPa but a slightly less aesthetically pleasing finish after anodizing. When using 6- and 7-series aluminum alloys as exterior components in electronic products, ensuring the aesthetics after anodizing is generally achieved by reducing the addition of alloying elements and achieving a high degree of solid solution. Therefore, aesthetics and strength are conflicting and difficult to balance.
[0003] Therefore, it is necessary to develop an aluminum alloy sheet that combines both aesthetics and strength. Summary of the Invention
[0004] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the first aspect of the present invention proposes an aluminum alloy composite sheet that can balance mechanical strength and aesthetics.
[0005] A second aspect of the present invention also provides a method for preparing an aluminum alloy composite sheet.
[0006] A third aspect of the present invention also provides an application of aluminum alloy composite sheet.
[0007] According to a first aspect of the present invention, an aluminum alloy composite plate is provided, the aluminum alloy composite plate comprising a first aluminum alloy layer and a second aluminum alloy layer connected in sequence;
[0008] By mass percentage, the composition of the first aluminum alloy layer includes Si: 0.4%–1.2%, Fe ≤ 0.1%, Cu: 0.4%–1.1%, Mn ≤ 0.1%, Mg: 0.7%–1.2%, Cr ≤ 0.1%, Zn: 0.1%–0.25%, other impurities < 0.1%, and the balance being Al;
[0009] The composition of the second aluminum alloy layer, by mass percentage, includes Si≤0.2%, Fe≤0.4%, Cu:1.0%~2.5%, Mn≤0.3%, Mg:1.4%~2.6%, Cr≤0.1%, Zn:4%~6%, other impurities <0.1%, and the balance being Al.
[0010] The aluminum alloy composite sheet according to embodiments of the present invention has at least the following beneficial effects:
[0011] The present invention comprises an aluminum alloy composite plate composed of a first aluminum alloy layer and a second aluminum alloy layer with specific component contents. The aluminum alloy composite plate has aesthetic appeal and high mechanical strength, and the first aluminum alloy layer and the second aluminum alloy layer have high peel strength.
[0012] Furthermore, in the first aluminum alloy layer described in this invention, Cu can improve the dispersion of the precipitated phase, forming an AlMgSi(Cu) phase together with Mg and Si. Simultaneously, Cu partially contributes to solid solution strengthening. This solid solution strengthening alters the lattice arrangement of the material, reducing the anisotropy caused by the addition of Mn and improving the appearance after oxidation. The Cu used in this invention is controlled within the range of 0.4% to 1.1%, resulting in better overall alloy performance. While adding a certain amount of Cu typically increases deformation resistance during extrusion, this invention utilizes this property to reduce the difference in flowability during extrusion caused by the difference in deformation resistance between the first and second aluminum alloy layers.
[0013] Furthermore, in the first aluminum alloy layer described in this invention, Mn and Cr are usually used as refining elements. They are difficult to dissolve in the matrix during extrusion and are distributed in the casting rod in a fine and dispersed state. During oxidation, they cause a potential difference with the surrounding matrix, resulting in an increase in corrosion points. Therefore, this invention limits the mass percentage of Mn and Cr elements to below 0.1%.
[0014] Furthermore, in the first aluminum alloy layer described in this invention, Fe is an unavoidable harmful impurity in the alloy. It is often in the form of coarse compound morphology. During extrusion deformation, it breaks and elongates, and is arranged linearly along the deformation direction. It is distributed inside the grains and on the grain boundaries, which will reduce the appearance effect after oxidation. Therefore, this invention limits the Fe element mass percentage to below 0.1%.
[0015] Furthermore, in the first aluminum alloy layer described in this invention, Zn has a relatively high binding energy with quenched vacancies. After quenching, Zn can combine with the vacancies, serving as nucleation sites for Mg-Si atomic clusters and accelerating the aging response of the alloy. This facilitates coordination with the aging process of the second aluminum alloy layer. However, excessive Zn addition can lead to poor corrosion resistance of the material matrix and affect the anodized appearance. Therefore, the Zn content used in this invention is controlled within the range of 0.1%-0.25%.
[0016] Furthermore, in the second aluminum alloy layer described in this invention, Mg and Zn serve as the main strengthening elements, forming MgZn2 and Al2Mg2Zn3 phases, which have high solubility in aluminum and change drastically with temperature fluctuations. MgZn2 exhibits a strong aging response effect, leading to a greater difference in aging precipitation efficiency between the first aluminum alloy layer and the aging heat treatment side. Increased Mg and Zn content results in increased strength and hardness. Therefore, this invention comprehensively considers product performance and the aging heat treatment process, controlling the amount of Mg and Zn added within the range defined by this invention.
[0017] According to a preferred embodiment of the present invention, in the first aluminum alloy layer, the mass ratio of Mg to Si is (0.6 to 1.55):1. This results in the formation of sufficient Mg₂Si precipitates for strengthening, and also provides interfacial bonding ability, thereby improving peel strength.
[0018] According to a preferred embodiment of the present invention, the Cu content in the second aluminum alloy layer is 1.2% to 1.5%. This prevents the difference in high-temperature fluidity between the first and second aluminum alloy layers from causing poor interfacial bonding.
[0019] According to a preferred embodiment of the present invention, in the second aluminum alloy layer, the mass ratio of Zn to Mg is ≥2.2; and the mass percentage of Cu is greater than the mass percentage of Mg. This forms a CuMgAl2 phase, which improves the alloy strength.
[0020] According to a second aspect of the present invention, a method for preparing the aluminum alloy composite plate described in the first aspect of the present invention is provided, comprising the following steps:
[0021] S1. Prepare ingot A from each component of the first aluminum alloy layer; prepare ingot B from each component of the second aluminum alloy layer;
[0022] S2. Cut the ingot A into a semicircle A; cut the ingot B into a semicircle B; combine the semicircles A and B and heat them to obtain an aluminum rod;
[0023] S3. Place the aluminum rod in an extrusion die for extrusion; then perform online quenching, stretching and artificial aging treatment in sequence to obtain the final product.
[0024] The method for preparing aluminum alloy composite plates according to embodiments of the present invention has at least the following beneficial effects:
[0025] This invention prepares aluminum alloy composite plates by casting, extruding, online quenching, stretching, and artificial aging of the first and second aluminum alloy layers. The aluminum alloy composite plates prepared by this method have the characteristics of aesthetics, high mechanical strength, and high peel strength.
[0026] According to a preferred embodiment of the present invention, in step S2, semicircle A is chamfered or raised; semicircle B is also chamfered or raised. This ensures that semicircles A and B do not misalign during assembly and reduces interface deformation caused by differences in the flowability of the two materials.
[0027] According to a preferred embodiment of the present invention, the guide groove of the extrusion die has an inverted conical shape; the depth of the guide groove is ≥30mm. This further improves the ability of semicircles A and B to fully weld within the die during extrusion, thereby increasing peel strength.
[0028] According to a preferred embodiment of the present invention, in step S3, the extrusion conditions include at least one of the following:
[0029] i. The extrusion temperature is 500~540℃;
[0030] ii. The extrusion speed is 1.0~6.0mm / s;
[0031] iii. The extrusion coefficient λ is 10 to 80.
[0032] According to a preferred embodiment of the present invention, the conditions for online quenching include at least one of the following:
[0033] i. The temperature before quenching is 520~540℃;
[0034] ii. Quenching cooling rate ≥ 30℃ / s;
[0035] iii. The temperature after quenching is ≤80℃.
[0036] According to a preferred embodiment of the present invention, the stretching amount is 0.5% to 1.5%. Thus, stretching achieves material straightening while simultaneously removing residual stress in the material.
[0037] According to a preferred embodiment of the present invention, the steps of the artificial aging process are as follows:
[0038] Hold at 120℃ for 16–20 hours; then raise the temperature to 190℃ and hold for 1–3 hours.
[0039] This ensures that the second aluminum alloy layer side maintains near-peak performance while the first aluminum alloy layer rapidly undergoes aging, and the second aluminum alloy layer side does not experience a significant performance reduction due to high-temperature aging.
[0040] According to a preferred embodiment of the present invention, in step S2, the heating temperature is 500-540°C.
[0041] According to a preferred embodiment of the present invention, in step S2, the heating time is 2 to 6 hours.
[0042] A third aspect of this invention provides the application of the aforementioned aluminum alloy composite sheet in the preparation of 3C products.
[0043] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Attached Figure Description
[0044] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0045] Figure 1 This is a schematic diagram of the preparation process in Embodiment 1 of the present invention;
[0046] Figure 2 This is a processing shape diagram of semicircles A and B in Embodiment 1 of the present invention;
[0047] Figure 3 These are top and cross-sectional views of the extrusion die according to Embodiment 1 of the present invention;
[0048] Figure 4 This is a diagram of the interface between the aluminum alloy composite plates of Embodiment 1 and Comparative Example 1 of the present invention.
[0049] Figure 5 This is a cross-sectional metallographic image of the aluminum alloy composite plate of Embodiment 1 of the present invention.
[0050] Figure 6 This is a diagram of the bonding interface of the aluminum alloy composite plate of Embodiment 1 of the present invention.
[0051] Figure 7 This is a bending photograph of the aluminum alloy composite plate of Embodiment 1 of the present invention.
[0052] Figure 8 These are peel force test diagrams of the aluminum alloy composite plates of Embodiments 1-3 of the present invention.
[0053] Figure 9 This is a diagram of the bonding interface of the aluminum alloy composite plate of Comparative Example 5 of the present invention.
[0054] Figure 10 These are oxidation images of the aluminum alloy composite plates of Comparative Example 6 and Example 1 of the present invention.
[0055] Figure 11 A diagram of the bonding interface of the aluminum alloy composite plate of Comparative Example 6 of this invention. Detailed Implementation
[0056] The following are specific embodiments of the present invention, and the technical solutions of the present invention will be further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0057] Unless otherwise specified, the reagents, methods and equipment used in this invention are all conventional reagents, methods and equipment in this technical field.
[0058] Example 1
[0059] This example provides an aluminum alloy composite sheet, the dosage of each component of which is shown in Table 1, and its flow diagram is shown below. Figure 1 As shown, its preparation method is as follows:
[0060] S1. Prepare ingot A from each component of the first aluminum alloy layer; prepare ingot B from each component of the second aluminum alloy layer; the preparation steps are as follows (the preparation steps for ingot A and ingot B are the same):
[0061] (1) Raw material preparation: Calculate the weight of raw materials required for the composition ratio in Table 1 by calculating the chemical composition and blending.
[0062] (2) Loading the furnace: Load the aluminum ingots from the above raw materials into the smelting furnace (regenerative energy-saving furnace);
[0063] (3) Heating and melting: Control the temperature inside the furnace at 750-780℃ so that the aluminum ingot is completely melted into aluminum melt I;
[0064] (4) Alloying: Add other intermediate alloys to aluminum melt I and stir to melt it, thus performing preliminary alloying of the melt to obtain aluminum melt II;
[0065] (5) Refining: Add refining agent to the aluminum melt II obtained in step (4) at a dosage of 1 kg / ton of aluminum melt II. The refining temperature is 730-750℃ and the refining time is 40 minutes. During the refining process, the aluminum melt obtained will be chemically analyzed. If the alloy composition is not within the range described in step (1), the alloy composition will be controlled within the range described in step (1) by fine-tuning the composition. At the same time as refining, high-purity argon gas is introduced into the aluminum melt through the permeable brick at the bottom of the furnace for stirring and exhaust. Then, the slag is removed to obtain aluminum melt III. The argon gas pressure is controlled at 0.05-0.1 MPa and the flow rate is controlled at 10 L / min.
[0066] (6) Alloy composition analysis: Alloy element analysis is performed on the melt III obtained after refining in step (5). If the alloy composition is not within the range described in step (1), the alloy composition is controlled within the range described in step (1) by fine-tuning the composition.
[0067] (7) Standing treatment: Aluminum melt III was left to stand for 40 minutes to obtain aluminum melt IV;
[0068] (8) Online degassing: Hydrogen is removed by using a degassing device to control the hydrogen content of aluminum melt IV to below 0.12 ml / 100 g Al aluminum;
[0069] (9) Online filtration: A dual-stage filtration system is used for purification. The first aluminum alloy layer uses an RD-grade foam ceramic tubular filter, and the second aluminum alloy layer uses an 80-mesh + 80-mesh foam ceramic plate filter.
[0070] (10) Casting: A semi-continuous water-cooled casting method is adopted, and the casting temperature is controlled at 680-710℃ to obtain aluminum alloy round ingots.
[0071] (11) Homogenization treatment: The obtained alloy round ingot is fully homogenized in a homogenization heat treatment furnace to eliminate dendrite segregation.
[0072] S2. Cut ingot A into a semicircle A with a length of 350mm; convex shape is added to semicircle A; cut ingot B into a semicircle B with a length of 350mm; chamfer semicircle B (e.g., ...). Figure 2 As shown, the green part is semicircle B and the yellow part is semicircle A; semicircle A and semicircle B are combined and placed in an aluminum rod heating furnace for heating (temperature 530℃; 5 hours) to obtain an aluminum rod;
[0073] S3. Place the aluminum rod in the extrusion die (top view and cross-sectional view of the extrusion die are shown in the figure). Figure 3 As shown, the guide channel is an inverted cone shape; the depth of the guide channel is 50mm. The sample is extruded (extrusion machine temperature is 520℃; extrusion speed (main cylinder forward speed) is 2.0mm / s, the sample is a 30*5mm sheet, and the extrusion ratio (extrusion coefficient λ) is 45). Then, it undergoes online quenching (within 15s of extrusion from the die, it enters the water-cooled quenching zone; the temperature before entering the quenching zone is 520~540℃, the water temperature is 40℃, the quenching cooling rate is ≥30℃ / s, and the temperature after quenching is ≤80℃), stretching (stretching amount is 1.0-1.4%), and artificial aging treatment (holding at 120℃ for 18 hours; then rapidly heating to 190℃ and holding for 2 hours) to obtain the final product.
[0074] Examples 2-3
[0075] This example provides an aluminum alloy composite sheet, the contents of which are shown in Table 1, and the preparation method is the same as in Example 1.
[0076] Example 4
[0077] This example provides an aluminum alloy composite sheet with a flow guide depth of 30mm in the mold design. The component content and preparation method are the same as in Example 1.
[0078] Comparative Example 1
[0079] This example provides an aluminum alloy composite sheet, with the same component content and preparation method as in Example 1. The difference is that in step S2, semicircle A has no protrusion and semicircle B has no chamfer design.
[0080] Comparative Example 2
[0081] This example provides an aluminum alloy composite sheet, with the same component content and preparation method as in Example 1, except that the extrusion die does not have an inverted conical guide design.
[0082] Comparative Example 3
[0083] This example provides an aluminum alloy composite sheet, with the same component content and preparation method as in Example 1. The difference is that the artificial aging treatment is a single-stage 150°C heat treatment for 24 hours.
[0084] Comparative Example 4
[0085] This example provides an aluminum alloy composite sheet, with the same component content and preparation method as in Example 1, except that the first aluminum alloy layer does not contain Zn.
[0086] Comparative Example 5
[0087] This example provides an aluminum alloy composite sheet, the composition of which is shown in Table 1. The preparation method is the same as in Example 1, except that the heating temperature is 485℃.
[0088] Comparative Example 6
[0089] This example provides an aluminum alloy composite sheet, the composition of which is shown in Table 1. The preparation method is the same as in Example 1, except that the heating temperature is 485℃ and the artificial aging process is carried out at 120℃ for 36 hours.
[0090] Table 1
[0091]
[0092] Performance testing
[0093] The aluminum rods prepared in Example 1 and Comparative Example 1 were subjected to interface testing, and the results are as follows: Figure 4 As shown, from Figure 4 It can be observed that the interface of Comparative Example 1 is deformed, affecting its use, while the interface of Example 1 is a straight line without deformation.
[0094] The aluminum alloy composite plates of Examples 1-3 and Comparative Examples 2-6 of the present invention were tested as follows, and the results are shown in Table 2:
[0095] Tensile strength and yield strength: Tensile test shall be conducted in accordance with GB / T 228.1-2021; specimen specifications shall be in accordance with GB / T16865-2023.
[0096] Vickers hardness: Refer to the test method in GB / T 4340.1-2024.
[0097] Peel strength: Refer to the test method of GB / T 7122-1996, and the requirement is >200N / 10mm.
[0098] Table 2
[0099]
[0100] The cross-section of the aluminum alloy composite plate prepared in Example 1 of this invention was etched with sodium hydroxide solution and subjected to metallographic analysis. The results are as follows: Figure 5 As shown, the two materials undergo extrusion recrystallization at a relatively flat interface in the middle, without any overheating issues, indicating that the extrusion process is set relatively reasonably.
[0101] The interface of the aluminum alloy composite plate prepared in Example 1 of this invention was mechanically polished and photographed. The results are as follows: Figure 6 As shown, metallurgical bonding occurs at the interface where the two materials meet, and the interface is free of pores and large particle inclusions.
[0102] The aluminum alloy composite sheet prepared in Example 1 of this invention was bent 150°, and the result is as follows: Figure 7 As shown, due to the different degrees of deformation of the metal on both sides of the central bonding interface, the location of the bonding interface is revealed after bending, but no bending cracking problem occurs.
[0103] The aluminum alloy composite plates prepared in Examples 1-3 of this invention were subjected to peel force tests, and the results are as follows: Figure 8 As shown, the values of the stable force segment of the test curve for a 10mm wide sample are all greater than 300N.
[0104] Compared with Example 1, Comparative Example 2 shows that the lack of an inverted conical flow guide design in the mold design greatly affects the bonding between the two materials, resulting in a reduction of peeling force by about 70%.
[0105] Compared with Example 1, Comparative Example 3 adopted a single-stage medium-temperature long-term aging scheme. The aging results showed that the first aluminum alloy layer was under-aged (tensile strength was close to the peak value, and yield strength only reached 90% of the peak value), while the second aluminum alloy layer was over-aged, with a performance loss of about 18%.
[0106] Compared with Example 1, Comparative Example 4 showed that without the addition of Zn, the peel strength of the composite board decreased by about 20%.
[0107] Comparing Comparative Example 5 with Example 1, the results are as follows: Figure 9 The material's high-temperature fluidity varies greatly, causing severe deformation of the bonding interface at the edges of the extruded product.
[0108] Compared to Example 1, Comparative Example 6 increased the alloy composition on the second aluminum alloy layer side, while the heat treatment process was biased towards the second aluminum alloy layer side. Ultimately, this resulted in insufficient solid solution and aging effect on the first aluminum alloy layer side, excessive performance degradation, and a poorer anodized appearance (e.g., ...). Figure 10 , Figure 10 The upper middle section shows the oxidized appearance of Example 1, and the lower section shows the oxidized appearance of Comparative Example 6; Furthermore, due to flowability issues, the bonding interface of the extruded product deforms, such as... Figure 11 The second aluminum alloy layer at the edge is deposited onto the first aluminum alloy layer.
[0109] The present invention has been described in detail above with reference to the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. An aluminum alloy composite sheet, characterized in that, The aluminum alloy composite plate includes a first aluminum alloy layer and a second aluminum alloy layer connected in sequence. By mass percentage, the composition of the first aluminum alloy layer includes Si: 0.4%~1.2%, Fe≤0.1%, Cu: 0.4%~1.1%, Mn≤0.1%, Mg: 0.7%~1.2%, Cr≤0.1%, Zn: 0.1~0.25%, other impurities <0.1%, and the balance being Al; By mass percentage, the composition of the second aluminum alloy layer includes Si≤0.2%, Fe≤0.4%, Cu:1.0%~2.5%, Mn≤0.3%, Mg:1.4%~2.6%, Cr≤0.1%, Zn:4%~6%, other impurities <0.1%, and the balance being Al; The aluminum alloy composite plate is prepared by the following method: S1. Prepare ingot A from each component of the first aluminum alloy layer; prepare ingot B from each component of the second aluminum alloy layer; S2. Cut the ingot A into a semicircle A; cut the ingot B into a semicircle B; combine the semicircles A and B and heat them to obtain an aluminum rod; S3. The aluminum rod is placed in an extrusion die for extrusion; Then, perform online quenching, stretching, and artificial aging treatments in sequence to obtain the final product; In step S2, the semicircle A is chamfered or raised; The semicircle B is chamfered or raised; the heating temperature is 500~540℃; The guide channel of the extrusion die has an inverted conical shape; the depth of the guide channel is ≥30mm; The steps for the manual aging process are as follows: Keep warm at 120℃ for 16-20 hours; then raise the temperature to 190℃ and keep warm for 1-3 hours.
2. The aluminum alloy composite sheet according to claim 1, characterized in that, In the first aluminum alloy layer, the mass ratio of Mg to Si is (0.6~1.55):
1.
3. The aluminum alloy composite sheet according to claim 1, characterized in that, In the second aluminum alloy layer, the Cu content is 1.2% to 1.5%.
4. The aluminum alloy composite sheet according to claim 1, characterized in that, In step S3, the extrusion conditions include at least one of the following: i. Extrusion temperature is 500~540℃; ii. The extrusion speed is 1.0~6.0 mm / s; iii. The extrusion coefficient λ is 10 to 80.
5. The aluminum alloy composite plate according to claim 4, characterized in that, The conditions for online quenching include at least one of the following: i. The temperature before quenching is 520~540℃; ii. Quenching cooling rate ≥ 30℃ / s; iii. The temperature after quenching is ≤80℃.
6. The application of the aluminum alloy composite sheet according to any one of claims 1 to 5 in the preparation of 3C products.
Citation Information
Patent Citations
Preparation method of 6xxx / 7xxx aluminum alloy composite
CN108396209A