A polycarbonate material, its preparation method and use

By introducing nitrogen and oxygen free radicals into polycarbonate materials through compound flame retardants, the problems of insufficient low-temperature impact strength and flame retardant performance are solved, and high-toughness thin-walled halogen-free flame-retardant polycarbonate materials are prepared, which are suitable for the field of electronics and electrical appliances.

CN119798946BActive Publication Date: 2026-11-24CHONGQING ORINKO TECH CO LTD CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411972574.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-30
Publication Date
2026-11-24
Estimated Expiration
2044-12-30

AI Technical Summary

Technical Problem

Polycarbonate materials have poor impact resistance at low temperatures, and traditional flame retardants release toxic gases and fumes during combustion, limiting their application scenarios.

Method used

A compound flame retardant is used, which includes an organosilicon flame retardant with nitrogen and oxygen free radicals in its structure and a nitrogen and oxygen free radical compound containing active groups. Stable nitrogen and oxygen free radicals are formed through group reaction, and active free radicals are captured to improve flame retardant performance. It is then compounded with sulfonate flame retardant to prepare a high-toughness thin-walled halogen-free flame retardant polycarbonate material.

Benefits of technology

It maintains good impact resistance in low-temperature environments down to -40°C, achieves ultra-thin flame retardancy of 0.5-0.8mm, and has excellent weather resistance and flame retardant properties, making it suitable for mid-to-high-end electronic and electrical appliance fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005219778430000061
    Figure BDA0005219778430000061
  • Figure BDA0005219778430000161
    Figure BDA0005219778430000161
  • Figure BDA0005219778430000162
    Figure BDA0005219778430000162
Patent Text Reader

Abstract

This invention discloses a polycarbonate material, its preparation method, and its applications, belonging to the field of polymer materials technology. The material, by weight, comprises 40-80 parts polycarbonate, 20-60 parts silicon-copolymerized polycarbonate, 0.1-0.5 parts sulfonate flame retardant, 0.1-0.5 parts compounded flame retardant, 0.3-0.8 parts anti-dripping agent, 0.1-0.4 parts antioxidant, and 0.2-0.8 parts lubricant. The compounded flame retardant is an organosilicon flame retardant with nitrogen and oxygen free radicals in its structure. This material maintains good impact resistance even at temperatures as low as -40°C. The compounded flame retardant not only has highly efficient flame retardant properties but also excellent weather resistance. With the combined action of the sulfonate and compounded flame retardants, it can meet the flame retardant requirements for ultra-thin parts of 0.5-0.8 mm, making it particularly suitable for mid-to-high-end laptops, e-book casings, and other electronic and electrical applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials technology, specifically relating to a polycarbonate material, its preparation method, and its application. Background Technology

[0002] Polycarbonate boasts excellent overall performance and good transparency, making it one of the most widely used and rapidly developing engineering plastics. It also exhibits good dimensional stability, mechanical properties, thermoelectric properties, and creep resistance, thus finding widespread application in various sectors of national production and daily life, including machinery, electronics, electrical appliances, and textiles. With product upgrades and iterations, lightweighting of plastic products has become a crucial development direction, leading to increasingly thinner plastic products and more stringent requirements for flame retardant properties. Furthermore, conventional polycarbonate exhibits poor impact strength at temperatures as low as -40°C, which limits its application scenarios.

[0003] Thin-walled flame-retardant polycarbonate materials are often compounded with silicone flame retardants for flame retardancy. For example, when a cage-type polysilsesquioxane flame retardant is added, the silicone flame retardant is oxidized and decomposed during the combustion and decomposition of the polymer material to form a silicate layer that isolates the air, thus playing a flame-retardant role. Using silicone flame retardants alone cannot achieve thin-walled flame retardancy. Patent application CN106349676A discloses a halogen-free flame-retardant PC and its preparation method. The specific raw material formula is as follows: 65-80% polycarbonate, 10-25% polycarbonate powder, 2.5-6.5% flame retardant, 0.2-0.5% anti-dripping agent, 2-5% modified filler, 0.5-1% carbon black, 0.5-1% antioxidant, and 0.2-1% lubricant. This invention uses a flame-retardant system compounded with sulfonate and silicone, which can achieve a UL94V-0 rating of 0.25mm. However, this invention exhibits brittleness under impact at low temperatures.

[0004] The chain reaction that occurs during the combustion of polymer materials releases a large number of reactive free radicals (such as OH·, O·, H·). The hydrogen halides produced by halogen flame retardants can capture these reactive free radicals, and the generated halogen free radicals can continue to participate in the reaction, thus cyclically blocking the combustion reaction. However, halogen flame retardants release large amounts of smoke and toxic and corrosive gases during combustion. Although halogen flame retardants have the advantages of high flame retardant efficiency and wide adaptability, their disadvantages in safety and environmental protection limit their application in polycarbonate materials. Summary of the Invention

[0005] The purpose of this invention is to provide a polycarbonate material, its preparation method, and its application, in order to solve the problem of poor flame retardant properties of polycarbonate materials.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] To achieve the above objectives, the first aspect of the present invention provides a polycarbonate material, wherein, by weight, the raw materials include 40-80 parts of polycarbonate, 20-60 parts of silicon copolymer polycarbonate, 0.1-0.5 parts of sulfonate flame retardant, 0.1-0.5 parts of compound flame retardant, 0.3-0.8 parts of anti-dripping agent, 0.1-0.4 parts of antioxidant, and 0.2-0.8 parts of lubricant. The compound flame retardant is an organosilicon flame retardant with nitroxide free radicals in its structure. The compound flame retardant is obtained by reacting an organosilicon flame retardant containing active groups with a nitroxide free radical compound containing active groups.

[0008] Nitrogen oxide radicals, which exist stably at room temperature, can also rapidly capture reactive free radicals such as C·, O2·, O·, OH·, and H·, exhibiting a quenching effect on reactive free radicals and thus demonstrating flame retardant potential. Since nitrile oxide radicals are stable at room temperature and effectively capture reactive free radicals generated by polymer degradation due to light, heat, and oxidative degradation, polycarbonate materials with added flame retardants exhibit excellent weather resistance.

[0009] Furthermore, the mass ratio of polycarbonate to silicon-co-polycarbonate is less than 1.5.

[0010] Furthermore, the polycarbonate is bisphenol A type polycarbonate, and the melt mass flow rate is 3-20 g / 10 min;

[0011] And / or, the melt mass flow rate of the silicon copolymer polycarbonate is 3 to 10 g / 10 min;

[0012] Furthermore, the sulfonate flame retardant includes at least one of potassium benzenesulfonylbenzenesulfonate, potassium perfluorobutylsulfonate, and sodium 2,4,5-trichlorobenzenesulfonate.

[0013] Furthermore, the organosilicon flame retardant is a cage-type polysilsesquioxane (POSS), and the general formula of the cage-type polysilsesquioxane (POSS) is (RS iO3 / 2)n, where n is an even number ≥6, and R is an organic group connected to the Si atom.

[0014] Furthermore, the organic groups on the structure of the organosilicon flame retardant are active groups, and the number of active groups is at least one.

[0015] Furthermore, the active groups on the structure of the organosilicon flame retardant are selected from one of epoxy, carboxyl, hydroxyl, amino, isocyanate, vinyl, allyl, and thiocyanate groups.

[0016] Furthermore, the organosilicon flame retardant is any one of the following: octaepoxy cage-type polysilsesquioxane (epoxy-POSS), octavinyl cage-type polysilsesquioxane (vinyl-POSS), octaglycidyl cage-type polysilsesquioxane (glycidyl-POSS), octacarboxyl cage-type polysilsesquioxane, acrylate cage-type polysilsesquioxane, allyl isobutyl cage-type polysilsesquioxane, trinorbornene isobutyl ester cage-type polysilsesquioxane, epoxy cyclohexyl cage-type polysilsesquioxane, trisilyl phenyl cage-type polysilsesquioxane, and octaammonium cage-type polysilsesquioxane.

[0017] The general formula for nitroxide free radical compounds is R>(NO·)x, where R is the active group and x takes the value of a positive integer.

[0018] Furthermore, the nitroxide radical compound has at least one nitroxide radical in its structure.

[0019] Furthermore, the nitroxide radical compound has at least one active group in its structure.

[0020] Furthermore, the active group on the structure of the nitroxide free radical compound is selected from one of epoxy, carboxyl, hydroxyl, amino, isocyanate, vinyl, allyl, and thiocyanate groups.

[0021] Further, the nitroxide free radical compound is 2,2,6,6-tetramethylpiperidine-1-oxy-4-amino-4-carboxylic acid, 4-(2-bromoacetamide)-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-epoxypropyloxy-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-amino-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-hydroxy-2,2,6,6-tetramethylpiperidine nitroxide free radical, 4-carboxyl-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4 One of the following: -isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-isothiocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-methacryloyloxy-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-(4-chloroformyl-benzoate)-2,2,6,6-tetramethylpiperidine-1-oxy radical, 3-carbamoyl-2,2,5,5-tetramethyltetrahydropyrrolidinyloxy radical, and 3-carboxyl-2,2,5,5-tetramethylpyrrolidine-1-oxy radical.

[0022] Furthermore, the preparation process of the compound flame retardant is as follows:

[0023] In a solvent containing an organosilicon flame retardant with active groups and a nitrile radical compound with active groups, a catalyst is added, the reaction temperature is 20–60℃, the reaction is stirred for 6–24 hours, and then the mixture is extracted and dried.

[0024] Furthermore, the anti-dripping agent is a polytetrafluoroethylene anti-dripping agent coated with acrylonitrile-styrene copolymer;

[0025] And / or, the antioxidant includes at least two of antioxidant 1076, antioxidant 1010, antioxidant 168, and antioxidant 627A;

[0026] And / or, the lubricant is at least one of pentaerythritol stearate, silicone powder, and polyester wax.

[0027] Accordingly, a second aspect of the present invention provides a method for preparing a polycarbonate material, comprising the steps of:

[0028] (1) Mixing: Mix the polycarbonate, silicon copolymer polycarbonate, sulfonate flame retardant, compound flame retardant, anti-dripping agent, antioxidant and lubricant in the specified amounts to obtain a mixture;

[0029] (2) Extrusion granulation: The mixture is added to a twin-screw extruder for granulation to obtain a high-toughness thin-walled halogen-free flame-retardant polycarbonate material.

[0030] Furthermore, the processing temperatures of each zone of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, and Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0031] Accordingly, a third aspect of the present invention provides an application of the aforementioned high-toughness thin-walled halogen-free flame-retardant polycarbonate material in the manufacture of parts.

[0032] As a technical solution of the present invention, the thickness of the high-toughness thin-walled halogen-free flame-retardant polycarbonate material part is 0.5 to 0.8 mm.

[0033] The beneficial effects of this invention are:

[0034] (1) The material prepared by the present invention still has good impact resistance at a low temperature of -40°C.

[0035] (2) Under the action of sulfonate flame retardant and compound flame retardant, the material prepared by the present invention can achieve an ultra-thin flame retardant thickness of 0.5 to 0.8 mm;

[0036] The high-toughness thin-walled halogen-free flame-retardant polycarbonate material of the present invention has high low-temperature impact performance, good weather resistance, and excellent flame-retardant properties. It can meet the flame-retardant requirements of ultra-thin parts of 0.5-0.8mm, and is especially suitable for mid-to-high-end laptops, e-book shells and other electronic and electrical products.

[0037] (3) The nitrogen and oxygen free radicals on the compound flame retardant of the present invention can play the same weather resistance principle as hindered amine light stabilizers. Without the addition of ultraviolet absorbers and light stabilizers, it not only has a highly efficient flame retardant effect, but also has excellent weather resistance.

[0038] The compound flame retardant of the present invention, while leveraging the flame retardant properties of organosilicon flame retardants, also utilizes the characteristic of nitrogen and oxygen free radicals to capture active free radicals, thus giving the compound flame retardant highly efficient flame retardant properties.

[0039] This invention prepares an organosilicon flame retardant with a nitrile oxide free radical structure, namely a compound flame retardant. While leveraging the flame-retardant properties of organosilicon, it also utilizes the ability of nitrile oxide free radicals to capture active free radicals, resulting in highly efficient flame retardancy. Without the addition of ultraviolet absorbers or light stabilizers to the polycarbonate material, the nitrile oxide free radicals on the compound flame retardant of this invention can exert the same weather-resistant principle as hindered amine light stabilizers, simultaneously improving the flame-retardant performance of ultra-thin materials and imparting excellent weather resistance to the material. This results in a polycarbonate material with excellent low-temperature impact resistance, good thin-walled flame retardant effect, and superior weather resistance. Detailed Implementation

[0040] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0041] The test methods and standards used in the following examples and comparative examples are as follows:

[0042] Tensile strength test: conducted according to ASTM D638 standard, with a tensile speed of 50 mm / min.

[0043] Izod notched impact test: Tensile properties were tested according to ASTM D256; the low-temperature notched impact test conditions were as follows: the test specimen was placed in a -40°C freezer for 4 hours and then removed to test the Izod notched impact strength.

[0044] Flame retardant performance test: The flame retardant performance test is conducted in accordance with the UL-94 standard. The test samples are standard flame retardant samples of 0.5mm and 0.8mm.

[0045] Xenon lamp aging test: The tensile specimens were aged according to GB / T16422.2-2022 for 1000 hours. The tensile strength retention rate and Izod notch impact retention rate were calculated after aging.

[0046] The specific information of the raw materials used in the following examples and comparative examples is as follows:

[0047]

[0048] Example 1

[0049] Octaglycidyl cage-type polysilsesquioxane (glycidyl-POSS) was dissolved in tetrahydrofuran at an equivalent ratio of 8:1 between the epoxy group and the hydroxyl group of 4-hydroxy-2,2,6,6-tetramethylpiperidine nitroxide radical (4-OH-TEMPO), with phosphoric acid as a catalyst. The reaction was stirred at 40°C for 6 hours and dried to obtain the POSS-grafted nitroxide radical compound, which is the compound flame retardant.

[0050] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.3 parts potassium benzenesulfonylbenzenesulfonate flame retardant, 0.1 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.1 parts antioxidant 168, 0.1 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0051] Example 2

[0052] Octaglycidyl cage-type polysilsesquioxane (glycidyl-POSS) was dissolved in tetrahydrofuran at an equivalent ratio of 8:1 between the epoxy group and the hydroxyl group of 4-hydroxy-2,2,6,6-tetramethylpiperidine nitroxide radical (4-OH-TEMPO), with phosphoric acid as a catalyst. The reaction was stirred at 40°C for 6 hours and dried to obtain the POSS-grafted nitroxide radical compound, which is the compound flame retardant.

[0053] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.3 parts potassium benzenesulfonylbenzenesulfonate flame retardant, 0.2 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.1 parts antioxidant 168, 0.1 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0054] Example 3

[0055] Octaglycidyl cage-type polysilsesquioxane (glycidyl-POSS) was dissolved in tetrahydrofuran at an equivalent ratio of 8:1 between the epoxy group and the hydroxyl group of 4-hydroxy-2,2,6,6-tetramethylpiperidine nitroxide radical (4-OH-TEMPO), with phosphoric acid as a catalyst. The reaction was stirred at 40°C for 6 hours and dried to obtain the POSS-grafted nitroxide radical compound, which is the compound flame retardant.

[0056] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.3 parts potassium benzenesulfonylbenzenesulfonate flame retardant, 0.3 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.1 parts antioxidant 168, 0.1 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0057] Example 4

[0058] Trisilyl alcohol phenyl cage-type polysilsesquioxane was dissolved in tetrahydrofuran at a 3:1 equivalent ratio of hydroxyl group to isocyanate group of 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, with dibutyltin dilaurate as catalyst. The reaction was stirred at 20°C for 24 hours and dried to obtain POSS grafted nitroxide radical compound, which is the compound flame retardant.

[0059] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.1 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0060] Example 5

[0061] Trisilyl alcohol phenyl cage-type polysilsesquioxane was dissolved in tetrahydrofuran at a 3:1 equivalent ratio of hydroxyl group to isocyanate group of 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, with dibutyltin dilaurate as catalyst. The reaction was stirred at 20°C for 24 hours and dried to obtain POSS grafted nitroxide radical compound, which is the compound flame retardant.

[0062] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.2 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0063] Example 6

[0064] Trisilyl alcohol phenyl cage-type polysilsesquioxane was dissolved in tetrahydrofuran at a 3:1 equivalent ratio of hydroxyl group to isocyanate group of 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, with dibutyltin dilaurate as catalyst. The reaction was stirred at 20°C for 24 hours and dried to obtain POSS grafted nitroxide radical compound, which is the compound flame retardant.

[0065] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.3 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0066] Example 7

[0067] Octacarboxylated cage-type polysilsesquioxane was dissolved in tetrahydrofuran at an equivalent ratio of 8:1 between the carboxyl group and the isocyanate group of 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, with dimethylethanolamine as a catalyst. The reaction was stirred at 60°C for 12 hours and then dried to obtain a POSS-grafted nitroxide radical compound, which is the compound flame retardant.

[0068] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.2 parts potassium benzenesulfonylbenzenesulfonate flame retardant, 0.1 parts perfluorobutylsulfonate flame retardant, 0.2 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0069] Comparative Example 1

[0070] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.3 parts potassium benzenesulfonylbenzenesulfonate flame retardant, 0.3 parts organosilicon flame retardant (octaglycidyl cage-type polysilsesquioxane), 0.4 parts anti-dripping agent, 0.1 parts antioxidant 168, 0.1 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0071] Comparative Example 2

[0072] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.3 parts potassium benzenesulfonylbenzenesulfonate flame retardant, 0.3 parts 4-hydroxy-2,2,6,6-tetramethylpiperidine nitroxide radical, 0.4 parts anti-dripping agent, 0.1 parts antioxidant 168, 0.1 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0073] Comparative Example 3

[0074] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.3 parts potassium benzenesulfonylbenzenesulfonate flame retardant, 0.3 parts organosilicon flame retardant (octaglycidyl cage-type polysilsesquioxane), 0.3 parts 4-hydroxy-2,2,6,6-tetramethylpiperidine nitroxide radical, 0.4 parts anti-dripping agent, 0.1 parts antioxidant 168, 0.1 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0075] Comparative Example 4

[0076] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.3 parts organosilicon flame retardant (trisilyl alcohol phenyl cage polysilsesquioxane), 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0077] Comparative Example 5

[0078] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.3 parts 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0079] Comparative Example 6

[0080] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.3 parts organosilicon flame retardant (trisilyl alcohol phenyl cage polysilsesquioxane), 0.3 parts 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0081] Comparative Example 7

[0082] Trisilyl alcohol phenyl cage-type polysilsesquioxane was dissolved in tetrahydrofuran at a 3:1 equivalent ratio of hydroxyl group to isocyanate group of 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, with dibutyltin dilaurate as catalyst. The reaction was stirred at 20°C for 24 hours and dried to obtain POSS grafted nitroxide radical compound, which is the compound flame retardant.

[0083] 63.5 parts polycarbonate, 35 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.3 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0084] Comparative Example 8

[0085] Trisilyl alcohol phenyl cage-type polysilsesquioxane was dissolved in tetrahydrofuran at a 3:1 equivalent ratio of hydroxyl group to isocyanate group of 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, with dibutyltin dilaurate as catalyst. The reaction was stirred at 20°C for 24 hours and dried to obtain POSS grafted nitroxide radical compound, which is the compound flame retardant.

[0086] 73.5 parts polycarbonate, 25 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.3 parts compound flame retardant, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0087] Comparative Example 9

[0088] Trisilyl alcohol phenyl cage-type polysilsesquioxane was dissolved in tetrahydrofuran at a 3:1 equivalent ratio of hydroxyl group to isocyanate group of 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, with dibutyltin dilaurate as catalyst. The reaction was stirred at 20°C for 24 hours and dried to obtain POSS grafted nitroxide radical compound, which is the compound flame retardant.

[0089] 58.5 parts polycarbonate, 40 parts silicon copolymer polycarbonate, 0.1 parts potassium perfluorobutyl sulfonate flame retardant, 0.3 parts UV-234 ultraviolet absorber, 0.4 parts anti-dripping agent, 0.2 parts antioxidant 168, 0.2 parts antioxidant 1076, and 0.4 parts pentaerythritol stearate. (1) Mixing: Add the above-mentioned formula components to a high-speed mixer and stir for 5 minutes to obtain a mixed material; (2) Extrusion granulation: Add the mixed material to a twin-screw extruder for granulation. The processing temperatures of each section of the twin-screw extruder are as follows: Zone 1: 225℃±5℃, Zone 2: 255℃±5℃, Zone 3: 255℃±5℃, Zone 4: 255℃±5℃, Zone 5: 265℃±5℃, Zone 6: 265℃±5℃, Zone 7: 275℃±5℃, Zone 8: 275℃±5℃, Zone 9: 265℃±5℃, Zone 10: 265℃±5℃. The die head temperature is 285℃±5℃, the screw speed is 300rpm~400rpm, and the vacuum degree is -0.5MPa~-0.9MPa.

[0090] Performance tests were conducted on Examples 1-7 and Comparative Examples 1-9, and the results are shown in Tables 1-2:

[0091] Table 1

[0092]

[0093] Table 2

[0094]

[0095]

[0096] The difference between Examples 1, 2, and 3, and Examples 4, 5, and 6 lies in the amount of compound flame retardant used. The comparison shows that increasing the amount of compound flame retardant significantly improves the flame retardant performance of the material. Compared to Examples 2 and 6, Example 7 adds potassium benzenesulfonylbenzenesulfonate, potassium perfluorobutylsulfonate, and a compound flame retardant. In Example 2, reducing the content of potassium benzenesulfonylbenzenesulfonate while increasing the content of potassium perfluorobutylsulfonate, and in Example 6, reducing the content of compound flame retardant while increasing the content of potassium benzenesulfonylbenzenesulfonate, both achieved a flame retardant effect of 0.5 mmV-0 (Example 7), indicating a good synergistic effect between the sulfonate flame retardant and the compound flame retardant.

[0097] Examples 3, 1, 2, and 3 are potassium benzenesulfonylbenzenesulfonate systems. The difference is that Example 3 is a compound flame retardant, 1 is an organosilicon flame retardant, 2 is a nitrile radical, and 3 is both an organosilicon flame retardant and a nitrile radical. Examples 6, 4, 5, and 6 are potassium perfluorobutylsulfonate systems. The difference is that Example 6 is a compound flame retardant, 4 is an organosilicon flame retardant, 5 is a nitrile radical, and 6 is both an organosilicon flame retardant and a nitrile radical. The comparison shows that adding only organosilicon flame retardants and nitrile radicals only allows for the limited expression of their respective properties and does not provide highly efficient flame retardant performance. Comparative Examples 1 and 4 show poor retention rates of tensile strength and notched impact strength under xenon lamp aging because their systems lack weather-resistant components, i.e., they lack nitrile radicals. The tensile strength retention and notched impact strength retention of Example 3 are similar to those of Comparative Examples 2 and 3, and the tensile strength retention of Example 6 is similar to that of Comparative Examples 5 and 6. This is because the nitroxide free radicals in their components exhibit the same weather-resistant properties as hindered amine light stabilizers; that is, the stable nitroxide free radicals can effectively capture the active free radicals generated by the photo-oxidative degradation of the polymer, effectively preventing the chain reaction of degradation. Moreover, the flame retardancy of Example 3 reaches 0.8 mmV-0, and the flame retardancy of Example 6 reaches 0.5 mmV-0. This is not only due to the flame retardant effect of the sulfonate flame retardant, but also the synergistic flame retardant effect of the organosilicon flame retardant (i.e., the compound flame retardant) with nitroxide free radicals in its structure. This is because at high temperatures, the organosilicon flame retardant forms a dense silicon oxide film layer similar to a ceramic structure, effectively preventing molten dripping; and the organosilicon flame retardant catalyzes the polymer to form a dense carbon layer, effectively isolating oxygen and heat. Furthermore, structurally, nitrile and oxygen radicals simultaneously and effectively quench the active free radicals released during combustion, thereby further improving flame retardant efficiency. In Comparative Examples 3 and 6, the organosilicon flame retardant and nitrile and oxygen radicals are uniformly dispersed and cannot simultaneously exert their synergistic flame retardant properties in situ, resulting in poor flame retardant performance. The difference between Example 6 and Comparative Examples 7 and 8 lies in the different ratios of polycarbonate and silicon-copolymer polycarbonate. A comparison shows that increasing the proportion of silicon-copolymer polycarbonate significantly improves low-temperature impact strength and thin-wall flame retardant performance; that is, the preferred ratio of polycarbonate to silicon-copolymer polycarbonate in this application is less than 1.5. The difference between Example 6 and Comparative Example 9 is that the compounded flame retardant is replaced with an ultraviolet absorber. A comparison shows that the compounded flame retardant has the same weather resistance level as the ultraviolet absorber, and the tensile strength retention rate and impact strength retention rate are similar. This is because the stable nitrile and oxygen radicals can effectively capture the active free radicals generated by the photo-oxidative degradation of the polymer, effectively preventing polymer degradation and improving the retention rate of the polymer's mechanical properties.

[0098] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0099] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A polycarbonate material, characterized in that, The raw materials, by weight, include 40-80 parts polycarbonate, 20-60 parts silicon-copolymer polycarbonate, 0.1-0.5 parts sulfonate flame retardant, 0.1-0.5 parts compound flame retardant, 0.3-0.8 parts anti-dripping agent, 0.1-0.4 parts antioxidant, and 0.2-0.8 parts lubricant. The compound flame retardant is an organosilicon flame retardant with nitrile radicals in its structure. The compound flame retardant is obtained by a group reaction between an organosilicon flame retardant containing active groups and a nitrile radical compound containing active groups. The mass ratio of polycarbonate to silicon-copolymer polycarbonate is less than 1.

5. The organosilicon flame retardant is a cage-type polysilsesquioxane, the general formula of which is (RSiO3 / 2)n, where n is an even number ≥6, and R is an organic group bonded to Si atoms; the organosilicon flame retardant has at least one active group on its structure.

2. The polycarbonate material according to claim 1, characterized in that, The polycarbonate is bisphenol A type polycarbonate, and the melt mass flow rate is 3~20g / 10min; And / or, the melt mass flow rate of the silicon copolymer polycarbonate is 3~10 g / 10 min.

3. The polycarbonate material according to claim 1, characterized in that, The sulfonate flame retardant is potassium benzenesulfonylbenzenesulfonate.

4. The polycarbonate material according to claim 1, characterized in that, The active groups on the structure of the organosilicon flame retardant are selected from one of epoxy, carboxyl, hydroxyl, amino, isocyanate, vinyl, allyl, and thiocyanate groups.

5. The polycarbonate material according to claim 1, characterized in that, The organosilicon flame retardant is an octaepoxy cage-type polysilsesquioxane.

6. The polycarbonate material according to claim 1, characterized in that, The organosilicon flame retardant is any one of octavinyl cage polysilsesquioxane, octaglycidyl cage polysilsesquioxane, octacarboxyl cage polysilsesquioxane, acrylate cage polysilsesquioxane, allyl isobutyl cage polysilsesquioxane, trinorbornene isobutyl ester cage polysilsesquioxane, epoxy cyclohexyl cage polysilsesquioxane, and trisilyl alcohol phenyl cage polysilsesquioxane.

7. The polycarbonate material according to claim 1, characterized in that, The active group on the structure of the nitroxide free radical compound is selected from one of epoxy, carboxyl, hydroxyl, amino, isocyanate, vinyl, allyl, and thiocyanate groups.

8. The polycarbonate material according to claim 1, characterized in that, The nitroxide free radical compounds are 2,2,6,6-tetramethylpiperidine-1-oxy-4-amino-4-carboxylic acid, 4-(2-bromoacetamide)-2,2,6,6-tetramethylpiperidine-1-oxo radical, 4-epoxypropyloxy-2,2,6,6-tetramethylpiperidine-1-oxo radical, 4-amino-2,2,6,6-tetramethylpiperidine-1-oxo radical, 4-hydroxy-2,2,6,6-tetramethylpiperidine nitroxide free radical, 4-carboxyl-2,2,6,6-tetramethylpiperidine-1-oxo radical, 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxo radical, and 4-isocyanate-2,2,6,6-tetramethylpiperidine-1-oxo radical. One of the following: cyanate ester-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-isothiocyanate-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-methacryloyloxy-2,2,6,6-tetramethylpiperidine-1-oxy radical, 4-(4-chloroformyl-benzoate)-2,2,6,6-tetramethylpiperidine-1-oxy radical, 3-carbamoyl-2,2,5,5-tetramethyltetrahydropyrrole nitroxide radical, and 3-carboxyl-2,2,5,5-tetramethylpyrrolidine-1-oxy radical.

9. A polycarbonate material according to claim 1, characterized in that, The preparation process of the compound flame retardant is as follows: In a solvent containing an organosilicon flame retardant with active groups and a nitrile radical compound with active groups, a catalyst is added, the reaction temperature is 20~60℃, the reaction is stirred for 6~24h, and then the mixture is extracted and dried.

10. A polycarbonate material according to claim 1, characterized in that, The anti-dripping agent is a polytetrafluoroethylene anti-dripping agent coated with acrylonitrile-styrene copolymer; And / or, the antioxidant includes at least two of antioxidant 1076, antioxidant 1010, antioxidant 168, and antioxidant 627A; And / or, the lubricant is at least one of pentaerythritol stearate, silicone powder, and polyester wax.

11. A method for preparing a polycarbonate material according to any one of claims 1-10, characterized in that, step include: (1) Mixing: Mix the polycarbonate, silicon copolymer polycarbonate, sulfonate flame retardant, compound flame retardant, anti-dripping agent, antioxidant and lubricant in the specified amounts to obtain a mixture; (2) Extrusion granulation: The mixture is added to a twin-screw extruder for granulation to obtain polycarbonate material.

12. The application of a polycarbonate material as described in any one of claims 1-10, characterized in that, This material is used to prepare high-toughness thin-walled halogen-free flame-retardant polycarbonate parts, wherein the thickness of the high-toughness thin-walled halogen-free flame-retardant polycarbonate parts is 0.5 to 0.8 mm.

Citation Information

Patent Citations

  • Halogen-free flame-retardant PC (polycarbonate) and preparation method thereof

    CN106349676A

  • Polycarbonate composition and preparation method thereof

    CN101519529A

  • Aryl POSS flame retardant with free radical quenching function and synthetic method and application thereof

    CN106349479A

  • Glass-fiber-reinforced flame-retardant polycarbonate composite material, and preparation method and applications thereof

    CN110157174A

  • Single-component intumescent flame retardant with free radical quenching function, preparation method and applications thereof

    CN110776635A