A nickel-molybdenum modified cobalt molybdate composite material, a preparation method thereof and neutral electrolytic water hydrogen evolution application
By growing nickel-molybdenum modified cobalt molybdate nanosheets and nanorods arrays on a conductive substrate, the problem of poor adsorption/activation capacity of neutral water electrolysis catalysts in neutral environments was solved, achieving a highly efficient and stable hydrogen evolution reaction in water electrolysis, which has important industrial application prospects.
Patent Information
- Application Number
- CN202410975845.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing neutral water electrolysis catalysts have low concentrations of water splitting reactants in neutral environments, resulting in poor catalyst adsorption/activation capacity, high overpotential, and poor stability, making it difficult to achieve large-scale application.
A nickel-molybdenum-modified cobalt molybdate composite material was prepared by growing a nanosheet-modified cobalt molybdate nanorod array on a conductive substrate using a hydrothermal method. This enhanced the material's conductivity and water adsorption capacity, improved electron transfer ability, and promoted the hydrogen evolution reaction.
It achieves efficient water electrolysis and hydrogen evolution under neutral conditions, with low overpotential, good stability, and can operate continuously under high current. It has excellent catalytic activity and stability, making it suitable for industrial applications.
Smart Images

Figure BDA0004954486720000091 
Figure HDA0004954486730000011 
Figure HDA0004954486730000012
Abstract
Description
Technical Field
[0001] This invention belongs to the field of neutral water electrolysis hydrogen production catalyst technology, and particularly relates to a nickel-molybdenum modified cobalt molybdate composite material, its preparation method, and its application in neutral water electrolysis hydrogen production. Background Technology
[0002] Hydrogen has a high energy density and its combustion products are zero-carbon and pollution-free, making it a potential new energy source for addressing the energy crisis and reducing dependence on fossil fuels. Currently, most industrial hydrogen production uses natural gas steam reforming and carbon vaporization reactions, which release large amounts of greenhouse gases such as CO2, exacerbating the greenhouse effect. Water electrolysis for hydrogen production not only produces high-purity hydrogen but also utilizes electricity generated from renewable energy sources, making it a promising and sustainable distributed hydrogen production technology. In recent years, significant progress has been made in developing high-performance non-precious metal catalysts to improve electrolyzer efficiency while controlling production costs. However, both proton exchange membrane-based acidic and anion exchange membrane-based alkaline electrolyzers require highly corrosive electrolytes, causing significant environmental pollution and severe damage to the electrolyzers. Therefore, developing water-splitting catalysts that operate efficiently under mild conditions is crucial for hydrogen production via water electrolysis. However, progress in the field of neutral water electrolysis is currently slow, mainly because the concentration of intermediate reactants in a neutral environment is low, which is not conducive to the adsorption / activation of reactants by the catalyst. Therefore, the rational design of catalyst components and the regulation of the catalyst's electronic structure to enable its efficient use in neutral water electrolysis technology will help realize the large-scale application of water electrolysis.
[0003] The water splitting process involves two half-reactions: the hydrogen evolution reaction (HER), which involves two electron transfers, and the oxygen evolution reaction (OER), which involves four electron transfers. Developing efficient catalysts for HER will greatly promote the development of the water splitting field. Although some noble metal catalysts, such as IrO2 and platinum (Pt), have been designed for neutral HER and have achieved good results, the low global reserves and high cost of noble metals undoubtedly hinder the large-scale application of water electrolysis technology. Therefore, some non-noble metal catalysts, including cobalt-based, nickel-based, and iron-based catalysts, have also been proposed and used in pH-neutral HER; however, these catalysts have high overpotentials (10 mA / cm²). 2 The overpotential at current densities exceeding 100 mV and the stability (below 50 hours) are both poor, making them far from practical applications. Among non-precious metal catalysts, cobalt-molybdenum-based catalysts are considered to be materials with HER activity comparable to precious metals. However, cobalt in cobalt-molybdenum-based catalysts is prone to precipitation during neutral water splitting reactions, resulting in extremely poor stability and rendering them unsuitable for practical applications. Summary of the Invention
[0004] The purpose of this invention is to provide a nickel-molybdenum modified cobalt molybdate composite material, its preparation method, and its application in neutral water electrolysis for hydrogen evolution. This composite material exhibits stable structure, abundant active sites, good conductivity, and strong water adsorption capacity. When used in the neutral water electrolysis for hydrogen evolution reaction, it exhibits low overpotential and strong stability even under high current conditions, demonstrating excellent catalytic activity and stability. Its preparation is simple and efficient, and it has significant application prospects.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] A nickel-molybdenum modified cobalt molybdate composite material is provided, comprising a conductive substrate and nickel-molybdenum modified cobalt molybdate grown on the conductive substrate, wherein the nickel-molybdenum modified cobalt molybdate has a nanosheet modified cobalt molybdate nanorod array morphology, wherein the nanosheet thickness is 5-80 nm and the nanorod diameter is 0.1-1 μm.
[0007] According to the above scheme, the conductive substrate is any one of the following: nickel foam, nickel mesh, nickel felt, stainless steel felt, nickel-iron foam, copper foil, copper foam, iron foam, titanium mesh, carbon cloth, carbon paper, graphite felt, carbon fiber, and carbon materials obtained by calcining various fruit shells and mollusk shells.
[0008] According to the above scheme, the nickel-molybdenum modified cobalt molybdate composite material is prepared by hydrothermal reaction of a conductive substrate with urea, ammonium fluoride, cobalt salt, molybdenum salt, nickel salt and water.
[0009] A method for preparing the above-mentioned nickel-molybdenum modified cobalt molybdate composite material is provided, comprising the following steps:
[0010] A conductive substrate is placed in a mixed solution of urea, ammonium fluoride, cobalt salt, molybdenum salt, nickel salt and water, and a hydrothermal reaction is carried out to grow a nanosheet-modified CoMoO4 nanorod array on the conductive substrate, thus obtaining a nickel-molybdenum-modified cobalt molybdate composite material.
[0011] Following the above procedure, after the reaction is complete, cool to room temperature, remove, wash, and dry.
[0012] According to the above scheme, the cobalt salt is any one of Co(NO3)2, CoSO4, CoCO3, Co3(PO4)2 and CoCl2.
[0013] According to the above scheme, the molybdenum salt is any one of Na2MoO4, K2MoO4 and (NH4)2MoO4.
[0014] According to the above scheme, the nickel salt is any one of Ni(NO3)2, NiSO4 and NiCl2.
[0015] According to the above scheme, the molar ratio of cobalt in the cobalt salt to molybdenum in the molybdenum salt is 1:0.3-1.2, preferably 1:0.4-0.7.
[0016] According to the above scheme, the molar ratio of cobalt in the cobalt salt to nickel in the nickel salt is 1:0.25-1, preferably 1:0.3-0.6.
[0017] According to the above scheme, the concentration of cobalt in the cobalt salt in the mixed solution is 0.005–0.200 mol / L, preferably 0.09–0.16 mol / L. A suitable concentration of Co and the ratio of metal elements are beneficial to the performance of the neutral water electrolysis hydrogen evolution reaction.
[0018] According to the above scheme, the molar ratio of cobalt in urea, ammonium fluoride and cobalt salt is 1:0.4-0.8:0.6-1.5.
[0019] According to the above scheme, in the mixed solution, the concentration of molybdenum in the molybdenum salt is 0.005–0.200 mol / L; the concentration of nickel in the nickel salt is 0.001–0.050 mol / L; the concentration of urea is 0.01–0.20 mol / L; and the concentration of ammonium fluoride is 0.01–0.20 mol / L.
[0020] According to the above scheme, the temperature of the hydrothermal reaction is 100-200℃.
[0021] According to the above scheme, the hydrothermal reaction time is 2-20 hours.
[0022] This invention provides an application of the above-mentioned nickel-molybdenum modified cobalt molybdate composite material in the hydrogen evolution reaction of water electrolysis under neutral conditions.
[0023] According to the above scheme, the nickel-molybdenum modified cobalt molybdate composite material is used as a hydrogen evolution electrode to carry out the water hydrogen evolution reduction reaction in a neutral three-electrode system.
[0024] Preferably, in the neutral three-electrode system, the carbon rod serves as the counter electrode and the calomel electrode serves as the reference electrode.
[0025] Preferably, in the neutral three-electrode system, the neutral electrolyte is a phosphate, sulfate, or chloride, and the concentration of the neutral electrolyte is 1-6 mol / L;
[0026] Compared with the prior art, the advantages of the present invention are:
[0027] 1. This invention provides a nickel-molybdenum modified cobalt molybdate composite material, comprising a conductive substrate and nickel-molybdenum modified cobalt molybdate grown on the conductive substrate. The nickel-molybdenum modified cobalt molybdate is a nanosheet-modified cobalt molybdate nanorod array morphology. On the one hand, it enhances the conductivity and water adsorption capacity of CoMoO4, improves electron transfer capacity, thereby promoting the reaction kinetics of hydrogen evolution reaction and enhancing the efficiency of electrocatalytic water reduction reaction, achieving efficient water electrolysis and hydrogen evolution under neutral conditions. On the other hand, it improves the stability of the composite material itself, reduces the precipitation of metal elements during the reaction process, and still has strong stability under high current conditions in the neutral reaction system. Specifically, when applied to the water electrolysis and hydrogen evolution reaction under neutral conditions, it exhibits high stability at 10 and 500 mA / cm². -2 At current densities, the required HER overpotential in neutral aqueous solutions is as low as 46 and 454 mV, respectively, and the system can operate for 1000 and 300 hours, respectively. Its neutral water reduction performance does not show significant degradation, indicating important application prospects.
[0028] 2. This invention provides a method for preparing a nickel-molybdenum modified cobalt molybdate composite material. Through a one-step hydrothermal method, nickel is introduced during the growth of a CoMoO4 nanorod array to finally obtain a nanosheet-modified CoMoO4 nanorod array. The preparation method is simple and efficient, with mild conditions and no need for calcination. The resulting composite material has a stable structure and exhibits excellent catalytic activity and stability as a neutral water reduction electrode, which is beneficial for industrial applications. Attached Figure Description
[0029] Figure 1 These are scanning electron microscope (SEM) images at different magnifications of the nanosheet / CoMoO4 nanorod structure (denoted as NiMo / CoMoO4) array grown on a nickel foam substrate after hydrothermal reaction in Example 1.
[0030] Figure 2 The images are scanning electron microscope (SEM) images at different magnifications of the cobalt molybdate (CoMoO4) nanorod array grown on a nickel foam substrate after hydrothermal reaction in Comparative Example 1.
[0031] Figure 3 The image shows the elemental distribution of Ni, Co, Mo, and O in NiMo / CoMoO4 obtained in Example 1, obtained by scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS).
[0032] Figure 4(a) X-ray diffraction (XRD) patterns of CoMoO4 and NiMo / CoMoO4; (b) Raman spectrum comparison of CoMoO4 and NiMo / CoMoO4; (c) Fe 2p energy level diagrams of X-ray photoelectron spectroscopy (XPS) of CoMoO4 and NiMo / CoMoO4; (d) Ni 3d energy level diagrams of NiMo / CoMoO4 via XPS.
[0033] Figure 5 The following are comparisons of the HER performance of NiMo / CoMoO4 with other samples in neutral electrolyte (1 mol / L phosphate buffer (PBS)): (a) linear sweep voltammetry (LSV) curve; (b) comparison of overpotential at different current densities; (c) Tafel slope plot; (d) electrochemical impedance spectroscopy (EIS).
[0034] Figure 6 (a) shows the voltage stability curve of NiMo / CoMoO4 at low current density in neutral electrolyte (1 mol / L PBS); (b) shows the voltage stability curve of NiMo / CoMoO4 at high current density in neutral electrolyte (1 mol / L PBS). Detailed Implementation
[0035] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0036] This invention provides a nickel-molybdenum modified cobalt molybdate composite material, comprising a conductive substrate and nickel-molybdenum modified cobalt molybdate grown on the conductive substrate. The nickel-molybdenum modified cobalt molybdate has a nanosheet modified cobalt molybdate nanorod array morphology, wherein the nanosheet thickness is 5-80 nm and the nanorod diameter is 0.1-1 μm.
[0037] In some specific embodiments, the conductive substrate is any one of the following: nickel foam, nickel mesh, nickel felt, stainless steel felt, nickel-iron foam, copper foil, copper foam, iron foam, titanium mesh, carbon cloth, carbon paper, graphite felt, carbon fiber, and carbon materials obtained by calcining various fruit shells and mollusk shells.
[0038] This invention also provides a method for preparing the above-mentioned nickel-molybdenum modified cobalt molybdate composite material, comprising the following steps:
[0039] A conductive substrate is placed in a mixed solution of urea, ammonium fluoride, cobalt salt, molybdenum salt, nickel salt and water, and a hydrothermal reaction is carried out to grow a nanosheet-modified CoMoO4 nanorod array on the conductive substrate, thus obtaining a nickel-molybdenum-modified cobalt molybdate composite material.
[0040] In some specific embodiments, the cobalt salt is any one of Co(NO3)2, CoSO4, CoCO3, Co3(PO4)2, and CoCl2; the molybdenum salt is any one of Na2MoO4, K2MoO4, and (NH4)2MoO4; and the nickel salt is any one of Ni(NO3)2, NiSO4, and NiCl2.
[0041] In some specific embodiments, the molar ratio of cobalt in the cobalt salt to molybdenum in the molybdenum salt is 1:0.3-1.2, preferably 1:0.4-0.7.
[0042] In some specific embodiments, the molar ratio of cobalt in the cobalt salt to nickel in the nickel salt is 1:0.25-1, preferably 1:0.3-0.6.
[0043] In some specific embodiments, the molar ratio of cobalt in urea, ammonium fluoride and cobalt salt is 1:0.4-0.8:0.6-1.5.
[0044] In some specific embodiments, the concentration of cobalt in the cobalt salt in the mixed solution is 0.005–0.200 mol / L, preferably 0.09–0.16 mol / L.
[0045] In some specific embodiments, in the mixed solution, the concentration of molybdenum in the molybdenum salt is 0.005–0.200 mol / L; the concentration of nickel in the nickel salt is 0.001–0.050 mol / L; the concentration of urea is 0.01–0.20 mol / L; and the concentration of ammonium fluoride is 0.01–0.20 mol / L.
[0046] In some specific embodiments, the hydrothermal reaction is carried out at a temperature of 100-200°C for a duration of 2-20 hours.
[0047] This invention also provides an application of the above-mentioned nickel-molybdenum modified cobalt molybdate composite material in the hydrogen evolution reaction of water electrolysis under neutral conditions.
[0048] In some specific embodiments, the nickel-molybdenum modified cobalt molybdate composite material is used as a hydrogen evolution electrode to carry out the water hydrogen evolution reduction reaction in a neutral three-electrode system.
[0049] Preferably, in the neutral three-electrode system, the carbon rod serves as the counter electrode and the calomel electrode serves as the reference electrode.
[0050] Preferably, in the neutral three-electrode system, the neutral electrolyte is a phosphate, sulfate, or chloride, and the concentration of the neutral electrolyte is 1-6 mol / L; more preferably, the solution pH is 7.
[0051] The following are specific implementation examples.
[0052] Example 1
[0053] A method for preparing a nickel-molybdenum modified cobalt molybdate composite material is provided, comprising the following steps:
[0054] A 1cm x 2cm nickel foam was sequentially placed in a 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water and sonicated for 15 minutes. The cleaned nickel foam was then placed in a 60mL mixed solution containing 0.15mol / L CoCl2, 0.05mol / L Ni(NO3)2, 0.06mol / L (NH4)2MoO4, 0.13mol / L urea, and 0.08mol / L ammonium fluoride. The reaction was carried out hydrothermally at 120℃ for 4 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly rinsed with anhydrous ethanol and deionized water, and then dried in an oven at 60℃ for 4 hours to obtain a nanosheet-modified CoMoO4 nanorod array catalyst (denoted as "NiMo / CoMoO4") grown on nickel foam.
[0055] Comparative Example 1
[0056] A method for preparing a CoMoO4 nanorod array is provided, comprising the following steps:
[0057] A 1cm x 2cm nickel foam was sequentially placed in a 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water and sonicated for 15 minutes. The cleaned nickel foam was then placed in a 10mL mixed solution containing 0.05mol / L CoCl2 and 0.05mol / L (NH4)2MoO4. The reaction was carried out hydrothermally at 160℃ for 6 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly rinsed with anhydrous ethanol and deionized water, and then dried in an oven set at 60℃ for 4 hours to obtain a CoMoO4 nanorod array catalyst (denoted as "CoMoO4") grown on the nickel foam.
[0058] Comparative Example 2
[0059] A method for preparing NiMoO4 nanorod arrays is provided, comprising the following steps:
[0060] A 2cm x 4cm nickel foam was sequentially placed in a 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water and sonicated for 15 minutes. The cleaned nickel foam was then placed in a 75mL mixed solution containing 0.1mol / L Ni(NO3)2 and 0.04mol / L (NH4)2MoO4. The reaction was carried out hydrothermally at 180℃ for 6 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly rinsed with anhydrous ethanol and deionized water, and then dried in an oven set at 60℃ for 4 hours to obtain a NiMoO4 nanosheet array catalyst (denoted as "NiMoO4") grown on the nickel foam.
[0061] Figure 1 and Figure 2 The images show SEM images of the NiMo / CoMoO4 catalyst obtained in Example 1 and the CoMoO4 catalyst obtained in Comparative Example 1, respectively. Specifically, the morphology of the prepared catalysts was observed on a JEOL JSM-7900 electron beam at an intensity of 12.6 keV. It can be seen that NiMo / CoMoO4 has the morphology of a nanosheet-modified nanorod array, where the nanosheet thickness is 5-80 nm and the nanorod size is 0.1-1 μm. CoMoO4, on the other hand, has the morphology of a nanorod array.
[0062] Figure 3 The image shows the EDS elemental distribution of the NiMo / CoMoO4 catalyst prepared in Example 1. Specifically, the catalyst morphology was observed on a JEOL 2100F spectrometer, and the elemental distribution was studied using an energy-dispersive spectroscopy (EDS) instrument equipped with a QUANTAX 200-TEM. It can be seen that Ni, Co, Mo, and O elements are uniformly distributed on the catalyst, successfully demonstrating the formation of CoMoO4 and the incorporation of Ni into the catalyst.
[0063] Figure 4 (a) shows the XRD pattern of the prepared NiMo / CoMoO4 catalyst, specifically obtained by XRD analysis on an X'PertPRO. Characteristic peaks for NiNi (PDF#1-1266) and cobalt molybdate (PDF#21-0868) can be observed. The prepared catalyst sample and XRD pattern were obtained at 500 mA / cm². 2 The sample after undergoing a continuous hydrogen evolution reaction at a current density for 300 hours was characterized by Raman spectroscopy. Figure 4 (b) A comparison of the Raman spectra of the sample before and after the hydrogen evolution reaction is shown. Specifically, the Raman spectral signal was acquired on a HORIBA LabRAM with a laser wavelength of 832 nm. Raman signals of Co-O, Ni-O, MO-O, and Mo-O-Co were observed, indicating the successful synthesis of nickel-molybdenum modified cobalt molybdate NiMo / CoMoO4. Figure 4(c) Shows a comparison of the Ni 2p energy level spectra of XPS before and after the hydrogen evolution reaction of the sample. It can be seen that after the reaction, the Ni of the catalyst... 2+ The peak shifts to lower energies. Figure 4 (d) shows a comparison of the Mo 3d energy level spectra obtained by XPS for NiMo / CoMoO4. Before the reaction, the 3d splitting peak spacing of Mo was 3.52 eV, indicating that the oxidation state of Mo was +6. However, in the sample after the continuous hydrogen evolution reaction, Mo had both +4 and +6 oxidation states. This is because the hydrogen evolution electrode continuously gains electrons during the water electrolysis reaction, thereby reducing the oxidation state of the catalyst. The reduction in the Mo oxidation state helps to protect the stability of the oxidation states of metallic Ni and Co, ensuring the catalytic activity of the catalyst. The specific steps for XPS spectroscopy acquisition were to acquire XPS signals on an ESCALAB250XI (Thermo) system.
[0064] The NiMo / CoMoO4 and CoMoO4 catalysts prepared in Example 1 and Comparative Example 1 were tested for their water reduction performance under neutral conditions. The procedure was as follows: A three-electrode system was constructed using NiMo / CoMoO4 or CoMoO4 catalyst as the working electrode, silver chloride electrode as the reference electrode, and graphite rod electrode as the counter electrode. The system was placed in a neutral electrolyte to test its water reduction performance. The electrolyte was 1 mol / L phosphate buffer solution with a pH of 7.
[0065] Figure 5 (a) and (b) show the linear sweep voltammetry (LSV) curves of CoMoO4, NiMo / CoMoO4, and NiMoO4 samples in 1 mol / L phosphate buffer solution, as well as a detailed comparison of HER overpotentials. It can be observed that NiMo / CoMoO4 exhibits significantly improved HER performance at 10 and 500 mA / cm², respectively. 2 At current densities, the required HER overpotentials are only 46 and 454 mV, far superior to commercially available Pt / C samples. Further calculations of the Tafel slopes of these samples were performed. Figure 5 As shown in (c), the NiMo / CoMoO4 sample exhibits a low Tafel slope of 48.88 mV / dec, indicating that NiMo / CoMoO4 promotes faster OER reaction kinetics. Simultaneously, NiMo / CoMoO4 possesses better electrical conductivity, thereby facilitating rapid electron transfer on the catalyst, as... Figure 5 (d) shows the smaller charge transfer resistance of NiMo / CoMoO4 on the electrochemical impedance spectroscopy.
[0066] Figure 6 (a) Shows the CoMoO4 and NiMo / CoMoO4 samples in 1 mol / L PBS solution at 10 A / cm 2Stability comparison at current densities. It can be seen that the stability of NiMo / CoMoO4 is greatly improved at 10 mA / cm². 2 At the specified current density, the NiMo / CoMoO4 sample can operate stably for 1000 hours, while the CoMoO4 sample gradually degrades in performance after 20 hours of operation. Figure 6 (b) Demonstrates the performance of CoMoO4 and NiMo / CoMoO4 samples in 1 mol / L PBS solution at 500 mA / cm². 2 Stability at current density. At 500 mA / cm² 2 Under high current density, the NiMo / CoMoO4 sample can operate stably for more than 300 hours, demonstrating its excellent stability.
[0067] Comparative Example 3
[0068] A calcined CoMoO4-based composite material is provided, comprising the following steps:
[0069] A 1cm x 2cm nickel foam was sequentially placed in a 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water and sonicated for 15 minutes. The cleaned nickel foam was then placed in a 60mL mixed solution containing 0.15mol / L CoCl2, 0.05mol / L Ni(NO3)2, 0.06mol / L (NH4)2MoO4, 0.13mol / L urea, and 0.08mol / L ammonium fluoride. The reaction was carried out hydrothermally at 120℃ for 4 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly washed with anhydrous ethanol and deionized water, then dried in an oven set at 60℃ for 4 hours, and finally calcined in a muffle furnace at 300℃ for 3 hours. The resulting product was designated NiMo / CoMoO4-1.
[0070] The NiMo / CoMoO4-1 obtained in this comparative example was subjected to HER overpotential performance testing. The results showed that at 10 mA / cm 2 Overpotential 93mV, 500mA / cm 2 The overpotential is 612mV.
[0071] Example 2
[0072] A method for preparing a nickel-molybdenum modified cobalt molybdate composite material is provided, comprising the following steps:
[0073] A 1cm x 2cm nickel foam was sequentially placed in a 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water, and sonicated for 15 minutes. The cleaned nickel foam was then placed in a 60mL solution containing 0.2mol / L Co(NO3)2, 0.05mol / L NiCl2, 0.06mol / L K2MoO4, 0.13mol / L urea, and 0.08mol / L ammonium fluoride. The reaction was carried out hydrothermally at 200℃ for 2 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly rinsed with anhydrous ethanol and deionized water, and then dried in an oven at 60℃ for 4 hours to obtain a nanosheet-modified CoMoO4 nanorod array catalyst grown on nickel foam (denoted as "NiMo / CoMoO4").
[0074] The prepared nanosheet-modified CoMoO4 nanorod array was used as the working electrode, a silver chloride electrode as the reference electrode, and a graphite rod electrode as the counter electrode to form a three-electrode system. The system was placed in a neutral electrolyte (6 mol / L sodium chloride) to test its water reduction performance. The sample exhibited water reduction performance at 10 and 500 mA / cm². 2 The overpotential of neutral water reduction at a given current density is shown in Table 1.
[0075] Example 3
[0076] A method for preparing a nickel-molybdenum modified cobalt molybdate composite material is provided, comprising the following steps:
[0077] Nanosheet-modified CoMoO4 nanorod arrays were synthesized using a hydrothermal method. A 1cm x 2cm nickel mesh was sequentially placed in 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water, and sonicated for 15 mins. Then, the cleaned nickel foam was placed in a 60mL solution containing 0.09mol / L CoCO3, 0.05mol / L Ni(NO3)2, 0.06mol / L (NH4)2MoO4, 0.13mol / L urea, and 0.08mol / L ammonium fluoride. The reaction was carried out hydrothermally at 140℃ for 16 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly washed with anhydrous ethanol and deionized water, and then dried in an oven set to 60℃ for 4 hours to obtain the nanosheet-modified CoMoO4 nanorod array catalyst grown on nickel foam (denoted as "NiMo / CoMoO4").
[0078] The prepared nanosheet-modified CoMoO4 nanorod array was used as the working electrode, the silver chloride electrode as the reference electrode, and the graphite rod electrode as the counter electrode to form a three-electrode system. The system was placed in a neutral electrolyte (5 mol / L phosphate buffer) to test its water reduction performance. The sample exhibited water reduction performance at 10 and 500 mA / cm². 2The overpotential of neutral water reduction at a given current density is shown in Table 1.
[0079] Example 4
[0080] A method for preparing a nickel-molybdenum modified cobalt molybdate composite material is provided, comprising the following steps:
[0081] A 1cm x 2cm nickel-iron foam was sequentially placed in a 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water and sonicated for 15 minutes. The cleaned nickel foam was then placed in a 60mL solution containing 0.07mol / L CoCl2, 0.05mol / L NiCl2, 0.06mol / L Na2MoO4, 0.13mol / L urea, and 0.08mol / L ammonium fluoride. The reaction was carried out hydrothermally at 180℃ for 12 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly rinsed with anhydrous ethanol and deionized water, and then dried in an oven at 60℃ for 4 hours to obtain a nanosheet-modified CoMoO4 nanorod array catalyst (denoted as "NiMo / CoMoO4") grown on nickel foam.
[0082] The prepared nanosheet-modified CoMoO4 nanorod array was used as the working electrode, the silver chloride electrode as the reference electrode, and the graphite rod electrode as the counter electrode to form a three-electrode system. The system was placed in a neutral electrolyte (1 mol / L phosphate buffer) to test its water reduction performance. The sample exhibited water reduction performance at 10 and 500 mA / cm². 2 The overpotential of neutral water reduction at a given current density is shown in Table 1.
[0083] Example 5
[0084] A method for preparing a nickel-molybdenum modified cobalt molybdate composite material is provided, comprising the following steps:
[0085] A 1cm x 2cm stainless steel felt was sequentially placed in a 3mol / L hydrochloric acid solution, anhydrous ethanol, and deionized water and sonicated for 15 minutes. Then, the cleaned nickel foam was placed in a 60mL solution containing 0.12mol / L CoCl2, 0.05mol / L NiSO4, 0.06mol / L K2MoO4, 0.13mol / L urea, and 0.08mol / L ammonium fluoride. The reaction was carried out hydrothermally at 150℃ for 8 hours. After the reaction was complete and cooled to room temperature, the catalyst was repeatedly rinsed with anhydrous ethanol and deionized water, and then dried in an oven set to 60℃ for 4 hours to obtain a nanosheet-modified CoMoO4 nanorod array catalyst grown on nickel foam (denoted as "NiMo / CoMoO4").
[0086] The prepared nanosheet-modified CoMoO4 nanorod array was used as the working electrode, silver chloride electrode as the reference electrode, and graphite rod electrode as the counter electrode to form a three-electrode system. The system was placed in a neutral electrolyte (2 mol / L potassium sulfate) to test its water reduction performance. The sample exhibited water reduction performance at 10 and 500 mA / cm². 2 The overpotential of neutral water reduction at a given current density is shown in Table 1.
[0087] Table 1. Summary of neutral water reduction properties of NiMo / CoMoO4 samples prepared in Examples 1-6
[0088]
[0089] The above are merely preferred embodiments of the present invention. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention, and these should also be considered within the scope of protection of the present invention. These will not affect the effectiveness of the implementation of the present invention or the practicality of the patent.
Claims
1. The application of a nickel-molybdenum modified cobalt molybdate composite material in the hydrogen evolution reaction of water electrolysis under neutral conditions; characterized in that, The nickel-molybdenum modified cobalt molybdate composite material includes a conductive substrate and nickel-molybdenum modified cobalt molybdate grown on the conductive substrate. The nickel-molybdenum modified cobalt molybdate has the morphology of cobalt molybdate nanorod array modified with nickel molybdate nanosheets, wherein the thickness of the nanosheets is 5-80 nm and the diameter of the nanorods is 0.1-1 μm.
2. The application according to claim 1, characterized in that, The nickel-molybdenum modified cobalt molybdate composite material is used as a hydrogen evolution electrode to carry out the water hydrogen evolution reduction reaction in a neutral three-electrode system.
3. The application according to claim 1, characterized in that, The conductive substrate is any one of the following: nickel foam, nickel mesh, nickel felt, stainless steel felt, nickel-iron foam, copper foil, copper foam, iron foam, titanium mesh, carbon cloth, carbon paper, graphite felt, carbon fiber, and carbon materials obtained by calcining various fruit shells and mollusk shells.
4. The application according to claim 1, characterized in that, The nickel-molybdenum modified cobalt molybdate composite material is prepared by hydrothermal reaction of a conductive substrate with urea, ammonium fluoride, cobalt salt, molybdenum salt, nickel salt and water.
5. The application according to claim 1, characterized in that, The preparation method of the nickel-molybdenum modified cobalt molybdate composite material includes the following steps: A conductive substrate is placed in a mixed solution of urea, ammonium fluoride, cobalt salt, molybdenum salt, nickel salt and water, and a hydrothermal reaction is carried out to grow a nanosheet-modified CoMoO4 nanorod array on the conductive substrate, thus obtaining a nickel-molybdenum-modified cobalt molybdate composite material.
6. The application according to claim 5, characterized in that, The cobalt salt is any one of Co(NO3)2, CoSO4, CoCO3, Co3(PO4)2, and CoCl2; the molybdenum salt is any one of Na2MoO4, K2MoO4, and (NH4)2MoO4; and the nickel salt is any one of Ni(NO3)2, NiSO4, and NiCl2.
7. The application according to claim 5, characterized in that, The molar ratio of cobalt in the cobalt salt to molybdenum in the molybdenum salt is 1:0.3-1.2; the molar ratio of cobalt in the cobalt salt to nickel in the nickel salt is 1:0.25-1; and the concentration of cobalt in the cobalt salt is 0.005-0.200 mol / L.
8. The application according to claim 5, characterized in that, The molar ratio of cobalt in urea, ammonium fluoride and cobalt salt is 1:0.4-0.8:0.6-1.
5.
9. The application according to claim 5, characterized in that, The hydrothermal reaction is carried out at a temperature of 100-200 ℃ for a time of 2-20 h.