A method for preparing a spinning solution and a device therefor

By using extruder shearing and magnetic heating through the feed tube during the spinning solution preparation process, the problem of polymer degradation at room temperature and pressure was solved, enabling continuous feeding and rapid dissolution under high temperature and high pressure, thus improving preparation efficiency and safety.

CN119800523BActive Publication Date: 2026-11-24GUANGDONG KINGFA TECH CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311316724.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-11
Publication Date
2026-11-24
Estimated Expiration
2043-10-11

AI Technical Summary

Technical Problem

In existing spinning solution preparation processes, polymers are prone to degradation when fed into the reactor at room temperature and pressure, which affects preparation efficiency.

Method used

The melt is formed by shearing in an extruder, and magnetic force and heating are applied in the feeding pipe to keep the melt under high temperature and high pressure before entering the reactor, thus avoiding polymer degradation. Magnetic additives are used to enhance intermolecular forces, enabling continuous feeding and rapid dissolution under high temperature and high pressure.

Benefits of technology

It improves the preparation efficiency of spinning solution, shortens the preparation time, avoids polymer degradation, and ensures the safety and efficiency of the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119800523B_ABST
    Figure CN119800523B_ABST
Patent Text Reader

Abstract

This invention relates to the field of spinning solution preparation technology, and discloses a method and apparatus for preparing spinning solution. The method involves shearing and extruding polyethylene through an extruder, transforming it from a solid into a fluid melt. This melt is then pressurized by a metering pump to form a high-temperature, high-pressure melt. More importantly, heating reduces heat loss as the melt flows through the feeding pipe, preventing solidification. Simultaneously, applying magnetic force to the magnetic material within the melt further increases the intermolecular forces, thus maintaining the polyethylene melt temperature and its dissolution temperature within a controllable range before entering the reactor. The reactor does not require slow heating and pressurization; the dissolution reaction can proceed directly, avoiding polymer degradation. This method enables continuous feeding and rapid dissolution under high temperature and pressure, significantly shortening the preparation time and improving efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of spinning solution preparation technology, and in particular to a method and apparatus for preparing a spinning solution. Background Technology

[0002] Flash spinning is a method for preparing nanofiber nonwoven fabrics. The principle is to dissolve the fiber-forming polymer in a suitable solvent under high temperature and high pressure to form a uniform spinning solution. Then, the solution is ejected from the spinneret. After ejection, the pressure suddenly drops to normal pressure, and the solvent evaporates instantly due to overheating, generating a large amount of airflow. While the polymer is cooling, it is stretched to form nanofiber bundles. The direction of movement of these bundles can be changed by baffles or other equipment. Before reaching the receiving device, they pass through a high-voltage electrostatic field, which charges each fiber and separates them. Then, through processes such as web laying and web fixing, a nonwoven fabric is formed.

[0003] In existing spinning solution preparation processes, polymers are typically added to a reactor at room temperature and pressure. As the reactor gradually heats up, the polymers are prone to degradation, which affects the efficiency of spinning solution preparation. There is an urgent need for a preparation process that allows the polymers to enter the reactor under high temperature and high pressure. Summary of the Invention

[0004] The purpose of this invention is to provide a safe and efficient method for preparing spinning solution.

[0005] To achieve the above objectives, the present invention provides a method for preparing a spinning solution, comprising the following steps:

[0006] The polyethylene, solvent, plasticizer, and magnetic additives are mixed and then added to the extruder;

[0007] After being sheared and heated by the extruder to form a melt, it is output to the metering pump;

[0008] The melt pressure is increased to 15-20 MPa by the metering pump.

[0009] When the melt is conveyed to the reactor through the feeding pipe, magnetic force and heating are applied simultaneously to make the melt temperature 200℃≤t≤220℃;

[0010] Shearing and dissolution are carried out through the reaction vessel.

[0011] In some embodiments of this application, the magnetic additive is made of one or more of nano-ferrite, AlNiCo alloy, and rare earth permanent magnet materials, and its content is 0.05 to 1 wt% of polyethylene.

[0012] In some embodiments of this application, the plasticizer is made from one or more of white oil and decahydronaphthalene, and its content is 15-30 wt% of polyethylene.

[0013] In some embodiments of this application, the feeding tube includes a tube body, an electromagnetic layer, and a heating layer. The tube body is connected to the discharge port. The electromagnetic layer and the heating layer are sequentially disposed on the outer peripheral wall of the tube body from the inside to the outside. The electromagnetic layer is used to apply magnetic force to the melt.

[0014] In some embodiments of this application, the weight-average molecular weight of the polyethylene is 100k to 4200k.

[0015] In some embodiments of this application, the polyethylene in the melt has a diameter of 1 mm to 3.5 mm and a length of 3 mm to 5 mm when it enters the reactor.

[0016] Another object of the present invention is to provide an apparatus for preparing a spinning solution, which applies the above-described method for preparing a spinning solution, the apparatus comprising:

[0017] An extruder, which is equipped with a feed port and a discharge port;

[0018] The feeding tube includes a tube body, an electromagnetic layer, and a heating layer. The tube body is connected to the outlet. The electromagnetic layer and the heating layer are arranged sequentially from the inside to the outside on the outer peripheral wall of the tube body. The electromagnetic layer is used to apply magnetic force to the melt.

[0019] A metering pump is installed at the discharge port and connected to the pipe body;

[0020] The reactor is connected to the extruder via the feed pipe.

[0021] In some embodiments of this application, the electromagnetic layer is an electromagnetic coil, which is wound around the outside of the tube, and the heating layer is attached to the outside of the electromagnetic coil.

[0022] In some embodiments of this application, the extruder is a single-screw extruder, the screw length-to-diameter ratio of the extruder is 1:30 to 1:40, and the screw compression ratio is 2 to 4.

[0023] In some embodiments of this application, a three-way valve is also included, which is disposed between the extruder and the metering pump and connects the two, and another output port of the three-way valve is connected to a melt delivery pipeline.

[0024] This invention provides a method for preparing spinning solution, which has the following advantages compared with the prior art:

[0025] The spinning solution preparation method provided by this invention transforms polyethylene from a solid into a fluid melt through shearing and extrusion in an extruder. This melt is then pressurized by a metering pump to form a high-temperature, high-pressure melt. More importantly, heating reduces heat loss as the melt flows through the feeding pipe, preventing solidification. Simultaneously, applying magnetic force to the magnetic material within the melt further increases the intermolecular forces, thus maintaining the polyethylene melt temperature and its dissolution temperature within a controllable range before entering the reactor. At this point, the reactor does not require slow heating and pressurization; the dissolution reaction can proceed directly, avoiding polymer degradation. This method enables continuous feeding and rapid dissolution under high temperature and pressure, significantly shortening the preparation time and improving efficiency. Attached Figure Description

[0026] Figure 1 This is a schematic flowchart of the method for preparing spinning solution according to an embodiment of the present invention;

[0027] Figure 2 This is a schematic diagram of the spinning solution preparation apparatus according to an embodiment of the present invention.

[0028] In the diagram: 1. Extruder; 11. Feed port; 12. Discharge port; 2. Feed pipe; 3. Three-way valve; 4. Reactor; 5. Melt conveying pipeline. Detailed Implementation

[0029] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0030] It should be understood that in the description of this application, the terms "center," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are used solely for the convenience of describing this application and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application. The terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. That is, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. Furthermore, unless otherwise stated, "a plurality of" means two or more.

[0031] It should be noted that, in the description of this application, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0032] like Figure 2 As shown, an embodiment of the present invention provides a spinning solution preparation apparatus, which includes an extruder 1, a feeding pipe 2, a metering pump and a reaction vessel 4.

[0033] The extruder 1 is equipped with a feed port 11 and a discharge port 12. The extruder 1 is a single-screw extruder 1 with a screw length-to-diameter ratio of 1:30 to 1:40, a compression ratio of 2 to 4, and a screw with equal depth but unequal pitch. The pitch of the metering section of the screw is the same as the screw diameter. Specifically, in this embodiment, corresponding to a 50-liter capacity reactor 4, the screw diameter can be specifically set to 65 mm, the length-to-diameter ratio to be 1:35, and the compression ratio to be 4. Based on this, the extruder 1 with this screw configuration can perform sufficient shearing action on polyethylene and plasticizer. Under high-temperature shearing action, the plasticizer enters the polyethylene molecular chain, increasing the intermolecular forces and further dissolving to form a melt. This results in the polyethylene in the melt entering the reactor 4 with a diameter of 1 mm to 3.5 mm and a length of 3 mm to 5 mm, facilitating subsequent shearing and dissolution in the reactor 4.

[0034] The feeding pipe 2 includes a pipe body, an electromagnetic layer, and a heating layer (not shown in the figure). The pipe body is connected to the outlet 12. The electromagnetic layer and the heating layer are sequentially disposed on the outer peripheral wall of the pipe body from the inside out. The electromagnetic layer is used to apply magnetic force to the melt. Preferably, the electromagnetic layer is an electromagnetic coil wound around the outside of the pipe body, and the heating layer is attached to the outside of the electromagnetic coil. Based on this, magnetic force and heating can be applied simultaneously to the melt flowing through the pipe body.

[0035] A metering pump, located at outlet 12 and connected to the pipe body, is used to pressurize the melt to maintain it at 15-20 MPa.

[0036] The reactor 4 is connected to the extruder 1 via the feed pipe 2. The reactor 4 is equipped with a cutting or crushing device, which causes the polyethylene sample to be broken into particles of a certain size, which then interact with the solvent to swell and finally complete the dissolution process.

[0037] Based on the above structure, the polyethylene and plasticizer are subjected to sufficient shearing action by a specially designed extruder 1 to form a melt. After being pressurized by a metering pump, the melt is fed into the reactor 4 at high temperature and high pressure through a feed pipe 2 equipped with an electromagnetic layer and a heating layer. This avoids polymer degradation and enables continuous feeding and rapid dissolution under high temperature and high pressure, which greatly shortens the preparation time and improves the preparation efficiency.

[0038] Optionally, such as Figure 2 As shown, in this embodiment, the spinning solution preparation device also includes a three-way valve 3, which is located between the extruder 1 and the metering pump, connecting the two. The other output port of the three-way valve 3 is connected to a melt delivery pipe 5. Therefore, the melt can be diverted and transported via the three-way valve 3.

[0039] like Figure 1 As shown in the figure, this embodiment of the invention also provides a method for preparing a spinning solution, which includes the following steps:

[0040] S1. Mix polyethylene, solvent, plasticizer and magnetic additive and add them into extruder 1;

[0041] S2, after being sheared and heated by extruder 1 to form a melt, it is output to the metering pump;

[0042] S3. Pressurize the melt by using a metering pump to make the melt pressure 15-20 MPa;

[0043] S4. When the melt is conveyed to the reactor 4 through the feed pipe 2, magnetic force and heating are applied to the melt at the same time to make the melt temperature 200℃≤t≤220℃;

[0044] S5. Shearing and dissolution are carried out through reaction vessel 4.

[0045] Based on the above method, polyethylene is transformed from a solid into a fluid melt through shearing and extrusion by extruder 1. This melt is then pressurized by a metering pump to form a high-temperature, high-pressure melt. More importantly, heating reduces heat loss as the melt flows through feed pipe 2, preventing solidification. Simultaneously, applying magnetic force to the magnetic material within the melt further increases the intermolecular forces, thus maintaining the polyethylene melt temperature and its dissolution temperature within a controllable range before entering reactor 4. Reactor 4 then allows for direct dissolution without slow heating and pressurization, avoiding polymer degradation. This enables continuous feeding and rapid dissolution under high temperature and pressure, significantly shortening preparation time and improving efficiency.

[0046] Optionally, in this embodiment, in step S1, the magnetic additive is made of one or more of nano-ferrite, AlNiCo alloy, and rare-earth permanent magnet materials, and its content is 0.05-1 wt% of polyethylene. The magnetic additive, mixed in polyethylene, can attract the magnetic layer, increasing the interaction force between intramolecular molecules in the melt and preventing solidification. It should be understood that when magnetic force and heating are applied to the melt simultaneously, the melt temperature is lower than the Curie temperature of the magnetic additive; that is, heating does not affect the magnetic properties of the magnetic additive.

[0047] Optionally, in this embodiment, the plasticizer is made from one or more of white oil and decahydronaphthalene, and its content is 15 to 30 wt% of polyethylene.

[0048] Optionally, in this embodiment, the weight-average molecular weight of polyethylene is 100k to 4200k. The preferred values ​​for the average molecular weight ranges are 100k to 1000k, 1000k to 2000k, 2000k to 3000k, and 3000k to 4200k. It should be understood that this molecular weight can be obtained by gel permeation chromatography.

[0049] Optionally, in this embodiment, the solvent is specifically 1,2-dichloroethane, and the final spinning solution concentration is 7% to 25 wt%.

[0050] In summary, the embodiments of the present invention provide a method for preparing spinning solution, which has advantages such as high preparation efficiency and high safety compared with the prior art.

[0051] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and substitutions can be made without departing from the technical principles of the present invention, and these improvements and substitutions should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a spinning solution, characterized in that, Includes the following steps: The polyethylene, solvent, plasticizer and magnetic additive are mixed and then added into the extruder (1); After being sheared and heated by the extruder (1) to form a melt, it is output to the metering pump; The melt pressure is increased to 15-20 MPa by the metering pump. When the melt is conveyed to the reactor (4) through the feed pipe (2), magnetic force and heating are applied to the melt at the same time, so that the melt temperature is 200℃≤t≤220℃; Shearing and dissolution are carried out through the reaction vessel (4); The feeding tube (2) includes a tube body, an electromagnetic layer and a heating layer. The electromagnetic layer and the heating layer are arranged sequentially from the inside to the outside on the outer peripheral wall of the tube body. The electromagnetic layer is used to apply magnetic force to the melt.

2. The method for preparing the spinning solution as described in claim 1, characterized in that: The magnetic additive is made of one or more of nano-ferrite, AlNiCo alloy, and rare earth permanent magnet materials, and its content is 0.05~1wt% of polyethylene.

3. The method for preparing the spinning solution as described in claim 1, characterized in that: The plasticizer is made from one or more of white oil and decahydronaphthalene, and its content is 15-30 wt% of polyethylene.

4. The method for preparing the spinning solution as described in claim 1, characterized in that: The extruder (1) has a discharge port (12), and the tube is connected to the discharge port (12).

5. The method for preparing the spinning solution as described in claim 4, characterized in that: The weight-average molecular weight of the polyethylene is 100k~4200k.

6. The method for preparing the spinning solution as described in claim 1, characterized in that: The polyethylene in the melt has a diameter of 1 mm to 3.5 mm and a length of 3 mm to 5 mm when it enters the reactor (4).

7. An apparatus for preparing spinning solution, characterized in that, The method for preparing spinning solution according to any one of claims 1-6, wherein the preparation apparatus comprises: The extruder (1) is provided with a feed port (11) and a discharge port (12); Feeding pipe (2), the feeding pipe (2) includes a pipe body, an electromagnetic layer and a heating layer. The pipe body is connected to the outlet (12). The electromagnetic layer and the heating layer are arranged sequentially from the inside to the outside on the outer peripheral wall of the pipe body. The electromagnetic layer is used to apply magnetic force to the melt. The electromagnetic layer is an electromagnetic coil. A metering pump is installed at the discharge port (12) and connected to the pipe body; The reactor (4) is connected to the extruder (1) through the feed pipe (2).

8. The apparatus for preparing spinning solution as described in claim 7, characterized in that: The electromagnetic coil is wound around the outside of the tube, and the heating layer is attached to the outside of the electromagnetic coil.

9. The apparatus for preparing spinning solution as described in claim 7, characterized in that: The extruder (1) is a single-screw extruder (1), the length-to-diameter ratio of the screw of the extruder (1) is 1:30~1:40, and the compression ratio of the screw is 2~4.

10. The apparatus for preparing spinning solution as described in claim 7, characterized in that: It also includes a three-way valve (3), which is located between the extruder (1) and the metering pump and connects the two. The other output port of the three-way valve (3) is connected to a melt delivery pipe (5).

Citation Information

Patent Citations

  • Magnetic control hydrate reaction generation device

    CN113842853A

  • Ultra-fine denier UHMW pe fiber

    US20230193518A1