Pvc composite sheet for photovoltaic backsheet film and method for preparing the same

By using PVC composite sheets in photovoltaic backsheet films and combining adhesive and hydrolysis-resistant layers, the problems of heat generation and brittleness of photovoltaic backsheet films are solved, thereby improving the service life and performance of photovoltaic modules.

CN119820952BActive Publication Date: 2026-11-24ANHUI JIAYANG NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411993391.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-31
Publication Date
2026-11-24
Estimated Expiration
2044-12-31

AI Technical Summary

Technical Problem

Existing photovoltaic backsheet films generate a lot of heat during use, are prone to yellowing and becoming brittle, which affects the lifespan of photovoltaic modules.

Method used

The material is made of PVC composite sheet, which includes an adhesive layer and a hydrolysis-resistant layer on both sides of the PVC substrate. The adhesive layer is composed of acrylic adhesive, inorganic filler, curing agent, etc., and the hydrolysis-resistant layer is composed of biaxially oriented polyester film and hydrolysis-resistant stabilizer. It is prepared by calendering and biaxial stretching process to enhance the bonding effect and weather resistance.

Benefits of technology

It improves the barrier properties, electrical insulation and heat resistance of photovoltaic backsheet film, reduces heat generation and extends the service life of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119820952B_ABST
    Figure CN119820952B_ABST
Patent Text Reader

Abstract

This invention relates to the field of photovoltaic backsheet technology, specifically to a PVC composite sheet for photovoltaic backsheet film and its preparation method. The PVC composite sheet for photovoltaic backsheet film includes a PVC substrate, and hydrolysis-resistant layers are connected to both sides of the PVC substrate by adhesive layers. The adhesive layers are composed of an acrylic adhesive, a first inorganic filler, a curing agent, a curing accelerator, a first hydrolysis-resistant stabilizer, a silane coupling agent, and a solvent. This invention uses relatively low-cost PVC material as the core layer, which reduces costs while also providing the photovoltaic backsheet film with good physical strength and impact resistance based on the high tensile strength of PVC material. This lays the foundation for maintaining the structural integrity of the photovoltaic backsheet film and resisting external pressure, thus ensuring the service life of the photovoltaic module.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photovoltaic backsheet technology, and more specifically to a PVC composite sheet for photovoltaic backsheet film and its preparation method. Background Technology

[0002] A photovoltaic (PV) backsheet (also known as a solar backsheet) is placed on the back of a photovoltaic (PV) module to protect and support the solar cells. Because PV backsheets are directly exposed to the air, they are susceptible to corrosion from water vapor, acidic gases, extreme temperatures, and ultraviolet radiation. Therefore, improving the weather resistance of PV backsheets has always been a focus of the industry. Furthermore, under prolonged exposure to sunlight, PV backsheets are prone to yellowing or cracking, which can severely affect their insulation and render the PV module unusable. Traditional PV backsheet films have low reflectivity (e.g., common PET films have a reflectivity of 80%-85%). The absorption of large amounts of light energy by the PV backsheet film can easily cause the solar module to overheat, affecting its lifespan. Therefore, high-reflectivity (≥97%) PV backsheet films have significant practical value. Summary of the Invention

[0003] The purpose of this invention is to address the problem that existing photovoltaic backsheet films generate a lot of heat during use, leading to yellowing and brittleness, which affects the service life of photovoltaic modules. This invention provides a PVC composite sheet for photovoltaic backsheet films and its preparation method. The PVC composite sheet for photovoltaic backsheet films provided by this invention has good barrier properties, electrical insulation, and heat resistance, while also having high reflectivity. It can effectively reduce the heat absorption on the surface of the photovoltaic backsheet, improve the conversion efficiency of the battery module, and its preparation method is simple and easy to operate.

[0004] To achieve the above objectives, the present invention provides a PVC composite sheet for photovoltaic backsheet film, comprising a PVC substrate, wherein both sides of the PVC substrate are respectively connected to a hydrolysis-resistant layer by an adhesive layer; wherein the adhesive layer comprises an acrylic adhesive, a first inorganic filler, a curing agent, a curing accelerator, a first hydrolysis-resistant stabilizer, a silane coupling agent and a solvent mixed together.

[0005] Preferably, the acrylic adhesive is an acrylic adhesive containing hydroxyl groups.

[0006] Preferably, the first inorganic filler is selected from one or a combination of at least two of titanium dioxide, silicon dioxide, aluminum oxide, aluminum sulfate, calcium carbonate, magnesium carbonate, aluminum silicate, and magnesium silicate.

[0007] Preferably, the particle size of the first inorganic filler is 0.01-1 μm.

[0008] Preferably, the first hydrolysis stabilizer is polycarbodiimide, carbodiimide, or a combination thereof.

[0009] Preferably, the adhesive layer comprises a mixture of the following components in weight percentages: 80-85% acrylic adhesive, 2-7% first inorganic filler, 3.5-5.5% curing agent, 0.2-0.5% curing accelerator, 0.1-0.5% first anti-hydrolysis stabilizer, 0.1-0.5% silane coupling agent, and 10-15% solvent.

[0010] Preferably, the thickness of the PVC substrate is 100-250 μm, the thickness of the adhesive layer is 5-15 μm, and the thickness of the hydrolysis-resistant layer is 20-50 μm.

[0011] Preferably, the hydrolysis-resistant layer is a biaxially oriented polyester film, and a second hydrolysis-resistant stabilizer is added to the interior of the biaxially oriented polyester film.

[0012] Preferably, the second hydrolysis stabilizer is polycarbodiimide, carbodiimide, or a combination thereof.

[0013] Preferably, the amount of the second hydrolysis-resistant stabilizer added is 5-8% of the total weight of the hydrolysis-resistant layer.

[0014] Preferably, a second inorganic filler is also added to the hydrolysis-resistant layer.

[0015] Preferably, the second inorganic filler is selected from one or a combination of at least two of titanium dioxide, silicon dioxide, aluminum oxide, aluminum sulfate, calcium carbonate, magnesium carbonate, aluminum silicate, and magnesium silicate.

[0016] Preferably, the particle size of the second inorganic filler is 0.01-0.1 μm.

[0017] Preferably, the amount of the second inorganic filler added is 1-3% of the total weight of the hydrolysis-resistant layer.

[0018] Preferably, the adhesive layer has a triangular prism-shaped protrusion structure pressed on the side near the hydrolysis-resistant layer, which is distributed along the length of the PVC composite sheet.

[0019] Preferably, the height of the protrusion structure is 5-20 μm and the apex angle is 120°±10°.

[0020] The present invention also provides a method for preparing the above-mentioned PVC composite sheet for photovoltaic backsheet film, comprising the following steps: preparing a PVC substrate using a calendering process; preparing a coating liquid for forming an adhesive layer; then coating the coating liquid onto the PVC substrate; and then bonding and fixing a hydrolysis-resistant layer formed by a biaxial stretching process onto the PVC substrate.

[0021] Through the above technical solution, by connecting the hydrolysis-resistant layer to both sides of the PVC substrate using adhesive layers, a photovoltaic backsheet film with excellent barrier properties, electrical insulation, and heat resistance is obtained while reducing raw material costs. Compared with traditional photovoltaic backsheet films that use PET material as the core layer, this invention uses relatively low-cost PVC material as the core layer. While reducing costs, it also leverages the high tensile strength of PVC material to give the photovoltaic backsheet film better physical strength and impact resistance, thus laying the foundation for maintaining the structural integrity of the photovoltaic backsheet film and resisting external pressure, ensuring the service life of the photovoltaic module. In addition, the first inorganic filler filled in the adhesive layer provided by this invention can improve the aging resistance and reflect the light transmitted through the hydrolysis-resistant layer. This not only improves the light utilization rate of the photovoltaic module but also reduces the heat generation of the photovoltaic backsheet film, effectively improving the problem of overheating of the photovoltaic backsheet film, which affects its lifespan and leads to yellowing, cracking, and other issues that affect the service life of the photovoltaic module.

[0022] Other features and advantages of the embodiments of the present invention will be described in detail in the following detailed description section. Attached Figure Description

[0023] The accompanying drawings are provided to further illustrate embodiments of the present invention and form part of the specification. They are used together with the following detailed description to explain the embodiments of the present invention, but do not constitute a limitation thereof. In the drawings:

[0024] Figure 1 This is a structural schematic diagram of a PVC composite sheet for photovoltaic backsheet film provided by the present invention;

[0025] Explanation of reference numerals in the attached figures

[0026] 1. PVC substrate; 2. Adhesive layer; 3. Hydrolysis resistant layer. Detailed Implementation

[0027] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings and specific examples. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the scope of the present invention.

[0028] Combination Figure 1 As shown, the present invention provides a PVC composite sheet for photovoltaic backsheet film. The PVC composite sheet for photovoltaic backsheet film includes a PVC substrate 1, and two sides of the PVC substrate 1 are respectively connected to a hydrolysis-resistant layer 3 by an adhesive layer 2. The adhesive layer 2 is composed of an acrylic adhesive, a first inorganic filler, a curing agent, a curing accelerator, a first hydrolysis-resistant stabilizer, a silane coupling agent and a solvent.

[0029] Compared to traditional photovoltaic backsheet films that use PET material as the core layer, this invention uses PVC substrate, which has relatively inexpensive raw materials and a relatively mature manufacturing process, as the core layer, thus reducing the cost of the photovoltaic backsheet film. In addition, thanks to the high tensile strength of PVC material, the photovoltaic backsheet film has good physical strength and impact resistance, which lays the foundation for maintaining the structural integrity of the photovoltaic backsheet film and resisting external pressure, ensuring the service life of the photovoltaic module.

[0030] In the technical solution provided by the present invention, the adhesive layer 2 serves as a connector on the one hand, and the first inorganic filler filled inside it can improve the aging resistance on the other hand. Furthermore, the first inorganic filler filled in the adhesive layer 2 can reflect the light transmitted through the hydrolysis resistant layer 3, which can improve the light utilization rate of the photovoltaic module on the one hand, and reduce the heat generation of the photovoltaic backsheet film on the other hand. This effectively improves the problem of overheating of the photovoltaic backsheet film, which affects its lifespan and leads to yellowing, cracking, and other issues that affect the service life of the photovoltaic module.

[0031] In this invention, the acrylic adhesive can be an acrylic adhesive containing hydroxyl groups. Acrylic adhesives containing carboxyl groups can chemically react with the surface of the PVC substrate, thereby enhancing the adhesion between the adhesive layer and the PVC substrate.

[0032] In this invention, the first inorganic filler may be selected from one or a combination of at least two of titanium dioxide, silicon dioxide, aluminum oxide, aluminum sulfate, calcium carbonate, magnesium carbonate, aluminum silicate, and magnesium silicate. The particle size of the first inorganic filler may be selected within an appropriate range. Preferably, the particle size of the first inorganic filler is 0.01-1 μm, for example, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, or 1 μm.

[0033] In this invention, the first hydrolysis-resistant stabilizer enhances the hydrolysis resistance of the hydrolysis-resistant layer on the outer side of the PVC substrate. Preferably, the first hydrolysis-resistant stabilizer can be polycarbodiimide, carbodiimide, or a combination of polycarbodiimide and carbodiimide. When a combination of polycarbodiimide and carbodiimide is used as the first hydrolysis-resistant stabilizer, the weight ratio of polycarbodiimide to carbodiimide can be 1:1.

[0034] In this invention, the amount of each raw material component in the adhesive layer can be selected within an appropriate range. In some embodiments of this invention, the adhesive layer comprises the following components in weight percentage: 80-85% acrylic adhesive, 2-7% first inorganic filler, 3.5-5.5% curing agent, 0.2-0.5% curing accelerator, 0.1-0.5% first anti-hydrolysis stabilizer, 0.1-0.5% silane coupling agent, and 10-15% solvent.

[0035] In this invention, the thickness of the PVC substrate is 100-250 μm, the thickness of the adhesive layer is 5-15 μm, and the thickness of the hydrolysis-resistant layer is 20-50 μm.

[0036] In this invention, the hydrolysis-resistant layer is a biaxially oriented polyester film, and a second hydrolysis-resistant stabilizer is added to the interior of the biaxially oriented polyester film. Preferably, the second hydrolysis-resistant stabilizer can be polycarbodiimide, carbodiimide, or a combination of polycarbodiimide and carbodiimide. When a combination of polycarbodiimide and carbodiimide is used as the second hydrolysis-resistant stabilizer, the weight ratio of polycarbodiimide to carbodiimide can be 1:1. In this invention, the amount of the second hydrolysis-resistant stabilizer added is 5-8% of the total weight of the hydrolysis-resistant layer.

[0037] In some embodiments, a second inorganic filler is further added to the hydrolysis-resistant layer; the second inorganic filler is selected from one or a combination of at least two of titanium dioxide, silicon dioxide, aluminum oxide, aluminum sulfate, calcium carbonate, magnesium carbonate, aluminum silicate, and magnesium silicate; the particle size of the second inorganic filler is 0.01-0.1 μm; and the amount of the second inorganic filler added is 1-3% of the total weight of the hydrolysis-resistant layer.

[0038] In some embodiments, the adhesive layer has a triangular prism-shaped protrusion distributed along the length of the PVC composite sheet pressed on the side near the hydrolysis-resistant layer; further, the height of the protrusion is 5-20 μm, and the apex angle is 120°±10°. This configuration further increases the contact area between the adhesive layer and the hydrolysis-resistant layer, thus improving the bonding effect.

[0039] The present invention also provides a method for preparing the above-mentioned PVC composite sheet for photovoltaic backsheet film, comprising the following steps: preparing a PVC substrate using a calendering process; preparing a coating liquid for forming an adhesive layer; then coating the coating liquid onto the PVC substrate; and then bonding and fixing a hydrolysis-resistant layer formed by a biaxial stretching process onto the PVC substrate.

[0040] The performance of the PVC composite sheet for photovoltaic backsheet film provided by the present invention will be further illustrated below through specific embodiments. Furthermore, the test methods for the adhesion performance, barrier properties, and weather resistance of the photovoltaic backsheet film in the following embodiments are briefly described below:

[0041] 1) Adhesion test

[0042] The obtained photovoltaic backsheet film was cut into strips 15mm wide and approximately 1m long. A small portion of the hydrolysis-resistant layer was peeled off from one end of each strip. The PVC substrate and the hydrolysis-resistant layer were clamped separately on a tensile testing machine (Instron universal testing machine) and stretched at a 180° angle until they were completely and continuously peeled apart. The tensile force data displayed during the stretching process was recorded, which indicates the force required for peeling. A greater peel force indicates better adhesion of the photovoltaic backsheet film.

[0043] 2) Barrier test

[0044] Barrier properties are characterized by water vapor transmission rate, and the test environment is 35±5℃ and 95±5% according to the method disclosed in ISO15106-3 test standard.

[0045] 3) Weather resistance test

[0046] Weather resistance is characterized by delamination, breakdown voltage, and discoloration. Delamination testing was performed on samples using the method disclosed in the IEC 61215 standard for solar panel certification / solar photovoltaic panels. The test conditions were: temperature 85℃, relative humidity 85%RH, and time 2000 hours. The presence or absence of delamination was observed; no delamination was considered OK, and delamination was considered NO. Breakdown voltage testing was performed on samples using the method disclosed in the ASTM F-149 standard. The discoloration test involved placing the sample at 60℃ under a 1KW ultraviolet xenon lamp for 150 hours and observing for discoloration; no discoloration was considered OK, and discoloration was considered NO.

[0047] Example 1

[0048] A PVC substrate with a thickness of 200 μm was prepared from PVC raw material (purchased from Formosa Plastics, model S-70) using a calendering process.

[0049] Prepare the coating liquid for forming the adhesive layer according to the following formula:

[0050] The composition includes: 82.5% hydroxyl-containing acrylic adhesive (brand name 8723, manufactured by Nippon Synthetic Chemicals Co., Ltd.); 3.5% inorganic filler (rutile titanium dioxide; particle size 0.02μm); 4.0% curing agent (brand name D201, Dornex); 0.5% curing accelerator (dibutyltin dilaurate); 0.5% hydrolysis stabilizer (polycarbodiimide, brand name P200, Stabaxol series from Rheinland AG, Germany); 0.5% silane coupling agent (NCO-C3H6-Si(OCH3)3); and 8.5% solvent (butyl acetate).

[0051] The above coating liquid is scraped onto both sides of the PVC substrate and a hydrolysis-resistant layer is adhered to each side; wherein the thickness of the adhesive layer is 10μm and the thickness of the hydrolysis-resistant layer is 50μm.

[0052] The hydrolysis-resistant layer is a biaxially oriented polyester film containing polycarbodiimide (grade P200, Stabaxol series from Rheinland, Germany) and titanium dioxide (rutile type, particle size 0.02μm). The amount of polycarbodiimide added is 5% of the total weight of the hydrolysis-resistant layer, and the amount of titanium dioxide added is 3% of the total weight of the hydrolysis-resistant layer.

[0053] The PVC composite sheet for photovoltaic backsheet film prepared in the above embodiments has an interlayer peel strength of 75N / 15mm and a water vapor transmission rate of 0.13g / m2·24h. In terms of weather resistance, the delamination phenomenon is OK, the breakdown voltage is 28.5kV, and the discoloration phenomenon is OK.

[0054] It can be seen from this that the PVC composite sheet for photovoltaic backsheet film provided by the present invention has excellent performance and can completely replace the existing photovoltaic backsheet film based on PET material as the core layer.

[0055] The optional embodiments of the present invention have been described in detail above with reference to the accompanying drawings and examples. However, the embodiments of the present invention are not limited to the specific details in the above embodiments. Within the scope of the technical concept of the embodiments of the present invention, various simple modifications can be made to the technical solutions of the embodiments of the present invention, and these simple modifications all fall within the protection scope of the embodiments of the present invention.

[0056] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the embodiments of the present invention will not describe the various possible combinations separately.

[0057] Furthermore, various different embodiments of the present invention can be combined arbitrarily, as long as they do not violate the spirit of the embodiments of the present invention, they should also be regarded as the content disclosed by the embodiments of the present invention.

Claims

1. A PVC composite sheet for photovoltaic backsheet films, characterized by, It includes a PVC substrate, and both sides of the PVC substrate are respectively connected to a hydrolysis-resistant layer by an adhesive layer; The adhesive layer is composed of an acrylic adhesive, a first inorganic filler, a curing agent, a curing accelerator, a first hydrolysis stabilizer, a silane coupling agent, and a solvent. The acrylic adhesive is an acrylic adhesive containing hydroxyl groups; The first inorganic filler is selected from one or a combination of at least two of titanium dioxide, silicon dioxide, aluminum oxide, aluminum sulfate, calcium carbonate, magnesium carbonate, aluminum silicate, and magnesium silicate; The thickness of the PVC substrate is 100-250μm, the thickness of the adhesive layer is 5-15μm, and the thickness of the hydrolysis-resistant layer is 20-50μm; The adhesive layer has a triangular prism-shaped protrusion structure pressed on the side near the hydrolysis-resistant layer, which is distributed along the length of the PVC composite sheet. The hydrolysis-resistant layer is a biaxially oriented polyester film, and a second hydrolysis-resistant stabilizer is added to the interior of the biaxially oriented polyester film.

2. The PVC composite sheet for photovoltaic backsheet film according to claim 1, characterized in that, The particle size of the first inorganic filler is 0.01-1 μm.

3. The PVC composite sheet for photovoltaic backsheet film according to claim 1, characterized in that, The first hydrolysis stabilizer is polycarbodiimide, carbodiimide, or a combination thereof.

4. The PVC composite sheet for photovoltaic backsheet film according to claim 1, characterized in that, The adhesive layer is composed of the following components in weight percentage: 82.5% acrylic adhesive, 3.5% first inorganic filler, 4.0% curing agent, 0.5% curing accelerator, 0.5% first anti-hydrolysis stabilizer, 0.5% silane coupling agent, and 8.5% solvent.

5. The PVC composite sheet for photovoltaic backsheet film according to claim 1, characterized in that, The second hydrolysis stabilizer is polycarbodiimide, carbodiimide, or a combination thereof.

6. The PVC composite sheet for photovoltaic backsheet film according to claim 1, characterized in that, The amount of the second hydrolysis-resistant stabilizer added is 5-8% of the total weight of the hydrolysis-resistant layer.

7. The PVC composite sheet for photovoltaic backsheet film according to claim 1, characterized in that, A second inorganic filler is also added to the hydrolysis-resistant layer.

8. The PVC composite sheet for photovoltaic backsheet film according to claim 7, characterized in that, The second inorganic filler is selected from one or a combination of at least two of titanium dioxide, silicon dioxide, aluminum oxide, aluminum sulfate, calcium carbonate, magnesium carbonate, aluminum silicate, and magnesium silicate.

9. The PVC composite sheet for photovoltaic backsheet film according to claim 7, characterized in that, The particle size of the second inorganic filler is 0.01-0.1 μm.

10. The PVC composite sheet for photovoltaic backsheet film according to claim 7, characterized in that, The amount of the second inorganic filler added is 1-3% of the total weight of the hydrolysis-resistant layer.

11. The PVC composite sheet for photovoltaic backsheet film according to any one of claims 1-10, characterized in that, The height of the protrusion structure is 5-20μm, and the apex angle is 120°±10°.

12. The method for preparing PVC composite sheet for photovoltaic backsheet film according to any one of claims 1-10, characterized in that, Includes the following steps: PVC substrates are prepared using a calendering process; A coating solution for forming the adhesive layer is prepared, and then the coating solution is applied to the PVC substrate. Next, a hydrolysis-resistant layer made by biaxial stretching process is bonded and fixed to the PVC substrate.

Citation Information

Patent Citations

  • Solar cell backboard

    CN101515603A

  • High-reflection solar cell backing plate

    CN105449024A

  • Photovoltaic backboard with rigid foam sandwich structure and production process thereof

    CN116100896A