A method and apparatus for efficiently stripping spent lithium-ion battery cathode material and aluminum foil

By combining flotation and aerated flotation equipment, the problem of separating lithium-ion battery cathode materials from aluminum foil has been solved, achieving efficient and low-cost separation, reducing aluminum impurity content, and making it suitable for industrial scale-up production.

CN119838767BActive Publication Date: 2026-11-24WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411776642.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-05
Publication Date
2026-11-24
Estimated Expiration
2044-12-05

AI Technical Summary

Technical Problem

In existing technologies, separating the cathode material of lithium-ion batteries from aluminum foil is difficult, resulting in a high aluminum content in the recycled repair material. Furthermore, traditional separation methods are energy-intensive, costly, and difficult to control impurities.

Method used

By employing flotation combined with aerated flotation equipment, and by adding a frother and controlling the distance between the agitator and the separator, efficient separation of the cathode material and aluminum foil is achieved, and the equipment is designed to be suitable for industrial scale-up.

Benefits of technology

The aluminum impurity content of the recycled repair material was significantly reduced, and the aluminum foil separation rate reached 95%. Furthermore, the aluminum impurities were further reduced by improving the flotation equipment, thereby improving separation efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119838767B_ABST
    Figure CN119838767B_ABST
Patent Text Reader

Abstract

This invention provides an efficient method for separating positive electrode material and aluminum foil from waste lithium-ion batteries, comprising: aeration stripping: placing the battery electrode material into an aeration flotation device, adding a certain amount of stripping agent, opening the aeration valve to start aeration, achieving the separation of the positive electrode material from the aluminum foil in the electrode material, and then closing the aeration valve; flotation separation: adjusting the distance between the agitator and the isolation screen, starting agitation, adding a foaming agent, stirring for a certain time, and then starting aeration. When the aluminum foil no longer floats, the distance between the agitator and the isolation screen is lowered, and agitation and aeration continue. The upper layer of material is collected as aluminum foil, and the lower layer of material is collected as positive electrode active material. The aeration flotation device includes an air flotation reactor, an agitator, an aeration plate, and an isolation screen. The isolation screen is placed on the aeration plate and together with it at the bottom of the air flotation reactor. The agitator is placed inside the air flotation reactor, and the distance between the agitator and the isolation screen is adjustable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of waste lithium-ion battery material recycling technology, specifically to an efficient method for separating waste lithium-ion battery cathode material and aluminum foil, and equipment for achieving efficient separation of waste lithium-ion battery cathode material and aluminum foil. Background Technology

[0002] In recent years, with the promotion of new energy vehicles by the state, the production of electric vehicles and the amount of lithium-ion batteries produced and scrapped have been increasing. Currently, battery recycling technologies are mainly dry and wet recycling. The former recovers valuable metal elements by incinerating them in a high-temperature furnace, which has problems such as environmental pollution and low recovery rate. The latter recovers elements through chemical leaching, precipitation, and extraction, which is a long process and costly. Unlike dry and wet recycling, direct repair and regeneration technology is attracting increasing attention from research institutions and recycling companies. This method separates battery materials and, through a shorter repair process, replenishes missing elements and restores the material structure, thereby achieving the recycling of battery materials and preserving the original performance of the materials to the greatest extent. It has advantages such as low cost, high quality, and environmental protection. For example, CN218215435U discloses a reaction vessel for battery electrode stripping, including a box body, the inner cavity of which serves as the space for electrode reaction; a stirring device, set at the bottom of the box body, used to drive the reaction liquid inside the box body to rotate, generating centrifugal force to separate and break the electrode sheets; and at least two filter plates, which are fixed in the inner cavity of the box body by multiple support rings set on the inner wall of the box body. However, this device only separates the black material and aluminum foil by stirring and crushing the electrode black material. During the process, the aluminum foil is also easily broken, resulting in a high level of aluminum impurities in the black material.

[0003] Because the positive electrode active material is tightly bonded to the aluminum foil through the binder, the direct repair and regeneration technology of battery materials faces the problem of difficulty in separating the positive electrode material from the aluminum foil during industrial scale-up, and the aluminum content of the regenerated repair material is too high. Although methods such as cyclone separation and gravity separation can improve the aluminum content problem, the yield is difficult to guarantee. There is an urgent need to develop an aluminum foil peeling technology and supporting equipment suitable for industrial scale-up. Summary of the Invention

[0004] The purpose of this invention is to solve at least one of the following technical problems:

[0005] (1) Cathode materials, as the most valuable part of battery recycling, are bonded to aluminum current collectors in the form of cathode sheets, mixed with conductive carbon and binders. Because the material properties of these sheets are not damaged, they can be directly reused after peeling, composition adjustment, and heat treatment, without the need for wet refining, and have extremely high tiered utilization value. Among them, the peeling process is the key to reducing impurities. At present, the mainstream peeling methods are mainly divided into aerobic calcination, anaerobic calcination combined with crushing and cyclone separation, etc., which have high energy consumption, high cost, and difficulty in controlling impurities. Physical solvent peeling has low cost, short process, and fewer impurities, especially for reducing aluminum impurity content, which is of great significance for in-depth research and engineering scale-up consideration.

[0006] (2) The scrapped positive electrode sheet is mainly composed of positive electrode material and aluminum foil, and the two have similar density and size. After solvent stripping, the positive electrode material and aluminum foil are mixed, which is difficult to separate in industry. There is little relevant research, and it is necessary to develop and customize equipment with high adaptability.

[0007] Therefore, this invention applies flotation to the separation of cathode materials and aluminum foil, adds a foaming agent to improve separation efficiency, takes into account separation effect, efficiency and cost, and designs supporting equipment suitable for industrial applications.

[0008] On one hand, the present invention provides an efficient method for peeling off the positive electrode material and aluminum foil of a waste lithium-ion battery, comprising the following steps:

[0009] Aeration stripping: Place the waste lithium-ion battery electrode material into the aeration flotation equipment, add a certain amount of stripping agent, open the aeration valve to start aeration, and achieve the separation of the positive electrode material from the aluminum foil in the electrode material. Then close the aeration valve.

[0010] Flotation separation: After adjusting the distance between the agitator and the isolation screen, start stirring, add foaming agent, stir for a certain period of time, and then start aeration. When the aluminum foil no longer floats up, lower the distance between the agitator and the isolation screen, continue stirring and aeration, collect the upper layer material as aluminum foil, and collect the lower layer material as positive electrode active material.

[0011] The aeration flotation equipment includes an air flotation reactor, a stirring paddle, an aeration disc, and a separation net. The separation net is placed on the aeration disc and together with it is placed at the bottom of the air flotation reactor. The stirring paddle is placed inside the air flotation reactor, and the distance between the stirring paddle and the separation net is adjustable.

[0012] In specific embodiments of this application, the aeration stripping step further has at least one of the following technical features:

[0013] (1) The preparation process of the waste lithium-ion battery electrode material includes: discharging and dismantling the waste lithium-ion battery to obtain positive electrode material, and then cutting the positive electrode material into square size;

[0014] Preferably, the side length of the square electrode material is 3-10 cm;

[0015] (2) The amount of stripping agent added is such that the solid content of the slurry is 1-5%;

[0016] Preferably, the solid content is 2-4%;

[0017] (3) The temperature of the stripping agent is 40-90℃;

[0018] Preferably, the temperature of the stripping agent is 50-70°C;

[0019] (4) The aeration gas flow rate of the aeration flotation equipment is 20-50 L / min;

[0020] (5) The mesh size of the isolation screen in the aeration flotation equipment is square;

[0021] Preferably, the side length of the square is 0.4-1 cm;

[0022] (6) The positive electrode material in the electrode material is one of lithium iron phosphate, ternary materials, and lithium cobalt oxide;

[0023] (7) The state of the electrode is one of the following: unfilled electrode, filled electrode, or cycle-failed electrode.

[0024] In this application, the positive electrode sheet material is cut into squares to control variables; square cutting makes it easier to control dimensions and eliminates interference from differences in buoyancy caused by irregular shapes. However, in actual production, the shape of the positive electrode sheet material can be arbitrary and does not need to be square.

[0025] Similarly, in this application, the mesh size of the isolation screen in the aeration flotation device can be any shape and does not need to be square.

[0026] In specific embodiments of this application, the stripping agent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, water, and oxalic acid.

[0027] Preferably, the stripping agent contains water; more preferably, the stripping agent is water.

[0028] In a specific embodiment of this application, during the flotation separation step, the initial distance between the stirring paddle and the isolation screen is 3-6 cm, and the rotational speed of the stirring paddle is 10-100 r / min.

[0029] In a specific embodiment of this application, when the aluminum foil no longer floats out, the distance between the agitator and the isolation net is reduced to 0.5-2.5cm, while the rotation speed of the agitator is 10-100r / min and the aeration air flow rate is 10-40L / min.

[0030] In this application, the agitator can be paused, speed adjusted, and raised / lowered. Pausing and speed adjustment improve the aluminum foil flotation rate, while the raising / lowering function ensures that the agitator is adjusted to the middle in the early stage of flotation, reducing disturbance to the bottom and improving the aluminum flotation rate. In the later stage of flotation, the agitator is lowered in conjunction with the isolation screen to break up the positive electrode material with the water flow, thereby improving the positive electrode material yield.

[0031] In a specific embodiment of this application, the foaming agent is one or more of sodium dodecanebenzenesulfonate and sodium dodecanesulfonate.

[0032] In a specific embodiment of this application, the amount of foaming agent added is 0.002-0.02% of the mass of the stripping agent, preferably 0.005-0.01%.

[0033] In a specific embodiment of this application, during the flotation separation step, a stripping agent needs to be added during the aeration process, and the amount of stripping agent added is 0.5-2 L / min.

[0034] In a specific embodiment of this application, the collected positive electrode active material is dried in an inert atmosphere, then pulverized, and then the pulverized material is calcined in an inert atmosphere to obtain positive electrode material repair material.

[0035] Preferably, the drying temperature is 80-120℃ and the drying time is 2-8 hours;

[0036] Preferably, the material is pulverized to 200-800 mesh;

[0037] Preferably, the calcination temperature is 500-800℃ and the time is 2-20h.

[0038] In a specific embodiment of this application, the aeration disc is made by using nanoporous aeration pipes and attaching them to a fixed frame with a fixing buckle. The aeration disc is placed on a support platform, which supports the aeration disc fixing frame. The aeration disc is detachable and replaceable. The aeration pipes are connected to the right aeration inlet and the left aeration inlet to achieve aeration.

[0039] In a specific embodiment of this application, the stirring paddle is a cross-shaped stirring paddle with a scraping brush attached to its edge; preferably, the stirring paddle is equipped with a scraping brush made of polytetrafluoroethylene material. The scraping function solves the problem of aluminum foil sticking to the wall, thus improving the aluminum foil's floating rate.

[0040] In this application, by placing an isolation net on the aeration disc, the positive electrode material is broken down and falls under the net by the shearing action of the water flow generated by the stirring paddle and the bottom isolation net, and is discharged from the bottom outlet of the reactor, thus realizing the collection of the positive electrode material.

[0041] In a specific embodiment of this application, the aerated flotation equipment further includes a motor, a scraper, and an overflow trough. The overflow trough is positioned above the flotation reactor and has an overflow outlet. Aluminum foil, along with the foam generated during flotation, passes through the overflow trough and exits from the overflow outlet. The scraper is positioned above the overflow trough and can rotate to prevent foam from overflowing the equipment. The motor is connected to the agitator via an agitator rod, providing power to the agitator.

[0042] The aeration flotation equipment further includes a reactor bottom cover, which is located below the flotation reactor for discharging the lower layer of material. The reactor bottom cover is connected to the flotation reactor via a bottom cover opening and closing cylinder, and the opening and closing of the reactor bottom cover and the flotation reactor is achieved by extending and retracting the bottom cover opening and closing cylinder. The reactor bottom cover has a bottom discharge port, which further reduces aluminum impurities. An anti-clogging air jet is provided near the bottom discharge port, which intermittently sprays high-pressure gas to prevent bottom clogging.

[0043] The aeration flotation equipment further includes a steam heating jacket for introducing steam to heat the vessel body. The steam heating jacket has a jacket steam heating inlet and a jacket steam heating outlet, with the jacket steam heating inlet located at the lower part of the steam heating jacket and the jacket steam heating outlet located at the upper part of the steam heating jacket.

[0044] On the other hand, this application provides an aeration flotation device for efficiently separating waste lithium-ion battery cathode materials and aluminum foil. The device includes an air flotation reactor, an agitator, an aeration plate, and a separator. The separator is placed on the aeration plate and together with it at the bottom of the air flotation reactor. The agitator is placed inside the air flotation reactor, and the distance between the agitator and the separator is adjustable.

[0045] The device has the technical features described above, which will not be repeated here.

[0046] Beneficial effects:

[0047] (1) This invention optimizes the industrial scale-up of the stripping process for recycling waste lithium-ion battery materials, and designs a highly adaptable flotation separation device for aluminum foil, which greatly reduces the aluminum impurity content of the recycled repair material.

[0048] (2) After the positive electrode material and aluminum foil are separated, the aluminum foil is separated by flotation. The aluminum foil separation rate is about 95%, but a small amount of aluminum foil remains. In order to further reduce the impurities of the positive electrode material product, and considering that the positive electrode material is more fragile than the aluminum foil, this invention improves the flotation equipment. It uses nanoporous aeration pipes and uses a fixing buckle to tie them to a fixed frame to make an aeration plate. The aeration pipes are connected to the right aeration inlet and the left aeration inlet to realize aeration. An isolation net is placed on the aeration plate. The water flow generated by the stirring paddle and the shearing action of the bottom isolation net break the positive electrode material into the net and discharge it from the bottom outlet of the reactor to realize the collection of the positive electrode material and further reduce aluminum impurities. At the same time, an anti-blocking jet nozzle is set to intermittently spray high-pressure gas to prevent bottom blockage.

[0049] (3) Aluminum foil is thin and light, and tends to stick to the wall under stirring, resulting in poor flotation. This invention uses a cross-shaped stirring paddle with a wall scraper. The edge of the stirring paddle is equipped with a soft brush made of polytetrafluoroethylene material to scrape the wall, which solves the problem of aluminum foil sticking to the wall and improves the flotation rate of aluminum foil. The aluminum foil is discharged from the overflow tank outlet through the overflow tank along with the foam generated by flotation. The rotating scraper can prevent foam from overflowing the equipment.

[0050] (4) During the flotation process of the present invention, the stirring paddle can realize pause, speed adjustment and lifting functions. Pause and speed adjustment improve the aluminum foil floatation rate. The upgrading function ensures that the stirring paddle is adjusted to the middle in the early stage of flotation, reducing the disturbance to the bottom and improving the aluminum floatation rate. In the later stage of flotation, the stirring paddle is lowered in conjunction with the isolation net to break the positive electrode material with water flow and improve the positive electrode material yield. Attached Figure Description

[0051] Figure 1 This is a schematic diagram of the structure of an aeration flotation device provided by the present invention;

[0052] Figure 2 This is a schematic diagram of the structure of an aeration net provided by the present invention;

[0053] For ease of illustration, only a portion of the isolation net 5 is shown, but in actual applications, the isolation net 5 is the same size as the aeration disc 6.

[0054] Figure 3 This is a schematic diagram of the structure of a stirring paddle provided by the present invention;

[0055] Figure 4 This is a schematic diagram of a device provided by the present invention for efficiently peeling off the positive electrode material and aluminum foil of a waste lithium-ion battery;

[0056] Figure 5 This is a process flow diagram of an efficient method for peeling off waste lithium-ion battery cathode material and aluminum foil provided by the present invention.

[0057] Among them, 1-variable frequency motor, 2-scraper, 3-overflow trough, 4-stirring paddle, 5-isolation net, 6-aeration disc, 61-aeration pipe, 7-aeration pipe fixing bracket, 8-support platform, 9-bottom cover switch cylinder, 10-air flotation reactor, 11-reactor bottom cover, 12-steam heating jacket, 41-stirring paddle scraping brush, 71-aeration pipe fixing buckle, N1-overflow trough outlet, N2-bottom outlet of reactor, N3-jacket steam heating outlet, N4-jacket steam heating inlet, N5-anti-clogging material jet nozzle, N6-left aeration inlet, N7-right aeration inlet. Detailed Implementation

[0058] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0059] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0060] In the description of this invention, it should be noted that the terms "upper," "lower," "inner," "outer," "front end," "rear end," "both ends," "one end," and "the other end," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0061] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installed," "equipped with," "connected," etc., should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be a connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0062] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0063] This invention provides an aeration flotation device, such as... Figure 1 As shown, the aeration flotation equipment is used to efficiently separate waste lithium-ion battery cathode materials and aluminum foil. It includes an air flotation reactor 10, a stirring paddle 4, an aeration plate 6, and a separation net 5. The separation net 5 is set on the aeration plate 6 and together they are set at the bottom of the air flotation reactor 10. The stirring paddle 4 is set inside the air flotation reactor 10, and the distance between the stirring paddle 4 and the separation net 5 can be adjusted.

[0064] like Figure 2 As shown, the aeration disc 6 is made by using nanoporous aeration tubes 61, which are fixed to the aeration tube fixing frame 7 with aeration tube fixing buckles 71, and placed on a support platform 8. The support platform 8 is used to support the aeration disc fixing frame 7, and the aeration disc 6 is detachable and replaceable. The aeration tubes 61 are connected to the right aeration inlet N7 and the left aeration inlet N6 to achieve aeration. The mesh of the isolation net 5 is square; preferably, the side length of the square is 0.4-1cm.

[0065] like Figure 3 As shown, the stirring paddle 4 is a cross-shaped stirring paddle with a scraper, and the edge of the stirring paddle is equipped with a scraper brush 41; preferably, the stirring paddle is equipped with a scraper brush made of polytetrafluoroethylene material.

[0066] The aeration flotation equipment further includes a motor 1, a scraper 2, and an overflow trough 3. The overflow trough 3 is positioned above the flotation reactor 10 and has an overflow outlet N1. Aluminum foil, along with the foam generated during flotation, is discharged from the overflow outlet N1 through the overflow trough 3. The scraper 2 is positioned above the overflow trough 3 and can rotate to prevent foam from overflowing the equipment. The motor 1 is connected to the agitator 4 via an agitator rod, providing power to the agitator.

[0067] The aeration flotation equipment further includes a reactor bottom cover 11, which is located below the flotation reactor and is used for discharging the lower layer of material. The reactor bottom cover 11 is connected to the flotation reactor 10 via a bottom cover switching cylinder 9, and the opening and closing of the reactor bottom cover 11 and the flotation reactor 10 is achieved by extending and retracting the bottom cover switching cylinder 9. The reactor bottom cover 11 has a bottom discharge port N2 and an anti-clogging air jet port N5, with the anti-clogging air jet port N5 located near the bottom discharge port N2.

[0068] The aeration flotation equipment further includes a steam heating jacket 12 for introducing steam to heat the vessel body. The steam heating jacket 12 has a jacket steam heating inlet N4 and a jacket steam heating outlet N3. The jacket steam heating inlet N4 is located at the lower part of the steam heating jacket 12, and the jacket steam heating outlet N3 is located at the upper part of the steam heating jacket 12.

[0069] On the other hand, the present invention provides a highly efficient method for separating waste lithium-ion battery cathode material and aluminum foil, utilizing the aforementioned aeration flotation equipment, such as... Figure 4 and Figure 5 As shown, it includes the following steps:

[0070] (1) After discharging and dismantling the waste lithium-ion battery, the positive electrode material is obtained. The positive electrode material is then cut into square pieces. Preferably, the side length of the square electrode material is 3-10cm, thus obtaining waste lithium-ion battery electrode material.

[0071] (2) Aeration and stripping: The waste lithium-ion battery electrode material is placed in the aeration flotation equipment, and a certain amount of stripping agent is added according to the solid content of 1-5%. Preferably, the stripping agent is pure water with a temperature of 40-90℃. Then, the aeration valve is opened to start aeration. Compressed air enters from the right aeration inlet N7 and the left aeration inlet N6 to achieve aeration. The aeration air flow rate is controlled at 20-50L / min, and aeration is carried out for 10-20min to achieve the stripping of the positive electrode material from the aluminum foil in the electrode material. Then, the aeration valve is closed.

[0072] (3) Flotation separation: Adjust the initial distance between the agitator and the isolation screen to 3-6cm, and set the agitator speed to 10-100r / min. Start stirring and add frother (dosage). After stirring for 1-10min, start aeration with an aeration flow rate of 10-40L / min. Add water during aeration, with a water addition rate of 0.5-2L / min. When the aluminum foil no longer floats, reduce the distance between the agitator and the isolation screen to 0.5-2.5cm, and continue stirring and aeration. After 10-40min, collect the upper layer material as aluminum foil, which is discharged from the overflow outlet N1 and enters the aluminum foil receiving tank. Collect the lower layer material as positive electrode active material, which is discharged from the bottom outlet N2 and filtered through a filter press to obtain the active material black material. The solvent filtered out is replenished with frother through the feeding tank and recycled back to the air flotation reactor via the circulation system.

[0073] (4) The collected positive electrode active material is dried in an inert atmosphere at 80-120℃ for 2-8 hours, then pulverized to 200-800 mesh, and then calcined in an inert atmosphere at 500-800℃ for 2-20 hours to obtain positive electrode material repair material.

[0074] The present invention will be further described in detail below through specific embodiments.

[0075] Examples 1-3

[0076] This embodiment provides an efficient method for peeling off the positive electrode material and aluminum foil from waste lithium-ion batteries, including the following steps:

[0077] (1) The positive electrode material is obtained by pre-processing the waste lithium-ion battery through discharge and dismantling.

[0078] (2) Aeration and stripping: Prepare 400g of electrode material, with electrode size 5*5cm. 2 The mesh sizes of the isolation mesh are 0.4*0.4 / 0.6*0.6 / 0.9*0.9cm. 2 Add pure water with a solid content of 2% and place it in a 20L air flotation reactor. Set the temperature to 60℃, the aeration flow rate to 40L / min, and the aeration time to 20min.

[0079] (3) Flotation separation: Adjust the height of the agitator from the isolation screen to 4cm, start the agitator, and set the speed to 100r / min. Add sodium dodecylbenzenesulfonate as a foaming agent, with a dosage of 0.008% of the total mass of the slurry. After stirring for 5min, start aeration with an aeration flow rate of 27L / min. Add 1L / min of water (including foaming agent) per minute. After aeration for 10min, adjust the height of the agitator from the isolation screen to 1cm, and set the stirring speed to 100r / min. After stirring for 20min, stop stirring and aeration, and collect the upper and lower layers of material respectively.

[0080] (4) The lower layer of positive electrode active material is placed in a nitrogen atmosphere for drying, and then pulverized. The pulverized black material is placed in a nitrogen atmosphere furnace for calcination (650℃, 3h) to obtain the positive electrode material repair material.

[0081] Examples 4-7

[0082] This embodiment provides an efficient method for peeling off the positive electrode material and aluminum foil from waste lithium-ion batteries, including the following steps:

[0083] (1) The positive electrode material is obtained by pre-processing the waste lithium-ion battery through discharge and dismantling.

[0084] (2) Aeration and stripping: Prepare 400g of electrode material, with electrode sizes of 3*3 / 5*5 / 7*7 / 10*10cm respectively. 2 The mesh size of the isolation net is 0.6*0.6cm. 2 Add pure water with a solid content of 2% and place it in a 20L air flotation reactor. Set the temperature to 60℃, the aeration flow rate to 40L / min, and the aeration time to 20min.

[0085] (3) Flotation separation: Adjust the height of the agitator from the isolation screen to 4cm, start the agitator, and set the speed to 100r / min. Add sodium dodecylbenzenesulfonate as a foaming agent, with a dosage of 0.008% of the total mass of the slurry. After stirring for 5min, start aeration with an aeration flow rate of 27L / min. Add 1L / min of water (including foaming agent) per minute. After aeration for 10min, adjust the height of the agitator from the isolation screen to 1cm, and set the stirring speed to 100r / min. After stirring for 20min, stop stirring and aeration, and collect the upper and lower layers of material respectively.

[0086] (4) The lower layer of positive electrode material is placed in a nitrogen atmosphere for drying, and then crushed. The crushed black material is placed in a nitrogen atmosphere furnace for calcination (650℃, 3h) to obtain the positive electrode material repair material.

[0087] Examples 8-10

[0088] This embodiment provides an efficient method for peeling off the positive electrode material and aluminum foil from waste lithium-ion batteries, including the following steps:

[0089] (1) The positive electrode material is obtained by pre-processing the waste lithium-ion battery through discharge and dismantling.

[0090] (2) Aeration and stripping: Prepare 400g of electrode material, with electrode size 7*7cm. 2 The mesh size of the isolation net is 0.6*0.6cm. 2 Add pure water with a solid content of 2% and place it in a 20L air flotation reactor. Set the temperature to 60℃, the aeration flow rate to 40L / min, and the aeration time to 20min.

[0091] (3) Flotation separation: Adjust the height of the agitator from the isolation screen to 4cm, start the agitator, and set the speed to 100r / min. Add sodium dodecylbenzenesulfonate as a foaming agent, with a dosage of 0.008% of the total mass of the slurry. After stirring for 5min, start aeration with an aeration flow rate of 27L / min. Add water (including foaming agent) at 1L / min per minute. After aeration for 10min, adjust the height of the agitator from the isolation screen to 2 / 1 / 0cm respectively, and set the stirring speed to 100r / min. After stirring for 20min, stop stirring and aeration, and collect the upper and lower layers of material respectively.

[0092] (4) The lower layer of positive electrode material is placed in a nitrogen atmosphere for drying, and then crushed. The crushed black material is placed in a nitrogen atmosphere furnace for calcination (650℃, 3h) to obtain the positive electrode material repair material.

[0093] Examples 11-13

[0094] This embodiment provides an efficient method for peeling off the positive electrode material and aluminum foil from waste lithium-ion batteries, including the following steps:

[0095] (1) The positive electrode material is obtained by pre-processing the waste lithium-ion battery through discharge and dismantling.

[0096] (2) Aeration and stripping: Prepare 400 / 600 / 800g of electrode material respectively, with electrode size 7*7cm. 2 The mesh size of the isolation net is 0.6*0.6cm. 2 Pure water was added at solid contents of 2%, 3%, and 4% respectively, and placed in a 20L air flotation reactor. The temperature was set at 60℃, the aeration flow rate was 40L / min, and the aeration time was 20min.

[0097] (3) Flotation separation: Adjust the height of the agitator from the isolation screen to 4cm, start the agitator, and set the speed to 100r / min. Add sodium dodecylbenzenesulfonate as a foaming agent, with a dosage of 0.008% of the total mass of the slurry. After stirring for 5min, start aeration with an aeration flow rate of 27L / min and add 1L / min of water (including foaming agent) per minute. After aeration for 10min, adjust the height of the agitator from the isolation screen to 1cm, and set the stirring speed to 100r / min. After stirring for 20min, stop stirring and aeration, and collect the upper and lower layers of material respectively.

[0098] (4) The lower layer of positive electrode material is placed in a nitrogen atmosphere for drying, and then crushed. The crushed black material is placed in a nitrogen atmosphere furnace for calcination (650℃, 3h) to obtain the positive electrode material repair material.

[0099] Comparative Example 1

[0100] The difference from Example 1 is that the aeration flotation device does not include a separation net, while the rest of the equipment structure and experimental steps are the same as in Example 1.

[0101] Comparative Example 2

[0102] The difference from Example 1 is that the stirring paddle does not include a wall-scraping soft brush, but the rest of the equipment structure and experimental steps are the same as in Example 1.

[0103] The black material products obtained in the above embodiments and comparative examples were tested to determine the aluminum content, aluminum yield, and black material yield. The results are shown in Table 1.

[0104] Table 1

[0105]

[0106]

[0107] As shown in Table 1, the product obtained in Example 12 had the best aluminum yield, black material yield, and aluminum content in the black material. In Comparative Example 1, the absence of a separating mesh caused aluminum foil to easily leak during flotation, resulting in a high aluminum content in the black material. In Comparative Example 2, the absence of a wall-scraping brush caused some electrode material and aluminum foil to easily adhere to the wall during stirring, making proper separation and collection impossible.

[0108] The specific embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0109] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0110] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A highly efficient method for peeling off the positive electrode material and aluminum foil from waste lithium-ion batteries, characterized in that, Includes the following steps: Aeration stripping: The waste lithium-ion battery electrode material is placed into the aeration flotation equipment, a certain amount of stripping agent is added, the aeration valve is opened to start aeration, so as to separate the positive electrode material from the aluminum foil in the electrode material, and then the aeration valve is closed; wherein the stripping agent is water; Flotation separation: After adjusting the distance between the agitator and the isolation screen to 3-6 cm, start stirring, add foaming agent, stir for a certain period of time, and then start aeration. When the aluminum foil no longer floats up, reduce the distance between the agitator and the isolation screen to 0.5-2.5 cm, continue stirring and aeration, collect the upper layer material as aluminum foil, and collect the lower layer material as positive electrode active material. The aeration flotation equipment includes an air flotation reactor, a stirring paddle, an aeration disc, and an isolation net. The isolation net is placed on the aeration disc and together with it is placed at the bottom of the air flotation reactor. The stirring paddle is placed inside the air flotation reactor, and the distance between the stirring paddle and the isolation net is adjustable. The mesh of the isolation screen in the aeration flotation device is square, and the side length of the square is 0.4-1 cm.

2. The method according to claim 1, characterized in that, The preparation process of the waste lithium-ion battery electrode material includes: discharging and dismantling the waste lithium-ion battery to obtain positive electrode material, and then cutting the positive electrode material into square sizes; The side length of the square electrode material is 3-10 cm.

3. The method according to claim 1, characterized in that, The amount of stripping agent added is such that the solid content of the slurry is 1-5%; The temperature of the stripping agent is 40-90℃.

4. The method according to claim 1, characterized in that, In the aeration stripping step, the aeration air flow rate of the aeration flotation equipment is 20-50 L / min.

5. The method according to claim 1, characterized in that, In the flotation separation step, the rotation speed of the agitator is 10-100 r / min.

6. The method according to claim 1, characterized in that, Once the aluminum foil stops floating, the stirring paddle speed is 10-100 r / min and the aeration gas flow rate is 10-40 L / min.

7. The method according to claim 1, characterized in that, The foaming agent is one or more of sodium dodecanebenzenesulfonate and sodium dodecanesulfonate; The amount of foaming agent added is 0.002-0.02% of the mass of the stripping agent.

Citation Information

Patent Citations

  • Reaction kettle for stripping battery pole piece

    CN218215435U

  • Method for rapidly stripping waste lithium iron phosphate positive electrode material from aluminum foil and application

    CN115295912A

  • Recycling method of pole piece

    CN118341791A

  • Separation and recovery device and method for positive and negative electrode materials of waste lithium battery

    CN118888895A

  • Solar cell module recycling method

    JP2014104406A