Preparation method of alumina porous ceramic for electrostatic chuck

The slurry composition and lyophilization process of alumina porous ceramics are adjusted through freeze-drying, which solves the problem of difficult to accurately control pore size and porosity in the prior art, and realizes mass production of high-performance alumina porous ceramics, meets the high-performance requirements in the semiconductor field, and reduces production costs and environmental impacts.

CN119841662AActive Publication Date: 2025-04-18HUBEI XINTAO TECHNOLOGY CO LTD

Patent Information

Application Number
CN202510011547.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-04
Publication Date
2025-04-18
Estimated Expiration
2045-01-04

AI Technical Summary

Technical Problem

The existing methods for preparing porous alumina porous ceramics have difficulties in precisely controlling the pore size and porosity, resulting in unstable material performance and it is difficult to prepare porous ceramics with highly uniform porous structures. The preparation process is complex, the cost is high, and the environmental friendliness is poor.

Method used

The freeze-drying method is used to prepare alumina porous ceramics. By adjusting the slurry composition and optimizing the lyophilization process, the pore structure is accurately regulated, and the mass production of semiconductor-grade alumina porous ceramics is realized.

Benefits of technology

The production of alumina porous ceramics with uniform porosity, adjustable pore size, small density and high mechanical strength is achieved, which meets the high performance requirements of the semiconductor field, reduces production costs and improves environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005228515070000101
    Figure BDA0005228515070000101
  • Figure HDA0005228515080000011
    Figure HDA0005228515080000011
Patent Text Reader

Abstract

The invention relates to a preparation method of alumina porous ceramic for an electrostatic chuck, which successfully obtains porous ceramic with uniform pore structure, adjustable porosity and aperture, small density and high strength by optimizing technological parameters such as freeze drying and taking ice crystals generated by water as a template. Aluminum oxide powder, a plasticizer, a dispersing agent, a binder, a defoaming agent, a thickening agent and the like are adopted as main raw materials, the formula of the slurry is adjusted, and the flowability, formability and stability of the slurry are improved. In addition, by doping the sintering aid, the porous ceramic also has good dielectric strength and compressive strength. The method not only can provide excellent thermal management performance, but also is simple in process, wide in raw material source, low in cost and environment-friendly, and provides a high-performance porous ceramic material with potential application potential for electrostatic chucks and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing a porous ceramic material, and in particular to a freeze-drying method for preparing alumina porous ceramics for electrostatic chucks in the semiconductor field. Specifically, the technical field of the present invention includes but is not limited to a method for preparing alumina porous ceramics for applications such as thermal management materials, electrostatic chucks, heat exchangers, and gas distributors in semiconductor manufacturing processes and related products. Background Art

[0002] Alumina porous ceramics are a type of material containing a large number of pores. Due to their unique physical and chemical properties, such as high porosity, low density, high strength, good chemical stability and thermal stability, they play a vital role in various fields. At present, the application background of porous ceramics is mainly reflected in the following aspects: (1) Environmental purification: In water treatment, gas purification and exhaust gas treatment, porous ceramics are used as filtering and adsorption materials to effectively remove impurities and pollutants. (2) Energy catalysis: In fuel cells, catalyst carriers and heat exchangers, porous ceramics with high specific surface area provide a larger active area and thermal conductivity. (3) Biomedicine: Porous ceramics are used to manufacture biological implants such as artificial bones and teeth. Because of their non-toxicity, good biocompatibility and ability to promote tissue growth. (4) Semiconductor field: Porous ceramics are important equipment and key components in semiconductor manufacturing. They can be used for filtering, dispersing and fixing in semiconductor equipment, as well as airflow control for thermal management in wafer processing, thereby improving the yield of silicon wafer processing.

[0003] Alumina porous ceramics have been gradually applied in more high-tech fields in recent years due to their special material properties. In particular, in the wafer processing process, the porous ceramics on the electrostatic chuck can provide good thermal management for the wafer and ensure its processing accuracy. The existing methods for preparing porous alumina ceramics mainly include foaming method, adding pore-forming agent method, organic foam impregnation method, sol-gel method, etc. Although these methods have their own advantages in the preparation of porous ceramics, they also have certain limitations: for example, there are difficulties in accurately controlling the pore size and porosity, resulting in unstable performance of the obtained materials, and it is difficult to prepare porous ceramics with highly uniform pore structure, which limits its application in some high-performance requirements. Some methods such as sol-gel method have long production cycle, low efficiency, and are not suitable for large-scale production. The preparation method requires expensive raw materials or special equipment, resulting in high cost. The foaming method and pore-forming agent method require the use of toxic and harmful foaming agents and chemical templates, which are environmentally unfriendly.

[0004] Freeze-drying, as a method for preparing high-porosity porous ceramics, has the following advantages: it can accurately design the shape, size and distribution of pores by controlling the formation and sublimation process of ice crystals, and can prepare porous ceramics with high porosity and highly uniform pore structure. It can prepare different types of pore structures, such as connected pores, closed pores, etc., to meet the needs of different applications. Water is used as a pore-forming agent, and the entire process does not involve the use of harmful chemicals, which meets environmental protection requirements.

[0005] However, there are still many problems in the preparation of porous ceramics using freeze-drying. For example, the process is complicated, special molds are required, and sodium hexametaphosphate is added to obtain a layered structure. However, the introduced sodium ions have a significant effect on the dielectric strength of porous ceramics, limiting their application in the semiconductor field.

[0006] There is an urgent need to propose a simple process that can adjust the slurry composition and optimize the simple freeze-drying process to precisely control the pores of porous ceramics without introducing other metal ions, thereby achieving mass production of semiconductor-grade alumina porous ceramics. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a method for preparing alumina porous ceramics for electrostatic chucks, comprising the following steps:

[0008] S1: preparing slurry: 100 parts by mass of alumina powder, 10 parts by mass of plasticizer, 10 parts by mass of dispersant, 8 parts by mass of binder, 5 parts by mass of defoaming agent, 3 parts by mass of thickener, and 100 parts by mass of water are mixed, and ball milled to obtain a premixed slurry. Then, 100 parts by mass of the premixed slurry is taken out, 6 parts by mass of sintering aid is added, and the premixed slurry is mixed using a ball mill. The ball milled slurry is filtered out and degassed to obtain a slurry with good rheological properties.

[0009] S2 molding and drying: pouring the slurry obtained in S1 into a mold, placing it in a freeze dryer for freeze drying, the freeze drying process includes a freezing stage and a sublimation stage, and then demolding to obtain a green body;

[0010] S3 debinding: in a debinding furnace, the green embryo obtained in S2 is heated from room temperature to 100-300°C at a certain heating rate r1 and kept at this temperature for a period of time t1, and then heated to 400-600°C at a certain heating rate r2 and kept at this temperature for a period of time t2;

[0011] S4 sintering: the green body in S3 is heated to 1400-1800°C, kept at this temperature for a certain period of time, and then naturally cooled to room temperature to finally obtain alumina porous ceramics;

[0012] Furthermore, the freezing stage is at normal pressure, the temperature is lowered from room temperature, the set temperature is -100 to -1°C, the insulation time is 1 to 50 hours, and the average cooling rate is 1 to 10°C / h;

[0013] The preferred average cooling rate is 1 to 6°C / h;

[0014] Furthermore, the pressure in the sublimation stage is 0.001 bar, the set temperature is -50 to -20°C, the insulation time is 5 to 36 hours, and the average heating rate is 1 to 20°C / h;

[0015] Preferably, the average heating rate is 1 to 10°C / h;

[0016] Furthermore, the heating rate r1 of the debinding step is 1 to 8°C / min;

[0017] Preferably, the r1 is 1 to 5°C / min;

[0018] The insulation time t1 is 1 to 6 hours;

[0019] Preferably, the t1 is 1 to 3 hours;

[0020] The heating rate r2 is 1 to 15°C / min;

[0021] Preferably, the r2 is 1 to 10°C / min;

[0022] The insulation time t2 is 1 to 10 hours;

[0023] Preferably, the t2 is 1 to 6 hours;

[0024] Furthermore, the heating rate of the sintering step is 1 to 20°C / min;

[0025] The preferred heating rate is 1 to 10°C / min;

[0026] The insulation time is 1 to 20 hours;

[0027] The preferred insulation time is 1 to 10 hours;

[0028] Furthermore, the alumina powder is high-purity alumina with a particle size d of 0.1 to 20 μm;

[0029] Preferably, the alumina powder has a particle size d of 1-10 μm;

[0030] Further, the plasticizer includes one or more combinations of glycerol, oleic acid, and dibutyl phthalate;

[0031] The preferred plasticizer is glycerol;

[0032] Further, the dispersant includes one or more combinations of ammonium polyacrylate copolymer, sodium polymethacrylate copolymer, and ammonium polymethacrylate copolymer;

[0033] The preferred dispersant is ammonium polyacrylate copolymer;

[0034] Further, the binder includes one or more combinations of polyvinyl alcohol, carboxymethyl cellulose, and hydroxyethyl cellulose;

[0035] Preferably, the binder is polyvinyl alcohol;

[0036] Further, the sintering aid includes one or more combinations of magnesium oxide, silicon oxide, and titanium oxide;

[0037] Preferably, the sintering aid is magnesium oxide.

[0038] Beneficial effects:

[0039] (1) Using ice crystals generated by water in alumina ceramic slurry as a template and adjusting the solid content of the formula and freeze-drying process parameters, alumina porous ceramics with uniform pore structure, adjustable porosity and pore size, low density and high mechanical strength can be prepared in batches.

[0040] (2) By adjusting the slurry formula, the fluidity, formability and stability of the slurry are improved, which is convenient for the next freeze-drying process. In addition, by doping sintering aids, the porous ceramics also have good dielectric strength and compressive strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 This is a microstructure photograph of the alumina porous ceramic prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0043] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] The present invention provides a method for preparing an alumina porous ceramic for an electrostatic chuck, comprising the following steps:

[0045] S1 Preparation of slurry

[0046] 100 parts by mass of alumina powder, 10 parts by mass of plasticizer, 10 parts by mass of dispersant, 8 parts by mass of binder, 5 parts by mass of defoaming agent, 3 parts by mass of thickener and 100 parts by mass of water are mixed and ball-milled to obtain a premixed slurry. Subsequently, 100 parts by mass of the premixed slurry are taken out, 6 parts by mass of sintering aid are added, and the mixture is mixed using a ball mill. The ball-milled slurry is filtered out and degassed to obtain a slurry with good rheological properties.

[0047] In step S1 of the present invention, the alumina powder is high-purity alumina with a particle size of 0.1 to 20 μm, and preferably the alumina powder has a particle size of 1 to 10 μm.

[0048] In the present invention, alumina powder with a particle size greater than 20 μm may lead to insufficient contact between particles, thereby affecting the densification and formation of pore structure during sintering. During the sintering process, large-particle powder is difficult to fully fuse at high temperature, resulting in a lower density and higher porosity of the ceramic, thereby affecting the mechanical properties of the ceramic, especially its compressive strength and hardness. In addition, large-particle powder may also lead to uneven pore distribution and produce larger holes, thereby affecting the surface smoothness and uniformity of the ceramic; alumina powder with a particle size less than 0.1 μm may lead to excessive contact and bonding between particles, and even in some cases, may form strong powder agglomeration. Powder agglomeration is often difficult to distribute evenly during the sintering process, resulting in an uneven ceramic structure formed during the sintering process, and may even cause cracks or microcracks, affecting the overall mechanical strength and reliability of the ceramic. In addition, too small particles will increase the surface area of ​​the powder, which may result in the inability to evenly remove moisture during freeze-drying, forming an uneven pore structure, further affecting the porosity and stability of the ceramic.

[0049] In the present invention, the plasticizer includes one or more combinations of glycerol, oleic acid, and dibutyl phthalate, and preferably the plasticizer is glycerol.

[0050] Plasticizers are usually used to improve the compatibility between alumina powder and binders, improve plasticity and fluidity during the molding process, and thus enhance the uniformity and stability of the molded body. Plasticizers reduce the friction between powder and binder, making it easier to mix and mold the raw materials during the molding process, avoiding molding difficulties or defects caused by tight or uneven bonding between particles. When glycerol is used as a plasticizer, the operability of the ceramic molded body can be significantly improved, and cracks and deformation problems during the molding process can be reduced. In addition, glycerol can also play a certain stabilizing role in the freeze-drying process, helping to control the evaporation of water at low temperatures and avoid the problem of uneven pore distribution.

[0051] In the present invention, the dispersant includes one or more combinations of ammonium polyacrylate copolymer, sodium polymethacrylate copolymer, and ammonium polymethacrylate copolymer. Preferably, the dispersant is ammonium polyacrylate copolymer.

[0052] The main function of the dispersant is to prevent the ceramic powder particles from agglomerating due to mutual attraction during the molding process, which leads to uneven particle distribution and affects the compactness and mechanical properties of the molded body. By improving the dispersibility of the powder, the dispersant can enhance the suspension of the powder in water, thereby ensuring a uniform molding mixture and avoiding cracks, uneven porosity or other defects during the subsequent freeze-drying or sintering process. Ammonium polyacrylate copolymer has good solubility in aqueous solution and can effectively avoid the occurrence of powder agglomeration, especially during freeze-drying and sintering processes, which can help ceramic materials obtain a more uniform pore structure and good mechanical properties.

[0053] In the present invention, the binder includes one or more combinations of polyvinyl alcohol, carboxymethyl cellulose, and hydroxyethyl cellulose, and preferably the binder is polyvinyl alcohol.

[0054] Binders are mainly used to improve the plasticity, fluidity and stability of ceramic powders during the molding process. It allows the particles to maintain a proper shape during the molding process, avoiding uneven molding due to excessive flow or aggregation of particles, which in turn affects the final pore structure and mechanical properties. In addition, binders can also improve the processing properties of ceramic slurries, so that during freeze drying or sintering, the powder can be evenly distributed, reducing the generation of cracks and uneven pores. Polyvinyl alcohol can dissolve in the aqueous phase to form a transparent viscous solution, ensuring that the powder is not easy to disperse and agglomerate during the molding process, helping to form a uniform slurry. In addition, polyvinyl alcohol is easily removed during the heat treatment process, will not have a negative impact on the sintering process of the ceramic, can completely disappear after sintering, and will not remain in the final ceramic product, thereby ensuring the purity and high performance of the ceramic material.

[0055] In the present invention, the sintering aid includes one or more combinations of magnesium oxide, silicon oxide, and titanium oxide. Preferably, the sintering aid is magnesium oxide.

[0056] Sintering aids can significantly improve the sintering performance, densification process and final mechanical properties of ceramics. Sintering aids can help ceramics complete sintering at a lower temperature by reducing the sintering temperature of alumina, promoting grain growth and improving pore structure, thereby improving the density and strength of the product and optimizing the overall performance of the ceramic. Magnesium oxide has a low melting point and can effectively reduce the sintering temperature of alumina during high-temperature sintering, shorten the sintering time, and improve the uniformity of grains during the sintering process.

[0057] S2 Forming and Drying

[0058] The slurry obtained in S1 is poured into a mold and placed in a freeze dryer for freeze drying. The freeze drying process includes a freezing stage and a sublimation stage. The green body is then demoulded to obtain the green body.

[0059] In the present invention, the freezing stage is at normal pressure, the temperature is lowered from room temperature, the set temperature is -100 to -1°C, the insulation time is 1 to 50 hours, the average cooling rate is 1 to 10°C / h, and the preferred average cooling rate is 1 to 6°C / h.

[0060] During the freezing stage, the freezing temperature is set to -100°C to -1°C. This temperature range ensures that the water in the sample forms uniform ice crystals before freezing without causing the ice crystals to be too large. Excessively large ice crystals will not only destroy the organizational structure of the sample, but may also affect the final quality of the product. A cooling rate of 1 to 10°C / h, preferably 1 to 6°C / h, is used. A moderate freezing temperature and cooling rate help control the size of ice crystals during the freezing process, making their distribution more uniform, thereby better controlling the pore uniformity and pore size of the porous ceramics, and obtaining alumina porous ceramics with low density and high mechanical strength. In addition, at a lower cooling rate, the growth rate of ice crystals is slower, and ice crystals can be precipitated evenly, thereby reducing the phenomenon of uneven freezing in the product. Too fast a freezing rate may cause incomplete local freezing of the sample, which may cause freezing on the surface of the sample, and there may be larger ice crystals inside, affecting the pore structure of the product and the effect of the subsequent sublimation stage.

[0061] In the present invention, the pressure in the sublimation stage is 0.001 bar, the set temperature is -50 to -20°C, the insulation time is 5 to 36 hours, the average heating rate is 1 to 20°C / h, and the preferred average heating rate is 1 to 10°C / h.

[0062] During the sublimation stage, the reduction of vacuum helps to accelerate the removal of moisture. Lower pressure can reduce the possibility of moisture forming liquid water during the sublimation process, which is very beneficial for maintaining the dryness and stability of the product. Compared with conventional drying methods, vacuum sublimation can better preserve the morphological structure of porous ceramics. Reasonable control of the sublimation rate not only helps to improve the efficiency of moisture removal, but also avoids sample damage caused by too fast heating. Too fast a heating rate may cause uneven sublimation of moisture inside the sample due to excessive pressure differences, and may even cause excessive temperature differences between the surface and the interior, resulting in too fast surface drying and the formation of a "hard shell", making it difficult for the internal moisture to sublimate smoothly, thus affecting the final product quality. A moderate heating rate can ensure uniform sublimation of the sample and reduce damage to the surface or interior of the product, especially for products that require high precision and high activity.

[0063] In the present invention, the solvent in the slurry is frozen into ice by freeze drying, and then the ice is removed from the ceramic green body by sublimation to leave pores. Different slurries have different components and solid contents, resulting in different eutectic points (temperatures at which the slurry just freezes), so freeze drying requires different freezing temperatures and sublimation temperatures to completely evaporate the solvent in the slurry and leave pores, otherwise it will not be completely dried.

[0064] S3 glue removal

[0065] In the debinding furnace, the green embryo obtained in S2 is heated from room temperature to 100-300°C at a certain heating rate r1 and kept at this temperature for a period of time t1, and then heated to 400-600°C at a certain heating rate r2 and kept at this temperature for a period of time t2.

[0066] In the present invention, the heating rate r1 of the debinding step is 1 to 8°C / min, preferably 1 to 5°C / min, and the insulation time t1 is 1 to 6h, preferably 1 to 3h.

[0067] In the present invention, by setting the heating rate r1 to the above range, thermal stress on the surface or inside of the embryo caused by too fast temperature changes can be effectively avoided, and the risk of embryo cracking can be reduced. A lower heating rate helps the moisture and solvent inside the embryo to evaporate slowly during the heating process, preventing the formation of cracks or deformation on the embryo surface due to too fast evaporation of water. If the temperature rises too fast, it may cause uneven formation of pores, thereby affecting the performance of porous ceramics. Through an appropriate holding time t1, it is ensured that the green embryo can fully remove volatile components, such as solvents or additives, when the temperature reaches 100 to 300 ° C, further ensuring the morphological stability of the embryo.

[0068] In the present invention, the heating rate r2 is 1 to 15°C / min, preferably the r2 is 1 to 10°C / min, the insulation time t2 is 1 to 10h, preferably the t2 is 1 to 6h.

[0069] In the present invention, by setting the heating rate r2 within the above range, it is helpful to uniformly cause physical changes between particles during the temperature rise in the debinding stage. A higher heating rate r2 can accelerate the temperature rise, shorten the heating time, and help improve production efficiency, while not causing excessive temperature differences and maintaining the uniformity of the entire green embryo. In addition, by setting the holding time within the above range, the bonding force of the alumina particles is improved within the temperature range of 400 to 600°C, forming a uniform porous ceramic structure.

[0070] S4 Sintering

[0071] The green body in S3 is heated to 1400-1800° C., kept at this temperature for a certain period of time, and then naturally cooled to room temperature to finally obtain alumina porous ceramics.

[0072] In the present invention, the heating rate of the sintering step is 1 to 20°C / min, preferably 1 to 10°C / min, and the holding time is 1 to 20h, preferably 1 to 10h. Heating too fast may cause excessive temperature differences in the ceramic body, resulting in uneven sintering behavior, and even defects such as cracks and warping. By setting the heating rate within the above range, local overheating or excessive temperature gradients can be avoided. By setting the holding time within the above range, the alumina particles can be fully fused and sintered under high temperature conditions, thereby improving the density and strength of the ceramic. Appropriate holding time can also ensure that organic matter and moisture are completely volatilized during the sintering process, avoiding residual volatile components from affecting the structure and properties of the ceramic. When the holding time is sufficient, the pore structure of the ceramic is uniform and stable, and the porosity and pore size distribution are effectively controlled.

[0073] The above and other advantages of the present invention may be better understood through the following examples, but the following examples are not intended to limit the scope of the present invention.

[0074] Example

[0075] The present invention is described below with reference to the following examples, but the present invention is not limited to the following examples.

[0076] Plasticizer (A)

[0077] A1: Glycerin

[0078] A2: Oleic acid

[0079] A3: Dibutyl phthalate

[0080] A4: Triethylene glycol acetate

[0081] Dispersant (B)

[0082] B1: Ammonium polyacrylate copolymer

[0083] B2: Sodium polymethacrylate copolymer

[0084] B3: Ammonium polymethacrylate copolymer

[0085] Binder (C)

[0086] C1: Polyvinyl alcohol

[0087] C2: Carboxymethyl cellulose

[0088] C3: Hydroxyethyl Cellulose

[0089] C4: Hydroxypropyl methylcellulose

[0090] Sintering aid (D)

[0091] D1: Magnesium oxide

[0092] D2: Silicon oxide

[0093] D3: Titanium oxide

[0094] D4: Yttrium Oxide

[0095] Example 1

[0096] This example uses freeze drying to prepare high-performance alumina porous ceramics: high-purity alumina powder is used as raw material, plasticizer, dispersant, binder, defoamer, thickener, sintering aid and deionized water are added, and the slurry is obtained by ball milling, and then through molding, freeze drying and sintering processes, alumina porous ceramic materials with a specific pore structure are obtained. The specific preparation steps are as follows:

[0097] S1: preparing slurry: 100 parts by mass of alumina powder with a particle size of 1 to 10 μm, 10 parts by mass of a plasticizer, 10 parts by mass of a dispersant, 8 parts by mass of a binder, 5 parts by mass of a polydimethylsiloxane defoaming agent, 3 parts by mass of a guar gum thickener, and 100 parts by mass of water are mixed, and ball milled at a stirring speed of 150 rpm for 4 hours to obtain a premixed slurry, then 100 parts by mass of the premixed slurry is taken out, 6 parts by mass of a sintering aid is added, and the mixture is mixed using a ball mill, and the ball-milled slurry is filtered out and degassed to obtain a slurry with good rheological properties;

[0098] S2 molding and drying: pour the slurry obtained in S1 into a mold and put it into a freeze dryer for freeze drying. The freeze drying process includes a freezing stage and a sublimation stage. The pressure in the freezing stage is normal pressure, and the temperature is lowered from room temperature. The set temperature is -80°C, the average cooling rate is 5°C / h, and the insulation time is 25h. The pressure in the sublimation stage is 0.001 bar, the set temperature is -30°C, the average heating rate is 8°C / h, and the insulation time is 36h. Then demolding is performed to obtain the green body;

[0099] S3 debinding: The green embryo obtained in S2 was heated from room temperature to 300°C in a debinding furnace at a heating rate of 5°C / min and kept at this temperature for 2 hours, and then heated to 450°C at a heating rate of 8°C / min and kept at this temperature for 5 hours.

[0100] S4 sintering: The green body in S3 is heated to 1500°C at a heating rate of 10°C / min, kept at this temperature for 10 hours, and then naturally cooled to room temperature to finally obtain alumina porous ceramics.

[0101] Examples 2 to 9 were carried out according to the above steps and the experimental conditions shown in Table 1.

[0102] Comparative Example 1

[0103] S1: preparing slurry: 100 parts by mass of alumina powder with a particle size of 1 to 10 μm, 10 parts by mass of a plasticizer, 10 parts by mass of a dispersant, 8 parts by mass of a binder, 5 parts by mass of a polydimethylsiloxane defoaming agent, 3 parts by mass of a guar gum thickener, and 100 parts by mass of water are mixed, and ball milled at a stirring speed of 150 rpm for 4 hours to obtain a premixed slurry, then 100 parts by mass of the premixed slurry is taken out, 6 parts by mass of a sintering aid is added, and the mixture is mixed using a ball mill, and the ball-milled slurry is filtered out and degassed to obtain a slurry with good rheological properties;

[0104] S2 molding and drying: pour the slurry obtained in S1 into a mold, put it into a freeze dryer for freeze drying, set the temperature to -30°C, the pressure to 0.001 bar, the average cooling rate to 2°C / h, the holding time to 48h, and then demold to obtain a green body;

[0105] S3 sintering: The green body in S2 is heated to 1500°C at a heating rate of 10°C / min, kept at this temperature for 20 hours, and then naturally cooled to room temperature to finally obtain alumina porous ceramics.

[0106] Comparative Examples 2 to 3 were carried out according to the above steps and the experimental conditions shown in Table 1.

[0107] Table 1 Experimental conditions of embodiments and comparative examples

[0108]

[0109] The porosity, compressive strength and dielectric strength of the alumina porous ceramics of the above examples and comparative examples are shown in Table 2 below:

[0110] Table 2 Properties of porous alumina ceramics prepared in Examples and Comparative Examples

[0111] Porosity (%) Compressive strength(MPa) Dielectric strength (kV / mm) Example 1 76.3 120.3 12.1 Example 2 73.6 120.0 11.6 Example 3 72.4 121.4 11.4 Example 4 63.1 125.8 8.5 Example 5 62.5 126.3 8.2 Example 6 65.4 123.7 9.4 Example 7 66.3 123.5 9.5 Example 8 68.3 122.0 10.7 Example 9 69.1 121.9 10.9 Comparative Example 1 50.1 127.6 6.8 Comparative Example 2 49.3 127.9 6.5 Comparative Example 3 48.6 128.3 6.0

[0112] As shown in Table 2, in Examples 1 to 9, the alumina porous ceramics prepared by freeze drying have high porosity, while ensuring good mechanical strength and high dielectric strength, and are suitable for use in semiconductor devices such as electrostatic chucks. In general, compared with the existing porous ceramic freeze drying preparation method, the alumina porous ceramics in the above examples show more excellent performance in porosity, mechanical strength, and dielectric properties, making them a promising candidate material for a variety of applications, especially in semiconductor devices and other fields requiring specific performance materials.

[0113] It should be noted that, according to the explanation and elaboration of the above description, those skilled in the art to which the present invention belongs may also make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some equivalent modifications and changes to the present invention should also be within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the invention.

Claims

1. A method for preparing alumina porous ceramics for electrostatic chucks, characterized in that: The following steps are involved: S1: preparing slurry: 100 parts by mass of alumina powder, 10 parts by mass of plasticizer, 10 parts by mass of dispersant, 8 parts by mass of binder, 5 parts by mass of defoaming agent, 3 parts by mass of thickener, and 100 parts by mass of water are mixed, and ball milled to obtain a premixed slurry. Then, 100 parts by mass of the premixed slurry is taken out, 6 parts by mass of sintering aid is added, and the premixed slurry is mixed using a ball mill. The ball milled slurry is filtered out and degassed to obtain a slurry with good rheological properties. S2 molding and drying: pouring the slurry obtained in S1 into a mold, placing it in a freeze dryer for freeze drying, the freeze drying process includes a freezing stage and a sublimation stage, and then demolding to obtain a green body; S3 debinding: in a debinding furnace, the green embryo obtained in S2 is heated from room temperature to 100-300°C at a certain heating rate r1 and kept at this temperature for a period of time t1, and then heated to 400-600°C at a certain heating rate r2 and kept at this temperature for a period of time t2; S4 sintering: The green body in S3 is heated to 1400-1800°C, kept at this temperature for a certain period of time, and then naturally cooled to room temperature to finally obtain alumina porous ceramics.

2. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The freezing stage is at normal pressure, and the temperature is lowered from room temperature, the set temperature is -100 to -1°C, the insulation time is 1 to 50 hours, the average cooling rate is 1 to 10°C / h, and the preferred average cooling rate is 1 to 6°C / h.

3. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The pressure in the sublimation stage is 0.001 bar, the set temperature is -50 to -20°C, the insulation time is 5 to 36 hours, the average heating rate is 1 to 20°C / h, and the preferred average heating rate is 1 to 10°C / h.

4. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The heating rate r1 of the debinding step is 1 to 8°C / min, preferably r1 is 1 to 5°C / min, the insulation time t1 is 1 to 6h, preferably t1 is 1 to 3h, the heating rate r2 is 1 to 15°C / min, preferably r2 is 1 to 10°C / min, the insulation time t2 is 1 to 10h, preferably t2 is 1 to 6h.

5. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The heating rate of the sintering step is 1 to 20° C. / min, preferably 1 to 10° C. / min, and the insulation time is 1 to 20 hours, preferably 1 to 10 hours.

6. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The alumina powder is high-purity alumina with a particle size d of 0.1 to 20 μm, and preferably the alumina powder has a particle size d of 1 to 10 μm.

7. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The plasticizer includes one or more combinations of glycerol, oleic acid, and dibutyl phthalate, and preferably the plasticizer is glycerol.

8. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The dispersant includes one or more combinations of ammonium polyacrylate copolymer, sodium polymethacrylate copolymer, and ammonium polymethacrylate copolymer. Preferably, the dispersant is ammonium polyacrylate copolymer.

9. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The binder includes one or more combinations of polyvinyl alcohol, carboxymethyl cellulose, and hydroxyethyl cellulose. Preferably, the binder is polyvinyl alcohol.

10. The method for preparing alumina porous ceramics for electrostatic chuck according to claim 1, characterized in that: The sintering aid includes one or more combinations of magnesium oxide, silicon oxide, and titanium oxide. Preferably, the sintering aid is magnesium oxide.

Citation Information

Patent Citations

  • Method for producing porous ceramic with oriented structure by employing freeze dehydration

    CN101429050A

  • Method for preparing aluminum oxide porous ceramic with composite structure by adopting freeze drying process

    CN102432327A

  • Orientated penetration porous ceramic for high temperature flue gas filtration and preparation method thereof

    CN104402411A

  • Porous material with central symmetry structure and method for preparing the same

    CN104945005A

  • Double-gradient porous ceramic material and preparation method thereof

    CN108083811A

Cited By

  • Alumina electrostatic chuck ceramic and integrated sintering method thereof

    CN120423860A

  • Alumina electrostatic chuck ceramic and its integrated sintering method

    CN120423860B

  • Alumina porous ceramic for electrostatic chuck and preparation method of alumina porous ceramic

    CN121135469A