A method for the conversion of biomass to 2,5-dimethylfuran

By using a tandem reaction of biomass feedstock with a solid acid catalyst and a hydrogenolysis catalyst, the problems of low catalytic efficiency and high cost in the preparation of 2,5-dimethylfuran have been solved, realizing an efficient and green method for converting biomass into 2,5-dimethylfuran. The products are easy to separate and the catalyst has good stability.

CN119859129BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311359263.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-19
Publication Date
2026-11-24
Estimated Expiration
2043-10-19

AI Technical Summary

Technical Problem

Existing technologies for the preparation of 2,5-dimethylfuran suffer from problems such as low catalytic efficiency, high cost, and environmental pollution, making it difficult to achieve large-scale application.

Method used

Biomass feedstock is reacted with a solid acid catalyst in the presence of various organic solvents to generate 5-hydroxymethylfurfural and its passivation products. Then, it is reacted with a hydrogenolysis catalyst to prepare 2,5-dimethylfuran. High-efficiency conversion is achieved in one step using SCM-36-SO₃H molecular sieve and Ni-SCM-X catalyst.

Benefits of technology

It achieves green and efficient conversion of biomass to 2,5-dimethylfuran, with high product selectivity, good catalyst stability, and easy product separation, thereby reducing production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119859129B_ABST
    Figure CN119859129B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing 2,5-dimethylfuran from biomass. The method includes: (1) reacting biomass feedstock with a solid acid catalyst in the presence of various organic solvents to obtain an organic solution containing 5-hydroxymethylfurfural and partially passivated 5-hydroxymethylfurfural functional groups; (2) reacting the organic solution obtained in step (1) with hydrogen gas and a hydrogenolysis catalyst to obtain 2,5-dimethylfuran. This method has the advantages of high product selectivity, good catalyst stability, and easy product separation, achieving a green and efficient conversion of biomass to 2,5-dimethylfuran.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic chemistry, specifically relating to a method for preparing 2,5-dimethylfuran from biomass conversion. Background Technology

[0002] With the advancement of science and technology and the development of society, human demand for traditional fossil energy sources such as coal, oil, and natural gas is increasing, leading to the depletion of fossil energy reserves on Earth. Furthermore, the combustion of fossil energy causes severe environmental pollution. Conversely, biomass, as a green and renewable energy source, is abundant on Earth, and its conversion and utilization process does not pollute the environment. Therefore, many scholars have focused on using biomass to supplement fossil energy. 2,5-Dimethylfuran (DMF), as an important product of biomass chemical conversion, has promising applications. It can be used as fuel, possessing a high energy density (31.5 MJ / L) and octane number (119). Compared with traditional bioethanol, DMF has significant advantages and is more suitable as a gasoline additive. Simultaneously, due to the presence of diene bonds on its furan ring, it can also undergo a Diels-Alder reaction (DA reaction) with monoolefins such as ethylene to directly synthesize bio-based p-xylene.

[0003] 2,5-Dimethylfuran is mainly prepared by hydrogenolysis of 5-hydroxymethylfurfural (HMF). When hydrogen is used as the hydrogen source, commonly used catalysts include supported noble metals such as ruthenium (Ru), platinum (Pt), and palladium (Pd), as well as transition metals such as nickel (Ni), copper (Cu), and cobalt (Co). CN105032427A reported that Ru / Co3O4 prepared by co-precipitation achieved a HMF conversion rate of over 99% and a DMF yield of 93.4% under H2 conditions of 130℃ and 0.7 MPa. 2,5-Dimethylfuran is mainly prepared by hydrogenolysis of 5-hydroxymethylfurfural under the catalysis of noble or non-noble metals. However, current production processes often suffer from high raw material costs and short catalyst lifetimes, resulting in high DMF prices and hindering large-scale application. CN103554066A reported a strategy for preparing 2,5-dimethylfuran from fructose using nickel-tungsten carbide supported on activated carbon as a catalyst. First, a tetrahydrofuran system containing sulfuric acid was used to prepare 5-hydroxymethylfurfural (DMF) via dehydration at 160°C (maximum yield 64%). Subsequently, under the action of a nickel-tungsten carbide catalyst supported on activated carbon, a maximum DMF yield of 95% was achieved. CN103554066A reported a one-step method for producing 2,5-dimethylfuran from fructose, using fructose as raw material, Ru / C and AlCl3 and inorganic acids as catalysts, and N,N′-dimethylformamide as solvent, achieving a DMF yield of up to 66.3%. All of the above reactions involve the use of liquid acid. Although the catalytic effect is excellent, liquid acid causes severe equipment corrosion, significant environmental pollution due to alkali neutralization wastewater treatment, and numerous side reactions. It also produces a large number of byproducts (such as humic acid), affecting product separation and the stability of the hydrogenolysis catalyst. Furthermore, the reported substrate concentrations for the hydrogenolysis of HMF to DMF are currently low, which would significantly increase separation costs to obtain pure DMF. Therefore, there is a greater need for an efficient and green method to catalyze the preparation of 2,5-dimethylfuran from biomass, which can efficiently convert biomass raw materials such as fructose and glucose into 2,5-dimethylfuran. Summary of the Invention

[0004] The technical problem this invention aims to solve is the low catalytic efficiency, high cost, and environmental pollution associated with existing 2,5-dimethylfuran preparation processes. This invention provides a method for preparing 2,5-dimethylfuran from biomass. This method is simple to operate and has the advantages of high product selectivity, good catalyst stability, and easy product separation, achieving a green and efficient conversion of biomass to 2,5-dimethylfuran.

[0005] To solve the above-mentioned technical problems, the present invention provides a method for preparing 2,5-dimethylfuran by biomass conversion, comprising:

[0006] (1) In the presence of various organic solvents, biomass raw materials react with solid acid catalysts to obtain an organic solution containing 5-hydroxymethylfurfural and partially passivated products of 5-hydroxymethylfurfural functional groups.

[0007] (2) The organic solution obtained in step (1) and hydrogen gas react with the hydrogenolysis catalyst to prepare 2,5-dimethylfuran.

[0008] According to the present invention, the biomass raw material in step (1) is one or more of cellulose, inulin, cellobiose, sucrose, glucose or fructose, preferably fructose and / or glucose, and more preferably fructose.

[0009] According to the present invention, in step (1), the organic solvent includes solvent I and solvent II, wherein solvent I is an alcohol solvent, preferably at least one of methanol, ethanol, n-propanol, n-butanol, isopropanol, isoamyl alcohol, ethylene glycol, propylene glycol, glycerol or octanol, and more preferably one or two of isopropanol, isoamyl alcohol or n-butanol; solvent II is selected from at least one of acetone, tetrahydrofuran, 1,4-dioxane, methyl isobutyl ketone, γ-valerolactone or toluene, preferably one or two of acetone, 1,4-dioxane or tetrahydrofuran.

[0010] According to the present invention, the mass ratio of solvent I to solvent II is 0.1 to 100:1, preferably 0.5 to 20:1; the mass ratio of the total mass of the organic solvent to the mass of the biomass raw material is 1 to 100:1, preferably 2 to 50:1; and the mass ratio of the biomass raw material to the solid acid catalyst is 0.2 to 20:1, preferably 0.4 to 20:1.

[0011] According to the present invention, the reaction temperature in step (1) is 90–220°C, preferably 120–200°C; the reaction time is 5–300 minutes, preferably 10–240 minutes. Further, the reaction is carried out under an inert gas (e.g., nitrogen) at a pressure of 0.1–3.0 MPa, preferably 0.5–2.0 MPa.

[0012] According to the present invention, the solid acid catalyst in step (1) is selected from any one of SCM-36-SO3H molecular sieve, SCM-1-SO3H molecular sieve, H-beta molecular sieve, USY molecular sieve, sulfonated carbon, or A-15 resin; preferably, the solid acid catalyst is SCM-36-SO3H molecular sieve; preferably, the SCM-36-SO3H molecular sieve... The acid / Lewis acid ratio is 2.2 to 4.0; the content of -SO3H in the SCM-36-SO3H molecular sieve is 1.9 wt% to 18.0 wt%; the ratio of the external surface area to the total specific surface area of ​​the SCM-36-SO3H molecular sieve is 0.25 to 1.0, preferably 0.3 to 0.7.

[0013] According to the present invention, the preparation method of the SCM-36-SO3H molecular sieve includes the following steps:

[0014] S1. Disperse H-SCM-36 molecular sieve in toluene, add a mercapto compound to form reaction solution A, and stir thoroughly;

[0015] S2. Filter the reaction solution A, wash it under reflux with dichloromethane and ethyl acetate to obtain solid B;

[0016] S3. Mix solid B, hydrogen peroxide, alcohol and water evenly, and stir at room temperature for 8-30 hours.

[0017] S4. After filtering the suspension obtained in S3, add dilute sulfuric acid, stir, filter, wash, and dry to obtain SCM-36-SO3H molecular sieve.

[0018] According to the present invention, SCM-36 molecular sieve raw powder is calcined to remove the structure directing agent, and then subjected to ion exchange and calcination to obtain H-SCM-36 molecular sieve. Both calcination and ion exchange are conventional operations in the art. Preferably, the silica-alumina ratio of the H-SCM-36 molecular sieve is 20–50; the ratio of terminal silanol groups to the sum of internal silanol groups and bridged hydroxyl groups is 0.4–1.2.

[0019] According to the present invention, SCM-36 molecular sieve is prepared by the following method:

[0020] A crystallization solution is prepared by mixing a silicon source, sodium aluminate, sodium hydroxide, an organic structure directing agent, and water. After crystallization, the solution is separated and dried to obtain SCM-36 molecular sieve raw powder. Further, the silicon source is at least one of silica sol and silica gel; the sodium aluminate contains 38%–43% Al₂O₃ and 30%–33% Na₂O by weight; the organic structure directing agent contains a trimethylethylammonium ion structure; in the crystallization solution, the molar ratio of silicon source (SiO₂), sodium aluminate (Al₂O₃), sodium hydroxide, organic structure directing agent (trimethylethylammonium ion), and water is 1:0.016–0.050:0.10–0.20:0.15–0.30:10–50. Further, the crystallization conditions are: crystallization temperature of 155–175℃ and crystallization time of 2–8 days. Further, separation and drying are standard procedures in the art.

[0021] According to the present invention, in step S1, the thiol compound is selected from one or more of mercaptoethanol, mercaptoacetic acid, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, dimethylmercaptopropionic acid, methyl mercaptopropionate, 1,3-dimercaptopropane, or 2,3-dimercapto-1-propanol; preferably 3-mercaptopropyltrimethoxysilane or 3-mercaptopropyltriethoxysilane.

[0022] According to the present invention, in step S1, the mass ratio of toluene to molecular sieve is 10–200:1, preferably 20–100:1; the molar ratio of thiol compound to H-SCM-36 molecular sieve is 0.0001–0.5, preferably 0.0005–0.5. The stirring conditions are: temperature 25–30°C, time 5–48 h.

[0023] According to the present invention, in step S2, the mass ratio of dichloromethane to H-SCM-36 molecular sieve is 10 to 80:1; the mass ratio of ethyl acetate to H-SCM-36 molecular sieve is 10 to 80:1; and the reflux washing time is 6 to 30 h.

[0024] According to the present invention, in step S3, the molar ratio of hydrogen peroxide to H-SCM-36 molecular sieve is 1 to 100, preferably 2 to 60.

[0025] According to the present invention, in step S3, the alcohol is one or more of methanol or ethanol. The mass ratio of the alcohol to the H-SCM-36 molecular sieve is 100 to 300:1.

[0026] According to the present invention, in step S3, the mass ratio of water to molecular sieve is 200 to 600:1.

[0027] According to the present invention, in step S4, the concentration of dilute sulfuric acid is 0.1 to 1.0 mol / L, and the amount of dilute sulfuric acid added is 10 to 100 mL / g molecular sieve.

[0028] According to the present invention, in step S4, the stirring conditions are: temperature of 25-30°C and time of 5-48h.

[0029] According to the present invention, in step (2), the mass ratio of the organic solution containing 5-hydroxymethylfurfural and its passivation product obtained in step (1) to the hydrogenolysis catalyst is 30 to 200:1, preferably 50 to 150.

[0030] According to the present invention, hydrogen gas is introduced into the reaction system in step (2) to adjust the reaction pressure. The reaction pressure is 0.5 to 4.0 MPa, preferably 0.5 to 3.0 MPa.

[0031] According to the present invention, the reaction conditions for step (2) are as follows: the reaction temperature is 130-220°C, preferably 150-200°C; the reaction time is 1-12h, preferably 2-10h.

[0032] According to the present invention, the product obtained in step (2) can be separated into 2,5-dimethylfuran by conventional methods, such as distillation.

[0033] According to the present invention, the hydrogenolysis catalyst in step (2) is a noble metal and / or non-noble metal hydrogenation catalyst, including any one of Pd / C, Pt / C, Ru / C, Pd / Al2O3, Pt / Al2O3, Ru / Al2O3, Ru / Co3O4, Ni-Co3O4 / C, Ni-Al2O3, Ni-Fe / C or Ni-SCM-X; preferably Ni-SCM-X.

[0034] According to the present invention, X in Ni-SCM-X is 14 or 15. SCM-14 molecular sieve and its preparation method are described in patent CN109081360A, the entire contents of which are incorporated herein by reference. SCM-15 molecular sieve and its preparation method are described in patent CN109081359A, the entire contents of which are incorporated herein by reference.

[0035] According to the present invention, the Ni-SCM-X, based on the mass of SCM-X, has a Ni content of 0.2wt% to 5.0wt%, preferably 0.5wt% to 3.0wt%; the Si / Ge molar ratio of the SCM-X is 1.5 to 8, preferably 2 to 7.

[0036] According to the present invention, the total acidity of Ni-SCM-X is 130–220 μmol·g. -1 Preferably, it is 150–200 μmol·g -1 .

[0037] According to the present invention, the Ni-SCM-X The acid / Lewis acid ratio is 0.3 to 0.8, preferably 0.4 to 0.6.

[0038] According to the present invention, in the Ni-SCM-X, metallic Ni and Ni 2+ molar ratio (Ni / Ni) 2+ The value is 0.02 to 0.15, preferably 0.05 to 0.12.

[0039] According to the present invention, in the Ni-SCM-X, the average size of the nickel particles is 2 to 6 nm, preferably 3 to 5 nm.

[0040] According to the present invention, the preparation method of Ni-SCM-X includes:

[0041] SCM-X molecular sieves are mixed with nickel-containing precursors, and the resulting product is dried, calcined, and reduced to obtain Ni-SCM-X. In the SCM-X molecular sieve, X is 14 or 15.

[0042] According to the present invention, the nickel-containing precursor is selected from at least one of nickel-cerocenium (bis(cyclopentadiene)nickel), bis-(1,5-cyclooctadiene)nickel, bis(tetramethylcyclopentadienyl)nickel, 1,2-bis(diphenylphosphine)ethane nickel chloride and bis(triphenylphosphine) nickel chloride, preferably nickel-cerocenium.

[0043] According to the present invention, the mass ratio of Ni (theoretical amount of Ni in organometallic precursor) to SCM-X molecular sieve is 0.2 to 8.0:100, preferably 0.5 to 5.0:100.

[0044] According to the present invention, the mixing is a physical mixing, and the mixing method includes grinding, ball milling, etc.

[0045] According to the present invention, the drying conditions are: drying at 50-130°C for 2-8 hours.

[0046] According to the present invention, the calcination conditions are: calcination at 300-650°C for 1-12 hours, and the calcination atmosphere is oxygen or air.

[0047] According to the present invention, the reduction is preferably carried out in a hydrogen atmosphere, the reduction temperature is 300-500°C, preferably 350-450°C, and the reduction time is 1-8 hours, preferably 2-6 hours.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] (1) This invention uses biomass as raw material, which is inexpensive and widely available. By adopting a functional group protection strategy, the chemically active, unstable, and difficult-to-store intermediate product HMF is selectively passivated in one step to generate RMF. This reduces the self-aggregation of HMF and the formation of other by-products to a certain extent, thereby achieving a high yield of the target product while increasing the substrate concentration.

[0050] (2) This invention directly uses RMF in the hydrogenolysis reaction, breaking carbon-oxygen bonds while eliminating protecting groups, thus completing the hydrogenation reaction and generating DMF. This solves the problem of generally low carbon yield in the hydrogenolysis of high-concentration HMF to DMF, and also avoids the high separation energy consumption caused by excessively low concentrations.

[0051] (3) This invention obtains the final product DMF through a series of biomass-RMF(HMF) and RMF(HMF)-DMF processes. Both reactions use the same dual organic solvent system, without involving complex RMF or HMF separation processes. The active groups are protected and eliminated during the series two-step reaction process, and no other by-products are generated throughout the process.

[0052] (4) This invention uses the novel SCM series molecular sieves as catalysts. In the sugar-RMF (HMF) reaction, H-SCM-36 with more silanol groups on the surface is preferred for sulfonate loading. In the RMF (HMF)-DMF reaction, silicon-germanium molecular sieves SCM-14 or SCM-15 are preferred for metal loading and selective hydrogenation. The catalysts used in the whole process add a bright touch to the creation of a bio-based PX production line. Attached Figure Description

[0053] Figure 1 A schematic diagram of the process for preparing 2,5-dimethylfuran from biomass in this invention;

[0054] Figure 2 Infrared spectra of SCM-36 and conventional FER molecular sieves;

[0055] Figure 3 The image shows the XRD pattern of the solid acid catalyst (SCM-36-SO3H) obtained in Example 1.

[0056] Figure 4 Here is a SEM image of the solid acid catalyst (SCM-36-SO3H) obtained in Example 1;

[0057] Figure 5 The image shows the pyridine infrared spectrum of the solid acid catalyst (SCM-36-SO3H) obtained in Example 1.

[0058] Figure 6 The XRD pattern of the hydrogenolysis catalyst (Ni-SCM-14) obtained in Example 21 is shown below.

[0059] Figure 7 The NH3-TPD diagram of the hydrogenolysis catalyst (Ni-SCM-14) obtained in Example 21 is shown.

[0060] Figure 8 XPS image of the hydrogenolysis catalyst (Ni-SCM-14) obtained in Example 21;

[0061] Figure 9 TEM image of the hydrogenolysis catalyst (Ni-SCM-14) obtained in Example 21;

[0062] Figure 10The image shows the XRD pattern of the hydrogenolysis catalyst (Ni-SCM-15) obtained in Example 22. Detailed Implementation

[0063] In this invention, the NH3 temperature-programmed desorption (NH3-TPD) experiment was conducted on a TPD / TPRAltamiraAMI-3300 instrument, and the total acid content was calculated by fitting and peaking the obtained spectrum.

[0064] In this invention, the XRD measurement method for the product is as follows: the phase composition of the sample is analyzed using a Rigaku Ultima IV X-ray powder diffractometer (Japan), with a CuKα ray source. Nickel filter, 2θ scanning range 2°-50°, operating voltage 35kV, current 25mA, scanning rate 10° / min.

[0065] In this invention, the acid content and type of the catalyst are determined using the pyridine adsorption infrared method (Nicolet Model 710 spectrometer). The specific operation steps are as follows: a) Sample pretreatment: The sample (approximately 30 mg) is compressed into a thin disc with a diameter of 13 mm and placed in an infrared sample cell; then, the sample is pretreated at 400°C under vacuum conditions for 1 hour. After the sample cell cools to room temperature, the infrared data of the sample is scanned as background. b) Pyridine adsorption: Pyridine vapor is introduced into the in-situ under room temperature and vacuum conditions until adsorption reaches equilibrium, with an adsorption time of 1 hour. c) Pyridine desorption: After adsorption, a vacuum is drawn at 100°C until the internal pressure no longer changes, with a desorption time of 40 minutes, and the infrared absorption spectra are scanned and recorded. The difference spectrum before and after pyridine adsorption is the obtained pyridine adsorption-infrared absorption spectrum. The acid content of the sample is semi-quantitatively calculated based on the spectrum.

[0066]

[0067] Where r and w are the diameter (cm) and mass (g) of the catalyst disc, respectively, and A is the integral absorbance value at the specified wavenumber peak based on the scanned pyridine adsorption-infrared absorption spectrum. IMEC is the integral molar extinction coefficient. L Version 2.22, IMEC B It is 1.67, C L L acid content (μmol·g) -1 ), C B The acidity of Brønsted acid (μmol·g) -1 ).

[0068] In this invention, the transmission electron microscope (TEM) used for the molecular sieve is a S-4800I1 field emission scanning electron microscope. The size of the nickel particles in the molecular sieve is obtained by statistically analyzing the sizes of approximately 30 nickel particles from the TEM images and then calculating the average value.

[0069] In this invention, the element binding energy on the catalyst surface was measured using a Thermo X-ray photoelectron spectrometer (ESCA LAB-250), with C1s = 284.6 eV used as an internal standard to correct the measured element signals.

[0070] In this invention, an inductively coupled plasma atomic emission spectrometer (ICP) of model Varian 725-ES is used to dissolve the analytical sample in hydrofluoric acid to detect the content of metal elements.

[0071] In this invention, 5-hydroxymethylfurfural (HMF), 5-R-oxymethylfurfural (R = ethyl, propionic, butyric, etc., abbreviated as RMF), and 2,5-dimethylfuran (DMF) were qualitatively analyzed by gas chromatography-mass spectrometry (GC-MS). The yields and conversions of 5-hydroxymethylfurfural and 5-R-oxymethylfurfural, as well as the yield of the reaction product 2,5-dimethylfuran, were analyzed by gas chromatography (GC). The GC-MS system was an Agilent 7890A from Agilent Technologies, USA, with an HP-5 nonpolar capillary column (30m, 0.53mm). The gas chromatograph was an Agilent 7890B, with a flame ionization detector (FID) and an SE-54 capillary column (30m, 0.53mm).

[0072] The DMF preparation reaction from biomass feedstock consists of two steps. The first step involves preparing HMF and RMF from the biomass feedstock. The yields of HMF and RMF are calculated using the following formulas:

[0073] The yield % of products HMF and RMF = (molar amount of HMF and RMF produced in the reaction n1) / (molar amount of hexose sugar units in the biomass substrate n0) × 100%. Wherein, the hexose sugar unit is C6H... 10 O5.

[0074] In the second process, HMF and RMF(n1) generated in the first process are used as raw materials and reacted with hydrogen to prepare DMF. The conversion formulas for HMF and RMF are as follows:

[0075] The conversion rate % of HMF and RMF = (the remaining molar amount of HMF and RMF after the second reaction n2) / (the molar amount of HMF and RMF in the reactants of the second process n1) × 100%.

[0076] In the second process, the DMF selectivity formula is:

[0077] Selectivity of product DMF % = (molar amount of DMF generated in the reaction n3) / (molar amount of HMF and RMF in the second process reactants n1 - molar amount of HMF and RMF remaining after the second process reaction n2) × 100%.

[0078] Combination Figure 1 The process for preparing 2,5-dimethylfuran from biomass according to the present invention is described below:

[0079] (1) In the presence of various organic solvents, biomass raw materials react with solid acid catalysts to obtain an organic solution containing 5-hydroxymethylfurfural and partially passivated products of 5-hydroxymethylfurfural functional groups.

[0080] (2) The organic solution containing 5-hydroxymethylfurfural and partially passivated 5-hydroxymethylfurfural functional groups obtained in process (1) is reacted with hydrogen and a hydrogenolysis catalyst to obtain a reaction product containing 2,5-dimethylfuran. The reaction product containing 2,5-dimethylfuran can be further separated to obtain 2,5-dimethylfuran.

[0081] To facilitate understanding of the present invention, the following embodiments are provided. However, these embodiments are only for the purpose of helping to understand the present invention and should not be regarded as specific limitations of the present invention.

[0082] Example 1

[0083] A mixture was prepared by stirring 14.35 g of deionized water, 0.604 g of sodium aluminate (containing 40.5 wt% Al₂O₃, 30.6 wt% Na₂O, with the balance being H₂O), 0.366 g of sodium hydroxide, 7.06 g of trimethylethyl ammonium hydroxide solution (containing 25.00 wt% trimethylethyl ammonium hydroxide) (organic structure directing agent R), and 12.60 g of silica sol (containing 40.0 wt% SiO₂) at room temperature for 4 hours. The final material ratio (molar ratio) was as follows:

[0084] SiO2 / Al2O3 = 35;

[0085] NaOH / SiO2 = 0.18;

[0086] Trimethylethylammonium hydroxide (R) / SiO2 = 0.20;

[0087] H2O / SiO2 = 18.

[0088] The mixture was placed in a stainless steel reactor and heated at 170°C and 20 rpm for 3 days to crystallize. After crystallization, the mixture was filtered, washed, and dried overnight in an oven at 100°C. The XRD pattern of the obtained product is shown below. Figure 1 As shown in Table 1, this is SCM-36 molecular sieve.

[0089] The SCM-36 molecular sieve obtained above was calcined to remove the structure-directing agent, followed by ion exchange and calcination to obtain H-SCM-36. The infrared spectrum of H-SCM-36 is shown below. Figure 2 As shown, 3739cm -1 The hydroxyl groups at the surface of the molecular sieve are attributed to silanol groups. As can be seen from the figure, H-SCM-36 molecular sieve has more Si-OH groups than conventional FER molecular sieves.

[0090] 1.5 g of H-SCM-36 molecular sieve and 1.0 g of 3-mercaptopropyltrimethoxysilyl group were added to 50 g of toluene and stirred thoroughly at 25-30 °C for 24 h. After stirring, the mixture was filtered, and 30.0 g of dichloromethane and 30.0 g of ethyl acetate were added and refluxed for 24 h. The resulting solid was then added to a mixture of 40 g of H2O2 (30%), 120 g of methanol, and 400 g of deionized water and stirred at room temperature for 15 h. After stirring, the mixture was filtered, and the precipitate was dispersed in 40 mL of sulfuric acid (0.6 mol / L) and stirred thoroughly for 15 h. Finally, the mixture was thoroughly washed with ethanol and water and dried to obtain H-SCM-36-SO3H.

[0091] XRD of the sample Figure 3 As shown. The SEM image of the sample is shown below. Figure 4 As shown. The pyridine infrared spectrum of the sample is as follows. Figure 5 As shown, the result calculated from this The acid ratio is 3.3.

[0092] Example 2

[0093] The H-SCM-36 molecular sieve is the same as in Example 1.

[0094] 1.5 g of H-SCM-36 and 0.5 g of 3-mercaptopropyltrimethoxysilyl group were added to 50 g of toluene and stirred thoroughly at 25-30 °C for 24 h. After stirring, the mixture was filtered, and 30.0 g of dichloromethane and 30.0 g of ethyl acetate were added and refluxed for 24 h. The resulting solid was then added to a mixture of 40 g of H2O2 (30%), 120 g of methanol, and 400 g of deionized water, and stirred at room temperature for 15 h. After stirring, the mixture was filtered, and the precipitate was dispersed in 40 mL of sulfuric acid (0.6 mol / L) and stirred thoroughly for 15 h. Finally, the mixture was thoroughly washed with ethanol and water and dried to obtain H-SCM-36-SO3H.

[0095] XRD of the sample and Figure 3 Similar. The SEM images of the samples are similar to... Figure 4 Similarly, the results were calculated from the pyridine infrared spectrum of the sample. The acid ratio is 3.0.

[0096] Example 3

[0097] The H-SCM-36 molecular sieve is the same as in Example 1.

[0098] 1.5 g of H-SCM-36 and 1.0 g of 3-mercaptopropyltriethoxysilyl group were added to 50 g of toluene and stirred thoroughly at 25-30 °C for 24 h. After stirring, the mixture was filtered, and 30.0 g of dichloromethane and 30.0 g of ethyl acetate were added and refluxed for 24 h. The resulting solid was then added to a mixture of 40 g of H2O2 (30%), 120 g of methanol, and 400 g of deionized water, and stirred at room temperature for 15 h. After stirring, the mixture was filtered, and the precipitate was dispersed in 40 mL of sulfuric acid (0.6 mol / L) and stirred thoroughly for 15 h. Finally, the mixture was thoroughly washed with ethanol and water and dried to obtain H-SCM-36-SO3H.

[0099] XRD of the sample and Figure 3 Similar. The SEM images of the samples are similar to... Figure 4 Similarly, the results were calculated from the pyridine infrared spectrum of the sample. The acid ratio is 3.1.

[0100] Example 4

[0101] The H-SCM-36 molecular sieve is the same as in Example 1.

[0102] 1.5 g of H-SCM-36 and 1.0 g of 3-mercaptopropyltrimethoxysilyl group were added to 50 g of toluene and stirred thoroughly at 25-30 °C for 24 h. After stirring, the mixture was filtered, and 30.0 g of dichloromethane and 30.0 g of ethyl acetate were added and refluxed for 24 h. The resulting solid was then added to a mixture of 20 g of H2O2 (30%), 120 g of methanol, and 400 g of deionized water, and stirred at room temperature for 15 h. After stirring, the mixture was filtered, and the precipitate was dispersed in 40 mL of sulfuric acid (0.6 mol / L) and stirred thoroughly for 15 h. Finally, the mixture was thoroughly washed with ethanol and water and dried to obtain H-SCM-36-SO3H.

[0103] XRD of the sample and Figure 3 Similar. The SEM images of the samples are similar to... Figure 4 Similarly, the results were calculated from the pyridine infrared spectrum of the sample. The acid ratio is 2.9.

[0104] Table 1 Properties of solid acid catalysts in Examples 1-4

[0105]

[0106] Examples 5-8

[0107] Using fructose as a substrate and tetrahydrofuran and n-butanol as solvents, 0.5 g of H-SCM-36-SO3H molecular sieve (from Examples 1-4), 4.0 g of fructose, 10 g of tetrahydrofuran, and 10 g of n-butanol were added to a high-pressure reactor equipped with a stirrer. Nitrogen gas at 0.5 MPa was introduced to prevent boiling of the organic solvents. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 165 °C for 30 min. The fructose conversion rate and the yields of the target products 5-hydroxymethylfurfural (HMF) and 5-R-oxymethylfurfural (RMF) were analyzed. The conversion rate and the sum of the HMF and RMF yields are shown in Table 2.

[0108] Table 2 Catalyst Evaluation Results of Examples 1-4

[0109]

[0110] Example 9

[0111] Using fructose as a substrate and tetrahydrofuran and n-butanol as solvents, 0.5 g USY, 4.0 g fructose, 10 g tetrahydrofuran, and 10 g n-butanol were added to a stirred high-pressure reactor. Nitrogen gas at 0.5 MPa was introduced to prevent boiling of the organic solvents. The temperature was raised to the preset temperature using a programmed heating mantle, and the reactor was then stirred magnetically. The reaction was carried out at 165 °C for 30 min. Analysis of the reaction solution yielded the fructose conversion rate and the yields of the target products 5-hydroxymethylfurfural (HMF) and 5-R-oxymethylfurfural (RMF). The fructose conversion rate was greater than 99%, and the sum of the yields of HMF and RMF was 62.7%.

[0112] Example 10

[0113] Using fructose as a substrate and tetrahydrofuran and n-butanol as solvents, 0.5 g of A-15 resin, 4.0 g of fructose, 10 g of tetrahydrofuran, and 10 g of n-butanol were added to a stirred high-pressure reactor. Nitrogen gas at 0.5 MPa was introduced to prevent boiling of the organic solvents. The temperature was raised to the preset temperature using a programmed heating mantle, and the reactor was then stirred magnetically. The reaction was carried out at 165 °C for 30 min. Analysis of the reaction solution yielded the fructose conversion rate and the yields of the target products 5-hydroxymethylfurfural (HMF) and 5-R-oxymethylfurfural (RMF). The fructose conversion rate was greater than 99%, and the sum of the yields of HMF and RMF was 60.3%.

[0114] Examples 11-19

[0115] To more intuitively describe the reaction conditions and results of Examples 11-19, the parameters and reaction results are listed in Table 3, where the fructose conversion rate is greater than 99%.

[0116] Table 3 Reaction conditions and results of Examples 11-19

[0117]

[0118] Example 20

[0119] Using fructose as a substrate and tetrahydrofuran and n-butanol as solvents, 0.5 g of the catalyst from Example 1 (H-SCM-36-SO3H), 4.0 g of fructose, 10 g of tetrahydrofuran, and 10 g of n-butanol were added to a high-pressure reactor equipped with a stirrer. Nitrogen gas at 0.5 MPa was introduced to prevent boiling of the organic solvents. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 165 °C for 30 min. The used catalyst was washed, dried, and then used in the next reaction. A total of four cycles were performed. The catalytic evaluation results are shown in Table 4.

[0120] Table 4 Catalyst recycling data from Example 1

[0121] Number of times to reuse Fructose conversion rate (%) HMF+RMF yield (%) 1 time >99 71.5 2 times >99 68.7 3 times >99 68.3 4 times >99 68.2

[0122] Example 21

[0123] SCM-14 molecular sieve was synthesized according to the preparation method in Example 1 of CN109081360A, wherein the Si / Ge molar ratio was 3.7. The nickel precursor was nickel-ceramic, and the mass ratio of Ni (theoretical amount of Ni in the organometallic precursor) to the above-mentioned SCM-14 molecular sieve was 1.1:100. The mixture was thoroughly ground in a mortar to obtain a uniformly dispersed mixture. The above product was dried in an oven at 100°C for 4 hours, then calcined at 550°C for 4 hours, and reduced under hydrogen conditions at a reduction temperature of 400°C for 3 hours. Ni-SCM-14 molecular sieve was obtained.

[0124] XRD of the sample Figure 6 As shown. The NH3-TPD of the sample is as follows. Figure 7 As shown, the total acid content calculated from this is 176 μmol·g. -1 The XPS values ​​of the sample are as follows: Figure 8 As shown, a binding energy of 852.0 eV corresponds to the metallic element Ni(2p) 3 / 2 The peak), with a binding energy of 855.6 eV, corresponds to divalent nickel (2). + Metallic Ni and Ni 2+ The molar ratio is calculated using the ratio of the two peak areas (Ni / Ni). 2+ The ratio was 0.08. The TEM image of the sample was as follows: Figure 9 As shown, the nickel is uniformly distributed without significant aggregation, and the average particle size is 3.5 nm. Inductively coupled plasma atomic emission spectrometry (ICP) determined the relative Ni content in the sample to be 1.1 wt%. The sample was calculated using pyridine adsorption infrared spectroscopy. The acid ratio is 0.52.

[0125] Example 22

[0126] SCM-15 molecular sieve was synthesized according to the preparation method in Example 1 of CN109081359A, wherein the Si / Ge molar ratio was 5.1. The nickel precursor was nickel-ceramic, and the mass ratio of Ni (theoretical amount of Ni in the organometallic precursor) to the above-mentioned SCM-15 molecular sieve was 1.2:100. The mixture was thoroughly ground in a mortar to obtain a uniformly dispersed mixture. The above product was dried in an oven at 80°C for 5 hours, then calcined at 550°C for 4 hours, and reduced under hydrogen atmosphere at a reduction temperature of 400°C for 2 hours. Ni-SCM-15 molecular sieve was obtained.

[0127] XRD of the sample Figure 10 As shown. The NH3-TPD of the sample and Figure 7 Similarly, the total acidity calculated from this is 155 μmol·g. -1 The XPS values ​​of the sample are... Figure 8 Similarly, a binding energy of 852.0 eV corresponds to the metallic element Ni (2p0). 3 / 2 The peak), with a binding energy of 855.6 eV, corresponds to divalent nickel (2). + Metallic Ni and Ni 2+ The molar ratio is calculated using the ratio of the two peak areas (Ni / Ni). 2+ The ratio was 0.11. The TEM values ​​of the sample were... Figure 9 Similarly, it can be seen that the nickel is evenly distributed without obvious aggregation, and the average particle size of the nickel is 4.0 nm. The relative Ni content in the sample was determined to be 1.2 wt% using inductively coupled plasma atomic emission spectrometry (ICP). The sample was calculated using pyridine adsorption infrared spectroscopy. The acid ratio is 0.45.

[0128] Examples 23-24

[0129] 0.2g of the catalyst from Examples 21-22 and 15g of the reaction product obtained in Example 5 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190°C for 3 hours. The HMF+RMF conversion rate and DMF selectivity of the product were calculated by gas phase analysis of the reaction product, as shown in Table 5.

[0130] Table 5 Catalytic evaluation results of catalysts in Examples 21-22

[0131]

[0132] Example 25

[0133] 0.2 g of Ni-Fe / C hydrogenolysis catalyst and 15 g of the reaction product obtained in Example 5 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5 MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190 °C for 3 h. Gas phase analysis of the reaction product showed that the HMF+RMF conversion rate was 95%, and the DMF selectivity was 71.2%.

[0134] Example 26

[0135] 0.2 g of Pd / C hydrogenolysis catalyst and 15 g of the reaction liquid obtained in Example 5 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5 MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190 °C for 3 h. The gas phase analysis of the reaction product showed that the HMF+RMF conversion rate was 99%, and the DMF selectivity was 70.1%.

[0136] Example 27

[0137] 0.2 g of Ru / Al₂O₃ hydrogenolysis catalyst and 15 g of the reaction product obtained in Example 5 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5 MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190 °C for 3 h. Gas phase analysis of the reaction product showed that the HMF+RMF conversion rate was greater than 99%, and the DMF selectivity was 73.5%.

[0138] Examples 28-33

[0139] The catalyst from Example 21 and the reaction product obtained in Example 5 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced. The temperature was raised to the preset temperature using a programmed heating mantle, and the reaction was carried out with magnetic stirring. To more intuitively describe the reaction conditions and results of Examples 28-33, the parameters and reaction results are listed in Table 6.

[0140] Table 6 Reaction conditions and results of Examples 28-33

[0141]

[0142] Example 34

[0143] 0.2 g of the catalyst from Example 21 and 15 g of the reaction product obtained in Example 5 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5 MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190°C for 3 hours. The used catalyst was washed, dried, and then added to the next reaction. The reaction was repeated a total of 4 times. The catalytic evaluation results are shown in Table 7.

[0144] Table 7 Catalyst Recycling Data from Example 21

[0145] Number of times to reuse HMF+RMF conversion rate (%) DMF selectivity (%) 1 time >99 80.5 2 times >99 78.9 3 times >99 78.2 4 times >99 77.8

[0146] Comparative Example 1

[0147] The alcohol solvents (tetrahydrofuran and n-butanol) in Example 5 were replaced with an equal amount of water.

[0148] Using fructose as a substrate and water as a solvent, 0.5 g of H-SCM-36-SO3H (from Example 1), 4.0 g of fructose, and 20 g of water were added to a high-pressure reactor equipped with a stirrer. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 165°C for 30 min. Analysis of the reaction product yielded fructose conversion and target product yield: fructose conversion > 99%, with only 5-hydroxymethylfurfural (HMF) produced, and an HMF yield of 25%.

[0149] 0.2 g of the catalyst from Example 21 and 15 g of the reaction product obtained from Comparative Example 1 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5 MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190°C for 3 hours. The selectivity of the product DMF was calculated by gas phase analysis of the reaction product. The HMF conversion rate was 99%, and the DMF selectivity was 60%.

[0150] Comparative Example 2

[0151] In Example 5, the alcohol solvents (tetrahydrofuran and n-butanol) were replaced with a water-organic two-phase solvent system.

[0152] Using fructose as a substrate and water + n-butanol as a solvent, 0.5 g of H-SCM-36-SO3H (from Example 1), 4.0 g of fructose, 10 g of water, and 10 g of n-butanol were added to a high-pressure reactor equipped with a stirrer. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 165°C for 30 min. Analysis of the reaction product yield revealed a fructose conversion rate >99%, and the combined yields of 5-hydroxymethylfurfural (HMF) and 5-R-oxymethylfurfural (RMF) were 48.1%.

[0153] 0.2 g of the catalyst from Example 21 and 15 g of the reaction product obtained in Comparative Example 2 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5 MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190 °C for 3 h. Gas phase analysis of the reaction liquid showed that the HMF+RMF conversion rate was 80%, and the selectivity of the product DMF was 56%.

[0154] Comparative Example 3

[0155] SCM-14 molecular sieve was synthesized according to the preparation method in Example 1 of CN109081360A, wherein the Si / Ge molar ratio was 3.7. The nickel precursor was nickel levulinate, and the mass ratio of Ni (theoretical amount of Ni in nickel nitrate) to the above SCM-14 molecular sieve was 1.0:100. The mixture was thoroughly ground in a mortar to obtain a uniformly dispersed mixture. The above product was dried in an oven at 100°C for 4 hours, then calcined at 550°C for 4 hours, and reduced under hydrogen atmosphere at a reduction temperature of 400°C for 3 hours. Ni-SCM-14 molecular sieve was obtained.

[0156] The Si / Ge molar ratio of the sample was determined to be 3.7 and the relative Ni content to be 1.0 wt% by inductively coupled plasma atomic emission spectrometry (ICP). The total acidity calculated based on the NH3-TPD of the sample was 161 μmol·g. -1 The results were calculated based on the pyridine infrared spectrum of the sample. The acid ratio is 0.82. The Ni / Ni ratio was calculated based on the XPS of the sample. 2+ The ratio was 0.35. Based on the TEM results of the sample, the average particle size of the nickel particles was calculated to be 10.3 nm.

[0157] Using fructose as a substrate and tetrahydrofuran and n-butanol as solvents, 0.5 g of H-SCM-36-SO3H (from Example 1), 4.0 g of fructose, 10 g of tetrahydrofuran, and 10 g of n-butanol were added to a high-pressure reactor equipped with a stirrer. Nitrogen gas at 0.5 MPa was introduced to prevent boiling of the organic solvent. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 165 °C for 30 min. The reaction product was analyzed to obtain the fructose conversion rate and the yields of the target products 5-hydroxymethylfurfural (HMF) and 5-R-oxymethylfurfural (RMF). The fructose conversion rate was >99%, and the HMF+RMF yield was 71.5%.

[0158] 0.2 g of the Ni-SCM-14 molecular sieve catalyst obtained in Comparative Example 3 and 15 g of the reaction product obtained in Comparative Example 3 were added to a high-pressure reactor equipped with a stirrer, and hydrogen gas was introduced at 1.5 MPa. The temperature was raised to the preset temperature using a programmed heating mantle, and then stirred magnetically. The reaction was carried out at 190 °C for 3 h. Gas phase analysis of the reaction product showed that the HMF+RMF conversion rate was 75%, and the DMF selectivity was 57%.

[0159] The specific embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing 2,5-dimethylfuran from biomass conversion, comprising: (1) In the presence of multiple organic solvents, biomass raw materials are reacted with solid acid catalysts to obtain an organic solution containing 5-hydroxymethylfurfural and partially passivated products of 5-hydroxymethylfurfural functional groups, wherein the biomass raw materials are one or more of cellulose, inulin, cellobiose, sucrose, glucose or fructose. (2) The organic solution obtained in step (1) and hydrogen gas react with the hydrogenolysis catalyst to prepare 2,5-dimethylfuran; The organic solvent includes solvent I and solvent II; solvent I is an alcohol solvent, and solvent II is selected from at least one of acetone, tetrahydrofuran, 1,4-dioxane, methyl isobutyl ketone, γ-valerolactone or toluene, and the mass ratio of solvent I to solvent II is 0.1 to 100:1; The solid acid catalyst mentioned in step (1) is SCM-36-SO3H molecular sieve, in which the content of -SO3H is 1.9wt%~18.0wt%, and the Brønsted acid / Lewis acid ratio of the SCM-36-SO3H molecular sieve is 2.2~4.0; The hydrogenolysis catalyst mentioned in step (2) is Ni-SCM-X, where X is 14 or 15. The molar ratio of metallic Ni to oxidized NiO in Ni-SCM-X is 0.02 to 0.

15. The average size of nickel particles in Ni-SCM-X is 2 to 6 nm. The content of Ni in Ni-SCM-X, based on the mass of SCM-X, is 0.2 wt% to 5.0 wt%. The Brønsted acid / Lewis acid ratio of Ni-SCM-X is 0.3 to 0.

8.

2. The method according to claim 1, characterized in that, In step (1), solvent I is at least one of methanol, ethanol, n-propanol, n-butanol, isopropanol, isoamyl alcohol, ethylene glycol, propylene glycol, glycerol, or octanol; solvent II is one or two of acetone, 1,4-dioxane, or tetrahydrofuran. And / or, the mass ratio of solvent I to solvent II is 0.5~20:1; And / or, the total mass ratio of organic solvents to biomass feedstock is 1~100:

1.

3. The method according to claim 2, characterized in that, In step (1), solvent I is one or two of isopropanol, isoamyl alcohol, or n-butanol; And / or, the total mass ratio of organic solvents to biomass feedstock is 2~50:

1.

4. The method according to claim 1, characterized in that, In step (1), the mass ratio of biomass feedstock to solid acid catalyst is 0.2~20:

1.

5. The method according to claim 4, characterized in that, In step (1), the biomass raw material is fructose and / or glucose; And / or, in step (1), the mass ratio of biomass feedstock to solid acid catalyst is 0.4~20:

1.

6. The method according to claim 1, characterized in that, In step (1), the reaction temperature is 90~220℃; the reaction time is 5~300 minutes. And / or, the reaction in step (1) is carried out under an inert gas with an inert gas pressure of 0.1~3.0 MPa.

7. The method according to claim 6, characterized in that, In step (1), the reaction temperature is 120~200℃; the reaction time is 10~240 minutes. And / or, the inert gas pressure in step (1) is 0.5~2.0MPa.

8. The method according to claim 1, characterized in that, The external specific surface area / total specific surface area of ​​the SCM-36-SO3H molecular sieve is 0.25~1.

9. The method according to claim 8, characterized in that, The external specific surface area / total specific surface area of ​​the SCM-36-SO3H molecular sieve is 0.3~0.

7.

10. The method according to claim 1, characterized in that, In the Ni-SCM-X, the Si / Ge molar ratio of the SCM-X molecular sieve is 1.5~8.

11. The method according to claim 1, characterized in that, The Ni-SCM-X, based on the mass of SCM-X, has a Ni content of 0.5wt%~3.0wt% (calculated as Ni). And / or, in the Ni-SCM-X, the Si / Ge molar ratio of the SCM-X molecular sieve is 2~7.

12. The method according to claim 1, characterized in that, The total acidity of the Ni-SCM-X is 130~220 µmol•g. -1 ; And / or, the molar ratio of metallic Ni to oxidized NiO in the Ni-SCM-X is 0.05~0.12; And / or, the average size of the nickel particles in the Ni-SCM-X is 3~5 nm.

13. The method according to claim 12, characterized in that, The total acidity of the Ni-SCM-X is 150~200 µmol•g. -1 ; And / or, the Brønsted acid / Lewis acid ratio of the Ni-SCM-X is 0.4~0.

6.

14. The method according to claim 1, characterized in that, In step (2), the mass ratio of the organic solution containing 5-hydroxymethylfurfural and its passivation products obtained in step (1) to the hydrogenolysis catalyst is 30~200:

1.

15. The method according to claim 1, characterized in that, In step (2), the mass ratio of the organic solution containing 5-hydroxymethylfurfural and its passivation products obtained in step (1) to the hydrogenolysis catalyst is 50~150:

1.

16. The method according to claim 1, characterized in that, Hydrogen gas is introduced into the reaction system in step (2) to adjust the reaction pressure; the reaction pressure is 0.5~4.0 MPa; And / or, the reaction conditions for step (2) are as follows: the reaction temperature is 130~220℃; the reaction time is 1~12h.

17. The method according to claim 16, characterized in that, The reaction pressure in step (2) is 0.5~3.0 MPa; And / or, the reaction conditions for step (2) are as follows: the reaction temperature is 150~200℃; the reaction time is 2~10h.

Citation Information

Patent Citations

  • Method for preparing 2,5-dimethyl furan

    CN103554066A

  • Preparation method of 2,5-dimethylfuran

    CN105032427A

  • Molecular sieve SCM-15 and its synthetic method and application

    CN109081359A

  • Molecular sieve SCM-14 and its synthetic method and application

    CN109081360A

  • Method for preparing 2,5-furandimethanol from biomass sugar

    CN112574142A