A method for resource utilization of clay lithium slag and cat litter prepared by the method
By mixing clay lithium slag with calcium salts and hydroxides and then aging and acidifying it to convert it into bentonite, and then mixing it with deodorizers, antibacterial agents and binders to granulate it, high-value-added cat litter is prepared. This solves the problems of high energy consumption and low-end utilization of lithium slag, and realizes the full utilization of lithium slag and the efficient preparation of cat litter.
Patent Information
- Application Number
- CN202411831966.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-12
AI Technical Summary
Existing lithium slag treatment methods suffer from high energy consumption, high cost, low-end utilization methods, and inability to achieve full utilization, especially the waste residue treatment problem of lithium extraction slag from clay using the sulfate process.
High-value cat litter is prepared by aging clay lithium slag with calcium salts and hydroxides, followed by acidification to convert it into bentonite, and finally granulating it with deodorizers, antibacterial agents and binders.
This method achieves full utilization of lithium slag, reduces energy consumption, increases the market value and economic benefits of the product, and produces cat litter with excellent water absorption and clumping properties.
Smart Images

Figure CN119866954B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste resource utilization technology, and in particular to a method for the resource utilization of clay lithium slag and the cat litter prepared therefrom. Background Technology
[0002] With the rapid rise of the new energy storage industry represented by lithium batteries, the lithium salt industry, including lithium carbonate, lithium hydroxide, and lithium chloride, has experienced tremendous growth. However, the corresponding industrial waste, lithium slag, has been increasing year by year. Typically, the production of 1 ton of lithium salt generates 8 to 10 tons of lithium slag. In 2018, the total domestic lithium carbonate production was 125,000 tons. It is estimated that approximately 1.25 million tons of lithium slag will be discharged annually. Including the accumulated amounts over the years, the domestic lithium slag stockpile could reach tens of millions of tons. The accumulation of lithium slag will cause a large amount of land waste and environmental pollution.
[0003] At present, the relevant research on lithium slag mainly focuses on the comprehensive utilization of lithium slag, and mainly tends to be related to building materials manufacturing and other fields. However, due to the uneven level of technology, the utilization of lithium slag is not high and the utilization method is relatively low-end and inexpensive. For example, the production of lightweight ceramic plates using lithium slag includes taking raw materials such as lithium slag, feldspar, quartz powder, and alumina and dry-processing them into powder, mixing them in proportion to obtain a mixture; adding water to the mixture and stirring, granulating, drying, and sieving to obtain granules; loading the granules into a sagger, spreading them out, and firing them at high temperature, and then cooling them to obtain lightweight ceramic plates. This method has the following shortcomings: (1) It requires the lithium slag to contain more than 5.5% manganese monoxide, which is a high requirement for the content of lithium slag; (2) The high-temperature firing temperature is above 1000℃, which results in very high energy consumption and high industrial production costs. In addition, there is a method of mixing lithium slag from lithium mica smelting with an aqueous solution, and then performing multi-stage washing and pressure filtration at 40-60℃ to obtain filter cake and filtrate. After impurity removal, the high-salt purification liquid is treated by vacuum permeation evaporation and thermal permeation evaporation to precipitate potassium sulfate and sodium sulfate, respectively, to obtain industrial-grade sodium sulfate and potassium sulfate products. This method has the following shortcomings: (1) The process of multi-stage washing and filtration and multiple impurity removal is complex and cumbersome; (2) Only the sulfate in the lithium slag is recovered and utilized, and a large amount of filter residue is still produced during the recovery process, which cannot solve the problem of waste disposal. There is also a method of preparing ultra-light ceramic particles by jointly disposing of lithium slag and fly ash. This method mainly includes: mixing lithium slag, fly ash and feldspar in proportion and granulating them, and then obtaining ultra-light ceramic particles after two calcination treatments. The method has the following shortcomings: (1) It uses two calcinations at temperatures above 450℃ and above 1150℃, which result in high calcination energy consumption and high production costs; (2) The products obtained have low market value and low economic benefits.
[0004] Therefore, there is an urgent need to provide a method for treating lithium slag to solve the above problems. Summary of the Invention
[0005] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, this invention provides a method for the resource utilization of clay lithium slag and the cat litter prepared from it. This method has the advantages of low energy consumption, high added value of lithium slag, and full utilization.
[0006] Therefore, the first aspect of the present invention provides a method for the resource utilization of clay lithium slag, comprising:
[0007] Clay lithium slag and calcium salt were mixed to obtain mixture 1;
[0008] The mixture 1 and hydroxide were mixed and aged to obtain mixture 2;
[0009] The mixture 2 is acidified to obtain mixture 3, which is used to prepare cat litter.
[0010] To address the problem of unusable slag from existing sulfate-process clay lithium extraction, this invention converts muscovite and illite in the lithium slag into bentonite through calcium salt and hydroxide aging. Following acidification, a mixture 3 is obtained, primarily composed of bentonite, which can be used as cat litter, thus achieving high-value utilization of clay lithium slag. Therefore, the solution provided by this invention offers a direction for solving the waste slag treatment problem of sulfate-process clay lithium extraction, with advantages such as low energy consumption, high added value of lithium slag, and full utilization.
[0011] According to embodiments of the present invention, the calcium salt includes at least one of calcium carbonate, calcium sulfate, calcium chloride, and calcium nitrate.
[0012] According to an embodiment of the present invention, the mass ratio of the clay lithium slag to the calcium salt is 1:(0.2-1).
[0013] According to an embodiment of the present invention, the hydroxide includes at least one of sodium hydroxide and potassium hydroxide.
[0014] According to an embodiment of the present invention, the mass ratio of the mixture 1 to the hydroxide is 1:(0.3-0.6).
[0015] According to an embodiment of the present invention, the aging treatment temperature is 50℃-80℃.
[0016] According to an embodiment of the present invention, the aging treatment time is 15-45 days.
[0017] According to an embodiment of the present invention, the acidification treatment includes contacting the mixture 2 with an acidic compound to obtain the mixture 3.
[0018] According to embodiments of the present invention, the acidic compound includes at least one of sulfuric acid and hydrochloric acid.
[0019] According to an embodiment of the present invention, the acidification treatment time is 30 min to 90 min.
[0020] According to an embodiment of the present invention, the mass ratio of the clay lithium slag to the acid compound is 1:(0.8-2).
[0021] According to an embodiment of the present invention, the mixture further includes: mixing the mixture 3 with a deodorant, an antibacterial agent, and a binder, granulating the mixture to obtain a mixture 4, wherein the mixture 4 is used as cat litter.
[0022] According to an embodiment of the present invention, the deodorizer includes at least one of modified zeolite, bamboo charcoal powder, and coconut shell activated carbon.
[0023] According to embodiments of the present invention, the antibacterial agent includes at least one of pyridine aqueous dispersants and polyguanidine aqueous solutions.
[0024] According to an embodiment of the present invention, the adhesive comprises water glass.
[0025] According to an embodiment of the present invention, the mass ratio of the clay lithium slag to the deodorizer is 1:(0.03-0.15).
[0026] According to an embodiment of the present invention, the mass ratio of the clay lithium slag to the antibacterial agent is 1:(0.03-0.06).
[0027] According to an embodiment of the present invention, the mass ratio of the clay lithium slag to the binder is 1:(0.30-0.45).
[0028] According to an embodiment of the present invention, the particle size of the mixture 4 is 3mm-6mm.
[0029] According to an embodiment of the present invention, the length of the mixture 4 is 6mm-8mm.
[0030] According to an embodiment of the present invention, the mixture 3 is dried for use in preparing cat litter, or the mixture 4 is dried for use in cat litter.
[0031] According to an embodiment of the present invention, the drying temperature is 70°C-90°C.
[0032] According to an embodiment of the present invention, the particle size of the clay lithium slag is 80-200 mesh.
[0033] A second aspect of this invention provides a cat litter obtained according to the resource utilization method described in the first aspect. This cat litter exhibits excellent absorbency and clumping properties.
[0034] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0035] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0036] Figure 1 The flowchart of the resource utilization method for clay lithium slag provided by the present invention is shown. Detailed Implementation
[0037] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0038] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. Furthermore, in the description of this invention, unless otherwise stated, "a plurality of" means two or more.
[0039] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0040] To facilitate understanding of the invention, certain technical and scientific terms are specifically defined below. Unless otherwise expressly defined elsewhere in this document, all other technical and scientific terms used herein have the meanings commonly understood by one of ordinary skill in the art to which this invention pertains.
[0041] In this document, the terms “comprising” or “including” are open-ended expressions, meaning that they include the contents specified in this invention, but do not exclude other aspects.
[0042] In this document, the terms “optionally,” “optionally,” or “optionally” generally refer to an event or condition that may, but may not, occur, and the description includes both cases in which the event or condition occurs and cases in which the event or condition does not occur.
[0043] According to embodiments of the present invention, a first aspect provides a method for the resource utilization of clay lithium slag, the method comprising:
[0044] (1) Mix clay lithium slag and calcium salt to obtain mixture 1.
[0045] According to specific embodiments of the present invention, the type of calcium salt is not particularly limited, as long as it provides calcium ions to convert clay lithium slag into calcium-based bentonite. Specific examples include, but are not limited to, calcium carbonate, calcium sulfate, calcium chloride, calcium nitrate, etc., with calcium carbonate and / or calcium sulfate being preferred.
[0046] According to a specific embodiment of the present invention, the mass ratio of the clay lithium slag to the calcium salt is 1:(0.2-1), for example, 1:0.2, 1:0.4, 1:0.6, 1:0.8, 1:1, etc.
[0047] According to a specific embodiment of the present invention, the particle size of the clay lithium slag is 80-200 mesh, which can be achieved by crushing or other methods.
[0048] (2) Mix the mixture 1 with the hydroxide and age it to obtain mixture 2.
[0049] This allows the muscovite and illite in clay lithium slag to be converted into bentonite. Bentonite is a clay primarily composed of montmorillonite minerals, with each bentonite particle consisting of thousands of tiny montmorillonite crystal nanosheets. Montmorillonite crystals are composed of two layers of silicon-oxygen tetrahedra sandwiching a layer of aluminum-oxygen octahedra. A large number of exchangeable cations are adsorbed between the crystal layers. These exchangeable cations become hydrated cations upon contact with water, significantly increasing the distance between the montmorillonite crystal nanosheets. Thus, the gaps between the structural units of montmorillonite—the nanosheets—can accommodate a large number of water molecules, giving bentonite excellent water absorption properties. It can then be used as cat litter, achieving high-value utilization of clay lithium slag.
[0050] According to specific embodiments of the present invention, the type of hydroxide is not particularly limited, and some specific examples include, but are not limited to, sodium hydroxide, potassium hydroxide, etc. Sodium hydroxide is preferred.
[0051] According to a specific embodiment of the present invention, the mass ratio of mixture 1 to hydroxide is 1:(0.3-0.6), for example 1:0.3, 1:0.4, 1:0.5, 1:0.6, etc.
[0052] According to a specific embodiment of the present invention, mixture 1 and a hydroxide solution are mixed and aged to obtain mixture 2. The mass ratio of mixture 1 to hydroxide solution is 1:(0.3-0.6), for example, 1:0.3, 1:0.4, 1:0.5, 1:0.6, etc. The concentration of hydroxide solution can be 5%-15%, which can be selected by those skilled in the art as appropriate, for example, the concentration of hydroxide solution is 5%, 10%, 15%, etc.
[0053] According to specific embodiments of the present invention, the temperature and time of the aging treatment are not particularly limited, and those skilled in the art can select them as appropriate. As some specific examples, the temperature of the aging treatment is 50℃-80℃, such as 50℃, 60℃, 70℃, 80℃, etc. The aging treatment time is 15d-45d, such as 15d, 20d, 25d, 30d, 35d, 40d, 45d, etc.
[0054] (3) The mixture 2 is acidified to obtain mixture 3, which is used to prepare cat litter.
[0055] According to a specific embodiment of the present invention, the acidification treatment includes contacting the mixture 2 with an acidic compound and obtaining the mixture 3 through an acid-base neutralization reaction. The type of the acidic compound is not particularly limited, and includes, but is not limited to, sulfuric acid, hydrochloric acid, etc. Further, the acidic compound participates in the reaction in solution form. The concentrations of the sulfuric acid solution and the hydrochloric acid solution are not particularly limited. The concentration of the sulfuric acid solution can be 3%-10%, for example, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc., and the concentration of the hydrochloric acid solution can be 3%-15%, for example, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc.
[0056] According to a specific embodiment of the present invention, the acidification treatment time is 30-90 minutes, for example, 30 minutes, 60 minutes, 90 minutes, etc. The treatment is preferably carried out by stirring, and the rotation speed can be selected as needed, for example, 100 r / min-300 r / min.
[0057] According to a specific embodiment of the present invention, the mass ratio of the clay lithium slag to the acidic compound is 1:(0.8-2), for example 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, etc.
[0058] According to a specific embodiment of the present invention, the mass ratio of the clay lithium slag to the acidic compound solution is 1:(0.8-2), for example, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, etc.
[0059] According to a specific embodiment of the present invention, after acidification treatment, the sample can be filtered, dried, and then pulverized to a mesh size of 80 or higher, for example, 80-200 mesh.
[0060] According to a specific embodiment of the present invention, the method further includes: mixing the mixture 3 with a deodorant, an antibacterial agent, and a binder, granulating the mixture to obtain a mixture 4, wherein the mixture 4 is used as cat litter. For details, please refer to [link to specific process]. Figure 1 This further enhances the properties of the material.
[0061] According to specific embodiments of the present invention, the types of deodorizer, antibacterial agent, and binder are not particularly limited. The deodorizer includes, but is not limited to, bamboo charcoal powder, modified zeolite, and coconut shell activated carbon, which can not only deodorize but also enhance the water absorption and cohesion of mixture 4. The antibacterial agent includes, but is not limited to, pyridine water dispersants and polyguanidine aqueous solutions, and the binder includes, but is not limited to, water glass.
[0062] According to specific embodiments of the present invention, the mass ratio of the clay lithium slag to the deodorizer is 1:(0.03-0.15), for example, 1:0.03, 1:0.04, 1:0.05, 1:0.07, 1:0.09, 1:0.10, 1:0.11, 1:0.12, 1:0.13, 1:0.14, 1:0.15, etc. The mass ratio of the clay lithium slag to the antibacterial agent is 1:(0.03-0.06), for example, 1:0.03, 1:0.04, 1:0.05, 1:0.06, etc.
[0063] According to specific embodiments of the present invention, the mass of the binder is not particularly limited. As some specific examples, the mass ratio of the clay lithium slag to the binder can be 1:(0.30-0.45), for example 1:0.3, 1:0.32, 1:0.34, 1:0.36, 1:0.38, 1:0.39, 1:0.41, 1:0.42, 1:0.44, 1:0.45.
[0064] According to a specific embodiment of the present invention, the particle size of the mixture 4 is 3mm-6mm, such as 3mm, 4mm, 5mm, 6mm, etc. The length of the mixture 4 is 6mm-8mm, such as 6mm, 7mm, 8mm, etc. Since cat litter is mostly cylindrical, the length of the mixture 4 refers to the height of the cylinder.
[0065] According to a specific embodiment of the present invention, the method further includes: drying the mixture 3 for preparing cat litter, or drying the mixture 4 for use as cat litter. The drying temperature is not particularly limited; as some specific examples, it can be carried out at 70°C-90°C. After drying, the mixture is sieved to remove particles and dust that do not meet the particle size standard, thereby obtaining mixture 3 which can be used to prepare cat litter, or mixture 4 which can be used as cat litter.
[0066] According to embodiments of the present invention, a second aspect provides a cat litter obtained according to the resource utilization method described in the first aspect. This cat litter thus exhibits good absorbency and clumping properties.
[0067] The present invention will be explained below with reference to embodiments. Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0068] Example 1
[0069] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0070] 2. Weigh 500g of lithium slag raw material, add 200g of calcium carbonate, and mix thoroughly to obtain mixture 1;
[0071] 3. Place mixture 1 in a petri dish, slowly add 300g of 10% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 40 days to obtain mixture 2.
[0072] 4. Add 400g of 5% sulfuric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0073] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0074] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 195g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0075] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0076] Example 2
[0077] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0078] 2. Weigh 500g of lithium slag raw material, add 200g of calcium sulfate, and mix thoroughly to obtain mixture 1;
[0079] 3. Place mixture 1 in a petri dish, slowly add 300g of 10% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 40 days to obtain mixture 2.
[0080] 4. Add 400g of 5% sulfuric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0081] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0082] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 195g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0083] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0084] Example 3
[0085] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0086] 2. Weigh 500g of lithium slag raw material, add 100g of calcium carbonate and 100g of calcium sulfate, and mix thoroughly to obtain mixture 1;
[0087] 3. Place mixture 1 in a petri dish, slowly add 300g of 10% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 30 days to obtain mixture 2.
[0088] 4. Add 200g of 5% sulfuric acid solution and 200g of 10% hydrochloric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0089] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0090] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 195g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0091] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0092] Example 4
[0093] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0094] 2. Weigh 500g of lithium slag raw material, add 150g of calcium carbonate and 150g of calcium sulfate, and mix thoroughly to obtain mixture 1;
[0095] 3. Place mixture 1 in a petri dish, slowly add 300g of 10% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 30 days to obtain mixture 2.
[0096] 4. Add 200g of 5% sulfuric acid solution and 200g of 10% hydrochloric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0097] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0098] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 220g of water glass to the mixture obtained in step 5 and mix and granulate. The granulation particle size is 4mm and the length is 7mm.
[0099] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0100] Example 5
[0101] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0102] 2. Weigh 500g of lithium slag raw material, add 150g of calcium carbonate and 100g of calcium sulfate, and mix thoroughly to obtain mixture 1;
[0103] 3. Place mixture 1 in a petri dish and slowly add 350g of 10% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 30 days to obtain mixture 2.
[0104] 4. Add 300g of 5% sulfuric acid solution and 200g of 10% hydrochloric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0105] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0106] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 205g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0107] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0108] Example 6
[0109] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0110] 2. Weigh 500g of lithium slag raw material, add 150g of calcium carbonate and 100g of calcium sulfate, and mix thoroughly to obtain mixture 1;
[0111] 3. Place mixture 1 in a petri dish, slowly add 350g of 8% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 40 days to obtain mixture 2.
[0112] 4. Add 200g of 5% sulfuric acid solution and 200g of 10% hydrochloric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0113] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0114] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 205g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0115] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0116] Example 7
[0117] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0118] 2. Weigh 500g of lithium slag raw material, add 150g of calcium carbonate and 100g of calcium sulfate, and mix thoroughly to obtain mixture 1;
[0119] 3. Place mixture 1 in a petri dish and slowly add 350g of 15% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 25 days to obtain mixture 2.
[0120] 4. Add 300g of 5% sulfuric acid solution and 200g of 10% hydrochloric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0121] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0122] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 205g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0123] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0124] Example 8
[0125] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0126] 2. Weigh 500g of lithium slag raw material, add 150g of calcium carbonate and 100g of calcium sulfate, and mix thoroughly to obtain mixture 1;
[0127] 3. Place mixture 1 in a petri dish and slowly add 400g of 10% sodium hydroxide solution to mixture 1 while stirring continuously. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 25 days to obtain mixture 2.
[0128] 4. Add 400g of 5% sulfuric acid solution and 200g of 10% hydrochloric acid solution to mixture 2, and stir with a stirrer at 200r / min for 60min to acidify, to obtain mixture 3;
[0129] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0130] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 205g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0131] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0132] Comparative Example 1
[0133] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0134] 2. Weigh 500g of lithium slag raw material, add 200g of calcium carbonate, and mix thoroughly;
[0135] 3. Place the mixed material in a petri dish, slowly add 300g of 10% sulfuric acid solution and 100g of 10% hydrochloric acid solution to the mixture, stirring continuously during the process. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 30 days.
[0136] 4. Add 500g of 5% sodium hydroxide solution to the aged sample and stir with a stirrer at 200r / min for 60min to alkalize it.
[0137] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0138] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 195g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0139] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0140] Comparative Example 2
[0141] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0142] 2. Weigh 500g of lithium slag raw material, add 200g of calcium sulfate, and mix thoroughly;
[0143] 3. Place the mixed material in a petri dish, slowly add 300g of 10% sulfuric acid solution and 100g of 10% hydrochloric acid solution to the mixture, stirring continuously during the process. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 30 days.
[0144] 4. Add 500g of 5% sodium hydroxide solution to the aged sample and stir with a stirrer at 200r / min for 60min to alkalize it.
[0145] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0146] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 195g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0147] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0148] Comparative Example 3
[0149] 1. Crush the clay lithium slag and pass it through a 100-mesh sieve to obtain lithium slag raw material;
[0150] 2. Weigh 500g of lithium slag raw material, add 150g of calcium carbonate and 100g of calcium sulfate, and mix thoroughly;
[0151] 3. Place the mixed material in a petri dish, slowly add 300g of 10% sulfuric acid solution and 100g of 10% hydrochloric acid solution to the mixture, stirring continuously during the process. After stirring evenly, seal with plastic wrap and place in a 60℃ oven for aging for 30 days.
[0152] 4. Add 500g of 5% sodium hydroxide solution to the aged sample and stir with a stirrer at 200r / min for 60min to alkalize it.
[0153] 5. After acidification, filter and dry the sample. After drying, crush the sample and pass it through a 100-mesh sieve. Add 20g of modified zeolite that has passed through an 80-mesh sieve and 50g of bamboo charcoal powder and mix evenly.
[0154] 6. Add 25g of 75% fluroxypyr·thiamethoxam water dispersant and 205g of water glass to the mixture obtained in step 5 for mixing and granulation. The granulation particle size is 4mm and the length is 7mm.
[0155] 7. After granulation, place the pellets in an oven at 80°C and dry them. After drying, sieve them to remove particles and dust that do not meet the size standards, and you will get bentonite cat litter.
[0156] Test case
[0157] The components of the samples before granulation in the examples and comparative examples (corresponding to the samples obtained in step 5) were analyzed, and the following performance tests were performed on the obtained cat litter:
[0158] (1) Test method for water absorption of cat litter: Weigh 300g of cat litter sample and place it in a designated container. Gradually add 0.9% sodium chloride solution, observe its water absorption degree, and measure the water absorption amount.
[0159] (2) Test method for cat litter water absorption time: Place a certain amount of cat litter sample in a designated container, pour in a certain amount of 0.9% sodium chloride solution, and record the time required for the cat litter to completely absorb water.
[0160] (3) Cat litter clumping performance test method: The cat litter sample that has clumped together is dropped freely from a height of 1 meter above the ground. It is considered qualified if it does not break apart when it hits the ground. The test results are shown in Table 1.
[0161] Table 1
[0162]
[0163] The results show that the method provided by this invention can convert clay lithium slag into bentonite (i.e., containing montmorillonite, silica, alumina, calcium oxide, calcium nitrate, etc.), resulting in cat litter with strong and stable water absorption and good clumping strength. In Table 1, "-" indicates that the cat litter prepared in Comparative Examples 1-3 had an excessively long water absorption time.
[0164] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0165] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A method for resource utilization of clay lithium mine residue, characterized in that, include: Clay lithium slag and calcium salt were mixed to obtain mixture 1; The mixture 1 and hydroxide were mixed and aged to obtain mixture 2; The mixture 2 is acidified to obtain mixture 3, which is used to prepare cat litter; The mass ratio of the clay lithium slag to the calcium salt is 1:(0.2-1); The mass ratio of the mixture 1 to the hydroxide is 1:(0.3-0.6); The mass ratio of the clay lithium slag to the acidic compound is 1:(0.8-2); The aging process is carried out at a temperature of 50℃-80℃; The aging process takes 15-45 days. The acidification treatment time is 30 min to 90 min.
2. The method of claim 1, wherein, The calcium salt includes at least one of calcium carbonate, calcium sulfate, calcium chloride, and calcium nitrate.
3. The method of claim 1, wherein, The hydroxide includes at least one of sodium hydroxide and potassium hydroxide.
4. The resource utilization method according to claim 1, characterized in that, The acidification process includes contacting the mixture 2 with an acidic compound to obtain the mixture 3.
5. The resource utilization method according to claim 4, characterized in that, The acidic compound includes at least one of sulfuric acid and hydrochloric acid.
6. The resource utilization method according to claim 1, characterized in that, Also includes: The mixture 3 is mixed with deodorant, antibacterial agent and binder, and granulated to obtain mixture 4, which is used as cat litter.
7. The resource utilization method according to claim 6, characterized in that, The deodorizing agent includes at least one of modified zeolite, bamboo charcoal powder, and coconut shell activated carbon.
8. The resource utilization method according to claim 6, characterized in that, The antibacterial agent includes at least one of pyridine water dispersible agents and polyguanidine aqueous solutions.
9. The resource utilization method according to claim 6, characterized in that, The adhesive includes water glass.
10. The resource utilization method according to claim 6, characterized in that, The mass ratio of the clay lithium slag to the deodorizer is 1:(0.03-0.15).
11. The resource utilization method according to claim 6, characterized in that, The mass ratio of the clay lithium slag to the antibacterial agent is 1:(0.03-0.06).
12. The resource utilization method according to claim 6, characterized in that, The mass ratio of the clay lithium slag to the binder is 1:(0.30-0.45).
13. The resource utilization method according to claim 6, characterized in that, The particle size of the mixture 4 is 3mm-6mm.
14. The resource utilization method according to claim 13, characterized in that, The length of the mixture 4 is 6mm-8mm.
15. The resource utilization method according to any one of claims 1-14, characterized in that, Also includes: The mixture 3 is dried for use in the preparation of cat litter, or the mixture 4 is dried for use as cat litter.
16. The resource utilization method according to claim 15, characterized in that, The drying temperature is 70℃-90℃.
17. The resource utilization method according to claim 1, characterized in that, The particle size of the clay-lithium slag is 80-200 mesh.
18. A type of cat litter, characterized in that, The cat litter is obtained by the resource utilization method according to any one of claims 1-17.
Citation Information
Patent Citations
Lithium slag doped cat litter and preparation thereof
CN118614402A