A method for desulfurization of lithium slag through hydrothermal synergistic CO2 conversion
The hydrothermal co-conversion method for CO₂ conversion solves the problem of low desulfurization efficiency in lithium slag, achieving efficient resource utilization and carbon emission reduction of lithium slag, simplifying the operation process and reducing costs.
Patent Information
- Application Number
- CN202510076998.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-01-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-01-17
AI Technical Summary
Existing lithium slag desulfurization technologies are inefficient, costly, and complex to operate, making it difficult to achieve a synergistic effect of efficient resource utilization and environmental protection.
By adjusting the pH, temperature, and liquid-solid ratio of the slurry through particle size screening and hydrothermal reaction, a hydrothermal reaction environment is formed. CO₂ is used to treat the lithium slag desulfurization solution, and CO₂ is synergistically converted to achieve desulfurization of lithium slag and conversion of CO₂.
It improves the sulfur removal efficiency in lithium slag, retains other effective components in lithium slag, reduces processing costs, and realizes large-scale resource utilization and carbon emission reduction.
Smart Images

Figure CN119870098B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium slag treatment and solid waste resource utilization and carbon emission reduction technology, and in particular to a method for desulfurizing lithium slag through hydrothermal synergistic CO2 conversion. Background Technology
[0002] With the development of lithium resource development technology, the process of extracting lithium resources from hard-rock lithium mines using sulfate roasting is becoming increasingly common, leading to a daily increase in the discharge of sulfur-containing lithium slag. Desulfurization treatment of lithium slag can help achieve better resource utilization.
[0003] Currently, lithium slag desulfurization technologies mainly include flotation desulfurization and thermochemical desulfurization. For example, Chinese patent CN108147658B addresses the tailings from lithium extraction via the spodumene sulfuric acid process. It involves adding dispersants and collectors, followed by gravity separation, flotation, or a combination of both, to obtain pyrophyllite raw material for glass fiber after desulfurization. Patent CN114226413B first grinds the lithium slag, then performs weak magnetic separation, strong magnetic separation, and flotation to obtain sulfur-containing tailings and flotation-processed material. The desulfurized material is then processed to prepare silica-alumina micropowder. Patent CN113976309B utilizes lithium slag to comprehensively recover lithium, tantalum, niobium, silica-alumina micropowder, iron concentrate, and gypsum. It also employs flotation desulfurization after adding collectors, ultimately removing sulfur from the lithium slag raw material in the form of gypsum. In the field of thermochemical desulfurization, patent CN110482894B mixes acid-process lithium slag powder and coking coal powder, and heat-treats them at 700℃-900℃ for 100-150 minutes, achieving a desulfurization rate of up to 63.6%. The desulfurized lithium slag powder is then used to replace cement in concrete. Patent CN118026239A discloses a method for mixing lithium slag with an inorganic acidic composite reagent, followed by a catalytic dissociation reaction to obtain a desulfurized and decalcified solution and desulfurized and decalcified slag. A salt inducer is added to the desulfurized and decalcified solution, and crystallization at low temperature yields fine grains such as calcium sulfate, ultimately achieving the resource utilization of desulfurized and decalcified lithium slag.
[0004] In conclusion, with the development of lithium resources, the comprehensive utilization of lithium slag has become an urgent issue. Lithium slag desulfurization is a crucial step in the resource utilization of lithium slag, and developing efficient, low-cost, and easy-to-operate lithium slag desulfurization technologies is of great significance for environmental protection and resource recycling in lithium resource development. Summary of the Invention
[0005] The purpose of this invention is to provide a method for desulfurizing lithium slag through hydrothermal synergistic CO2 conversion. This method creates a hydrothermal reaction environment by screening particles and adjusting conditions such as slurry pH, temperature, and liquid-solid ratio to promote the removal of sulfur from lithium slag. At the same time, CO2 is used to treat the lithium slag desulfurization solution, synergistically converting CO2, thereby simultaneously achieving the process of lithium slag desulfurization and CO2 conversion.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution: Step a: The lithium slag obtained after lithium extraction from sulfate roasted lepidolite concentrate through a lithium leaching process is ground and then screened. Step b: Based on the particle size of the lithium slag after screening, prepare slurries of different particle sizes, transport them to the reactor, adjust the material-liquid ratio, and adjust the pH of the slurry. Step c: Set the reaction temperature and reaction time in the reactor, start the hydrothermal reaction, introduce CO2 gas, and stir during the reaction process; In step d, after the reaction time is over, solid-liquid separation is performed. The solid is dried to obtain desulfurized lithium slag. CO2 gas is then introduced into the separated solution to achieve solution pretreatment and CO2 co-conversion. The pretreated solution can be reused in step b.
[0007] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. By controlling the following technical parameters, the technical objectives and beneficial effects of the present invention can be better achieved.
[0008] Preferably, the particle size of the lithium slag powder after grinding in step a is 60 mesh to 250 mesh.
[0009] Preferably, the liquid used for preparing the slurry in step b is an alkaline waste liquid or an alkaline solid waste leachate such as metallurgical slag, with a material-to-liquid ratio of 1:10~30, and the pH of the adjusted slurry is 7~13.
[0010] Preferably, the reaction temperature in step c is between 20°C and 95°C, the reaction time is between 5 min and 30 min, and the stirring method is mechanical paddle stirring or electromagnetic stirring.
[0011] Preferably, the temperature of the slurry in step c can be achieved by using waste heat recovery as a heating source.
[0012] Preferably, the solid-liquid separation method in step d is sedimentation, filtration, or centrifugation.
[0013] Preferably, the CO2 gas introduced in step d is pure CO2 gas or CO2-containing industrial waste gas.
[0014] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a method for desulfurizing lithium slag through hydrothermal synergistic CO2 conversion. The method utilizes a hydrothermal reaction, and by screening the lithium slag particle size and correspondingly controlling and adjusting the pH, temperature, liquid-solid ratio, and other conditions of the slurry, a hydrothermal reaction environment is formed to promote the removal of sulfur from the lithium slag. The desulfurization solution of the lithium slag is then treated with CO2, thereby simultaneously achieving lithium slag desulfurization and CO2 conversion.
[0015] Compared with the prior art, the present invention has the following beneficial effects: (1) The method of the present invention controls the hydrothermal reaction conditions based on the lithium slag particle size, efficiently removes sulfur from the lithium slag, and retains other effective components such as calcium required for the large-scale utilization of lithium slag in the building materials field, thereby improving the added value of desulfurized lithium slag utilization.
[0016] (2) The method described in this invention can utilize alkaline solid waste such as alkaline waste liquid or metallurgical slag, and can utilize low-temperature waste heat as a heat source. At the same time, it can absorb and transform CO2-containing industrial waste gas, thereby realizing resource synergistic recycling, disposal and utilization and carbon emission reduction.
[0017] (3) The method described in this invention has a simple process flow, the process is easy to operate and control, the reaction conditions are mild, and it can also be used to treat and utilize other waste resources, thereby reducing the treatment cost and improving economic benefits while achieving good social and environmental benefits. Attached Figure Description
[0018] Figure 1 This is a process flow diagram of the hydrothermal synergistic CO2 conversion method for desulfurizing lithium slag provided by the present invention. Detailed Implementation
[0019] The technical solution of the present invention and its resulting technical effects will be further described in detail below through specific examples.
[0020] The following examples are typical but not limiting embodiments of the method described in this invention. The lithium slag used in the examples was obtained from a lithium extraction plant using the sulfate process in Jiangxi Province.
[0021] Example 1 A method for desulfurizing lithium slag through hydrothermal synergistic CO2 conversion includes the following steps: 5g of 250-mesh lithium slag was placed in a high-pressure reactor, and 100g of steel slag leaching solution was added. The pH of the solution was tested to be 11.63. The high-pressure reactor was turned on, and the temperature of the reactor was adjusted to 30℃. The reactor was stirred and reacted for 15 minutes, and CO2 gas was continuously introduced.
[0022] After the reaction was completed, the solution was filtered to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 4.16% (calculated as SO3), while the sulfur content of the original 250-mesh lithium slag sample was 14.30% (calculated as SO3), and the desulfurization rate was 70.91%.
[0023] Example 2 5g of 250-mesh lithium slag was placed in a high-pressure reactor, 150g of waste alkali solution was added, the pH of the solution was tested to be 12.72, the high-pressure reactor was turned on, the temperature of the reactor was adjusted to 90℃, and the reaction was stirred for 30 minutes, while CO2 gas was continuously introduced.
[0024] After the reaction was completed, the solution was centrifuged to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 3.49% (calculated as SO3), while the sulfur content of the original 250-mesh lithium slag sample was 14.30% (calculated as SO3), and the desulfurization rate was 75.59%.
[0025] Example 3 5g of 60-mesh lithium slag was placed in a high-pressure reactor, and 50g of steel slag leaching solution was added. The pH of the solution was tested to be 10.55. The high-pressure reactor was turned on, and the temperature of the reactor was adjusted to 60℃. The reactor was stirred and reacted for 25 minutes, while CO2 gas was continuously introduced.
[0026] After the reaction was completed, the solution was centrifuged to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 3.02% (calculated as SO3), while the sulfur content of the original 60-mesh lithium slag sample was 8.65% (calculated as SO3), and the desulfurization rate was 65.09%.
[0027] Example 4 5g of 120-mesh lithium slag was placed in a high-pressure reactor, 100g of waste alkali solution was added, the pH of the solution was tested to be 10.78, the high-pressure reactor was turned on, the temperature of the reactor was adjusted to 90℃, and the reaction was stirred for 30 minutes, while CO2 gas was continuously introduced.
[0028] After the reaction was completed, the solution was filtered to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 4.07% (calculated as SO3), while the sulfur content of the original 120-mesh lithium slag sample was 13.03% (calculated as SO3), and the desulfurization rate was 68.76%.
[0029] Example 5 5g of 200-mesh lithium slag was placed in a high-pressure reactor, 150g of waste alkali solution was added, the pH of the solution was tested to be 11.34, the high-pressure reactor was turned on, the temperature of the reactor was adjusted to 60℃, and the reaction was stirred for 30 minutes, while CO2 gas was continuously introduced.
[0030] After the reaction was completed, the solution was filtered to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 3.60% (calculated as SO3), while the sulfur content of the original 200-mesh lithium slag sample was 13.65% (calculated as SO3), and the desulfurization rate was 73.63%.
[0031] Example 6 5g of 120-mesh lithium slag was placed in a high-pressure reactor, and 50g of steel slag leaching solution was added. The pH of the solution was tested to be 10.56. The high-pressure reactor was turned on, and the temperature of the reactor was adjusted to 50℃. The reactor was stirred and reacted for 15 minutes, and CO2 gas was continuously introduced.
[0032] After the reaction was completed, the solution was filtered to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 3.94% (calculated as SO3), while the sulfur content of the original 120-mesh lithium slag sample was 13.03% (calculated as SO3), and the desulfurization rate was 69.76%.
[0033] Comparative Example 1 A method for desulfurizing lithium slag, comprising the following steps: 5g of 120-mesh lithium slag was placed in a high-pressure reactor, 150g of deionized water was added, the pH of the solution was tested to be 7.06, the high-pressure reactor was turned on, the temperature of the reactor was adjusted to 60℃, and the reaction was stirred for 120 minutes, while CO2 gas was continuously introduced.
[0034] After the reaction was completed, the solution was filtered to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 5.21% (calculated as SO3), while the sulfur content of the original 120-mesh lithium slag sample was 13.03% (calculated as SO3), and the desulfurization rate was 60.02%.
[0035] Comparative Example 2 A method for desulfurizing lithium slag, comprising the following steps: 5g of 250-mesh lithium slag was placed in a high-pressure reactor, 100g of deionized water was added, the pH of the solution was tested to be 7.11, the high-pressure reactor was turned on, the temperature of the reactor was adjusted to 90℃, and the reaction was stirred for 15 minutes.
[0036] After the reaction was completed, the solution was filtered to obtain desulfurized lithium slag solid, which was then dried. The sulfur content of the desulfurized lithium slag was tested to be 6.07% (calculated as SO3), while the sulfur content of the original 250-mesh lithium slag sample was 14.30% (calculated as SO3), and the desulfurization rate was 57.55%.
[0037] As can be seen from the above embodiments and comparative examples, the method of the present invention adjusts the pH, temperature, liquid-solid ratio, and other conditions of the slurry according to the lithium slag particle size to form a hydrothermal reaction system, thereby promoting the removal of sulfur from the lithium slag. By utilizing alkaline waste liquid or alkaline solid waste such as metallurgical slag, and using low-temperature waste heat as a heat source, it absorbs and converts CO2-containing industrial waste gas, simultaneously achieving resource synergistic recovery, disposal, and utilization, as well as carbon emission reduction. The method has a simple process flow, is easy to operate and control, has mild reaction conditions, and can synergistically dispose of and utilize other waste resources, thereby reducing treatment costs, improving economic efficiency, and showing broad application prospects.
[0038] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for desulfurizing lithium slag through hydrothermal synergistic CO2 conversion, characterized in that, Includes the following steps: Step a: The lithium slag is ground and then screened; the lithium slag is obtained by lithium extraction from sulfate roasted lepidolite concentrate through a lithium leaching process. Step b: Based on the particle size of the lithium slag after screening, use alkaline waste liquid to prepare slurries of lithium slag of different particle sizes, and transport them to the reactor. The mass ratio of lithium slag to alkaline waste liquid is 1:10~30, and the pH of the slurry is adjusted to 7~13. Step c: Set the reaction temperature and reaction time in the reactor, start the hydrothermal reaction, introduce CO2 gas, and stir during the reaction process; Step d: After the reaction time is over, solid-liquid separation is performed. The solid is dried to obtain desulfurized lithium slag. CO2 gas is continued to be introduced into the solution after separation to achieve solution pretreatment and CO2 co-conversion. The pretreated solution can be reused in step b. In step a, the particle size of the lithium slag after grinding is 60 mesh to 250 mesh; The reaction temperature in step c is between 20℃ and 95℃, the reaction time is between 5 min and 30 min, and the stirring method is mechanical paddle stirring or electromagnetic stirring. The solid-liquid separation method described in step d is sedimentation, filtration, or centrifugation; The CO2 gas introduced in step d is pure CO2 gas or industrial waste gas containing CO2.
Citation Information
Patent Citations
A method for high-value comprehensive utilization of lithium slag
CN108147658B
A desulfurization method for acid-process lithium slag powder and its application.
CN110482894B
A method for the comprehensive recovery of lithium, tantalum, niobium, silica-alumina powder, iron concentrate and gypsum from lithium slag
CN113976309B
A comprehensive treatment process for lithium slag
CN114226413B
Method for preparing high-purity calcium sulfate by desulfurizing and decalcifying lithium slag
CN118026239A