Glass restoration method from organic material

By using cleaning, gradual grinding, and polishing methods, the scratch and aging problems of glass made of organic materials were solved, achieving efficient repair and improved light transmittance.

CN119871164BActive Publication Date: 2026-11-24BEIJING MINGCHE INFORMATION TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510257865.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-05
Publication Date
2026-11-24
Estimated Expiration
2045-03-05

AI Technical Summary

Technical Problem

In existing technologies, scratches and aging problems of glass made of organic materials are difficult to repair effectively. Chemical fumigation accelerates aging, while ordinary grinding results in poor light transmittance.

Method used

After cleaning with cleaning solution, use sandpaper and abrasives of different grits to gradually polish and grind the surface. The first abrasive removes stains and aged surface layer, the second abrasive removes sandpaper marks, and the third abrasive removes glare.

Benefits of technology

It effectively removes scratches and aging damage from organic glass, improves light transmittance, avoids secondary damage, and restores the mirror effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119871164B_ABST
    Figure CN119871164B_ABST
Patent Text Reader

Abstract

This invention provides a method for repairing glass made of organic materials, comprising: cleaning with a cleaning solution to remove surface stains; performing a first polishing treatment with a first abrasive to remove residual stains and aged surface layers; polishing with sandpaper of different grits in ascending order of grit; performing a second polishing treatment with a second abrasive to remove sanding marks; and performing a third polishing treatment with a third abrasive to remove glare and restore a mirror finish. The method of this invention can improve the repair effect and efficiency of glass made of organic materials, thereby enhancing its appearance and extending its service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of glass repair technology using organic materials, and particularly to a method for glass repair using organic materials. Background Technology

[0002] Organic glass is made from polymerized high-molecular compounds, making its surface highly susceptible to scratches. This scratches break the surface molecular chains, increasing the difficulty of repair. Repair methods for organic glass include chemical fumigation and ordinary grinding. However, chemical fumigation is less effective for severely aged areas, especially those with deep cracks, as it damages the internal molecular chains and accelerates the aging process, leading to rapid yellowing. Ordinary grinding, typically using sandpaper, can result in poor light transmittance after treatment. Summary of the Invention

[0003] This invention provides a method for repairing glass made of organic materials, which can at least solve some of the above-mentioned technical problems existing in the prior art.

[0004] In a first aspect, embodiments of the present invention provide a method for repairing glass made of organic materials, comprising:

[0005] Clean with a cleaning solution to remove surface stains;

[0006] The first polishing treatment is performed with the first abrasive to remove residual stains and aged surface layers;

[0007] Use sandpaper of different grits to sand in order of increasing grit;

[0008] A second polishing process is performed using a second abrasive to remove sanding marks formed by sandpaper sanding;

[0009] A third polishing process is performed using a third abrasive to remove glare patterns.

[0010] In an optional embodiment, in the first polishing process, the polishing machine rotates at a speed of 1500-2000 rpm, the polishing disc is a short wool disc, and the polishing disc maintains a 15-degree angle with the glass surface.

[0011] In an optional embodiment, the first abrasive comprises the following components by mass percentage:

[0012] Silicon carbide 9.70%-9.55%, alumina 11.20%-11.05%, silica 9.45%-9.30%, cleaning agent 1.70%-2.10%, rust remover 1.90%-2.10%, lubricant 2.40%-2.55%, emulsifier 1.90%-2.10%, thickener 0.95%-1.10%, pH adjuster 0.45%-0.55%, balance is deionized water.

[0013] In an optional embodiment, sanding is performed using sandpaper of different grits, in ascending order of grit, including:

[0014] For deep scratches, use 600-grit wet sandpaper to sand along the scratch lines;

[0015] Use 1500-grit sandpaper to completely cover the 600-grit sandpaper marks during sanding;

[0016] Use 2000-grit sandpaper to completely cover the 1500-grit sandpaper marks during sanding.

[0017] In an optional embodiment, when sanding with 1500-grit sandpaper and 2000-grit sandpaper, sand back and forth along the horizontal or vertical direction.

[0018] In an optional embodiment, the second abrasive comprises the following components by mass percentage:

[0019] The abrasive particles comprise 16%-22%, rust remover 1.00%-1.40%, lubricant 1.25%-1.70%, emulsifier 1.00%-1.40%, thickener 0.50%-0.70%, pH adjuster 0.25%-0.35%, with the balance being deionized water. The abrasive particles include silicon carbide and alumina.

[0020] In an optional embodiment, the mass percentage of the abrasive particles in the second abrasive is as follows: silicon carbide 8.75%-9.50% and alumina 10.50%-11.25%.

[0021] In an optional embodiment, in the second polishing process, an eccentric polishing machine is used, and a long wool disc is used as the polishing disc. During the polishing process, the applied pressure reduces the thickness of the long wool disc by 1 / 3, and a grid-shaped polishing trajectory is used, with alternating horizontal and vertical polishing.

[0022] In an optional embodiment, the third abrasive comprises the following components by mass percentage:

[0023] Silicon carbide 9.70%-10.30%, alumina 11.50%-12.00%, silicon dioxide 9.50%-10.50%, rust remover 1.90%-2.10%, lubricant 2.40%-2.55%, emulsifier 1.90%-2.10%, thickener 0.95%-1.10%, pH adjuster 0.45%-0.55%, balance is deionized water.

[0024] In an optional embodiment, the third polishing process employs a figure-eight polishing trajectory, and the glass surface temperature is controlled below 60°C during the polishing process.

[0025] One embodiment of the present invention has the following advantages or beneficial effects:

[0026] In the method for repairing glass made of organic materials according to embodiments of the present invention, a cleaning solution is used to clean the surface to remove stains; a first polishing treatment is performed with a first abrasive to remove residual stains and aged surface layers; sandpaper of different grits is used to polish the glass in ascending order of grit; a second polishing treatment is performed with a second abrasive to remove sanding marks; and a third polishing treatment is performed with a third abrasive to remove glare. The method of this embodiment of the present invention uses a combination of polishing and grinding to repair glass made of organic materials, and employs different abrasives to perform multiple polishing treatments on the glass, repairing scratches, aging, and other damage to the surface of the glass, and improving the light transmittance after repair. Attached Figure Description

[0027] The above and other features and advantages of the present invention will become more apparent from a detailed description of exemplary embodiments thereof with reference to the accompanying drawings.

[0028] Figure 1 This is a schematic flowchart illustrating a method for repairing glass made of organic materials according to an exemplary embodiment;

[0029] Figures 2-6 These are images of the samples after the second polishing treatment according to Example 1 and Comparative Examples 4-7. Detailed Implementation

[0030] Exemplary embodiments will now be described more fully with reference to the accompanying drawings. However, these exemplary embodiments can be implemented in many forms and should not be construed as limited to the embodiments set forth herein; rather, they are provided so that the invention will be thorough and complete, and the concept of the exemplary embodiments will be fully conveyed to those skilled in the art. The same reference numerals in the drawings denote the same or similar structures, and therefore their detailed description will be omitted.

[0031] The terms “a,” “one,” “the,” and “the” are used to indicate the existence of one or more elements / components / etc.; the terms “including” and “having” are used to indicate an open-ended meaning of inclusion and that other elements / components / etc. may exist in addition to the listed elements / components / etc.

[0032] See Figure 1 This invention provides a method for repairing glass made of organic materials, comprising:

[0033] Clean with a cleaning solution to remove surface stains;

[0034] The first polishing treatment is performed with the first abrasive to remove residual stains and aged surface layers;

[0035] Use sandpaper of different grits to sand in order of increasing grit;

[0036] A second polishing process is performed using a second abrasive to remove sanding marks formed by sandpaper sanding;

[0037] A third polishing process is performed using a third abrasive to remove glare patterns.

[0038] In the organic material glass repair method of this invention, cleaning with a cleaning solution removes surface stains and prevents large dust particles from damaging the glass surface during subsequent processing. A first polishing treatment with a first abrasive removes residual stains and aged surface layers. Stubborn stains and aged surface layers remaining after cleaning can be removed through the first polishing treatment, laying the foundation for subsequent repairs and preventing new damage caused by residual stubborn stains and aged surface layers during sanding. In this invention, sanding with sandpaper of different grits, in ascending order of grit, removes surface scratches and improves surface smoothness. In this invention, a second polishing treatment with a second abrasive removes sanding marks, and a third polishing treatment with a third abrasive removes glare and restores a mirror-like effect. The method of this invention uses a combination of polishing and grinding to repair glass made of organic materials. Different abrasives are used to polish the glass made of organic materials multiple times to repair scratches, aging and other damage on the surface of the glass made of organic materials, and to improve the light transmittance after repair.

[0039] In some embodiments, a glass-specific cleaning solution made of organic materials is used for thorough cleaning. The cleaning solution can remove stains such as oil and dust, ensuring that no large dust particles cause secondary scratches during subsequent processing.

[0040] When cleaning glass made of organic materials, a pre-cleaning process can be performed first, followed by spraying a cleaning solution. Pre-cleaning can involve rinsing with clean water. When spraying the cleaning solution, it can be sprayed evenly from top to bottom, and then wiped from left to right using a cleaning bear paw glove. Then rinse. The rinsing sequence can be from top to bottom, moving in one direction. Ensure the cleaning solution is rinsed thoroughly. In practice, the cleaning solution can use neutral nano-active factors, which can easily dissolve various stubborn stains and remove more than 90% of stains. Ultrasonic cleaning or other methods can also be used in the cleaning process.

[0041] In some embodiments, during the first polishing process, the polishing machine rotates at 1500-2000 rpm, a short-wool polishing disc is used, and the polishing disc is held at a 15-degree angle to the glass surface. Using the first abrasive and the above polishing process, stubborn stains, fine scratches, and aged surface layers can be removed. A handheld polishing machine can be used. Applying appropriate pressure during polishing, maintaining a 15-degree angle between the polishing disc and the glass surface, and operating at a speed of 1500-2000 rpm are effective in removing stubborn stains, fine scratches, and aged surface layers.

[0042] In some embodiments, the first abrasive includes first abrasive particles and a cleaning agent. The mass percentage of the first abrasive particles in the first abrasive can be 29.9%-30.3%, and the mass percentage of the cleaning agent can be 1.7%-2.1%. Through the combination of the first abrasive particles and the cleaning agent, stubborn stains, minor scratches, and aged surfaces can be effectively removed.

[0043] The first abrasive particles may include silicon carbide, aluminum oxide, and silicon oxide.

[0044] The first abrasive may also include appropriate amounts of rust remover, lubricant, emulsifier, thickener and pH adjuster.

[0045] In some embodiments, the first abrasive comprises the following components by weight percentage: silicon carbide 9.70%-9.55%, alumina 11.20%-11.05%, silica 9.45%-9.30%, cleaning agent 1.70%-2.10%, rust remover 1.90%-2.10%, lubricant 2.40%-2.55%, emulsifier 1.90%-2.10%, thickener 0.95%-1.10%, pH adjuster 0.45%-0.55%, with the balance being deionized water. In these embodiments of the invention, a reasonable formulation balances the efficiency and effectiveness of the first polishing treatment.

[0046] The particle size of silicon carbide and alumina can be 0.5-1 μm. Both silicon carbide and alumina can be high-purity, low-metal-ion types, with uniform particle size. The particle size of silicon oxide can be 30-80 nm. High-purity colloidal microparticles are used, with spherical particles, concentrated particle size, and uniform particle size.

[0047] When repairing glass made of organic materials, the first abrasive of this invention can efficiently remove stubborn stains, as well as minor scratches and aged surfaces, without causing secondary damage to the glass.

[0048] The preparation process of the first abrasive may include the following steps: weighing each component according to the proportions; adding the proportioned components to deionized water using a high-speed disperser to fully blend and homogenize the raw materials, thereby obtaining a polishing emulsion. When adding each component, different temperatures and methods of addition can be used according to the chemical and physical properties of each component.

[0049] In some embodiments, polishing with sandpaper of different grits may include: when the glass surface has deep scratches, polishing the deep scratches with 600-grit wet sandpaper. Polishing with sandpaper of different grits may also include polishing with 1500-grit sandpaper and 2000-grit sandpaper respectively. A glass surface is considered to have deep scratches when the scratch depth is greater than a target value. The target value can range from 30μm to 80μm. Specific target values ​​can be 40μm, 50μm, 60μm, or 70μm. For example, when the glass surface has scratches deeper than 30μm, it indicates that the glass surface has deep scratches, and 600-grit wet sandpaper can be used to polish the glass surface.

[0050] When sanding with sandpaper of different grits, the sanding in the later stages should completely cover the sanding marks left by the previous sanding.

[0051] In some embodiments, sanding is performed using sandpaper of different grits, in ascending order of grit, including:

[0052] For deep scratches, use 600-grit wet sandpaper to sand along the scratch lines;

[0053] Use 1500-grit sandpaper to completely cover the 600-grit sandpaper marks during sanding;

[0054] Use 2000-grit sandpaper to completely cover the 1500-grit sandpaper marks during sanding.

[0055] Using 600-grit wet sandpaper along the scratch lines can remove deeper scratches. Using 1500-grit and 2000-grit sandpaper in sequence can eliminate sandpaper marks from previous sanding and improve surface smoothness.

[0056] When using 600-grit wet sandpaper for sanding, you can use either manual sanding or a polishing machine.

[0057] When sanding with 1500-grit and 2000-grit sandpaper, a polishing machine can be used. For example, a polishing machine with a 6-8 inch sandpaper disc can be used with 1500-grit and 2000-grit sandpaper respectively.

[0058] In some embodiments, when sanding with 1500-grit or 2000-grit sandpaper, sanding is performed back and forth in a horizontal or vertical direction. Back and forth sanding in a horizontal or vertical direction can achieve better sanding results than circular sanding.

[0059] In some embodiments, the second abrasive comprises the following components by mass percentage:

[0060] The mixture consists of 16%-22% abrasive particles, 1.00%-1.40% rust remover, 1.25%-1.70% lubricant, 1.00%-1.40% emulsifier, 0.50%-0.70% thickener, 0.25%-0.35% pH adjuster, and the balance being deionized water. The abrasive particles include silicon carbide and alumina. Polishing with a second abrasive effectively removes sanding marks and avoids the formation of noticeable fiber marks on the glass surface.

[0061] In some embodiments, the mass percentage of abrasive particles in the second abrasive is as follows: silicon carbide 8.75%-9.50% and alumina 10.50%-11.25%. A reasonable ratio of silicon carbide and alumina can achieve better polishing effect and efficiency.

[0062] The particle size of silicon carbide and alumina can be 3.5-5μm. Silicon carbide and alumina can be high-purity, low-metal-ion type, with uniform particle size.

[0063] The preparation process of the second abrasive may include the following steps: weighing each component according to the proportions; adding the proportioned components to deionized water using a high-speed disperser to fully blend and homogenize the raw materials, thereby obtaining a polishing emulsion. Different temperatures and addition methods can be used when adding each component, depending on its chemical and physical properties.

[0064] In some embodiments, in the second polishing process, an eccentric polishing machine is used, the polishing disc is a long wool disc, and during the polishing process, the applied pressure reduces the thickness of the long wool disc by 1 / 3, and a grid-shaped polishing trajectory is used, with horizontal and vertical polishing alternating.

[0065] In some embodiments, the third abrasive comprises the following components by mass percentage:

[0066] The abrasive comprises 9.70%-10.30% silicon carbide, 11.50%-12.00% alumina, 9.50%-10.50% silicon oxide, 1.90%-2.10% rust remover, 2.40%-2.55% lubricant, 1.90%-2.10% emulsifier, 0.95%-1.10% thickener, 0.45%-0.55% pH adjuster, and the balance being deionized water. The third abrasive of this invention can efficiently remove residual polishing marks and glare, and also avoids fiber marks caused by the polishing pad.

[0067] The particle size of silicon carbide and alumina can be 0.5-1 μm. Both silicon carbide and alumina can be high-purity, low-metal-ion type, with uniform particle size. The particle size of silicon oxide can be 30-80 nm. Silicon oxide can be high-purity colloidal microparticles, with spherical particles, concentrated particle size, and uniform particle size.

[0068] The preparation process of the third abrasive may include the following steps: weighing each component according to the proportions; adding the proportioned components to deionized water using a high-speed disperser to ensure thorough mixing and homogenization of the raw materials, thereby obtaining a polishing emulsion. Different temperatures and addition methods can be used when adding each component, depending on its chemical and physical properties.

[0069] In some embodiments, the third polishing process employs a figure-eight polishing trajectory, and the glass surface temperature is controlled below 60°C during the polishing process.

[0070] In this embodiment of the invention, the raw materials for each abrasive can be commercially available materials. Specifically, the cleaning agent can be, for example, sodium dioctyl sulfosuccinate, the rust remover can be triethanolamine borate, the lubricant can be glycerol, the emulsifier can be polyacrylamide, the thickener can be amine oxide, and the pH adjuster can be sodium tripolyphosphate.

[0071] The organic materials used to make glass in this invention include PMMA, PC, PETG, etc.

[0072] The embodiments of the present invention will be described below with reference to specific examples, comparative examples, and related tests. The raw materials used in the following embodiments and comparative examples are described below:

[0073] Silicon carbide, Shanghai Jinxindun Metal Materials Technology Co., Ltd., models: 500 nanometer silicon carbide 100g; 1 micrometer silicon carbide 1 kg; 3.5-5 micrometer silicon carbide 1 kg.

[0074] Alumina, Shanghai Jinxindun Metal Materials Technology Co., Ltd., models: 500 nanometer alumina 1 kg; 1 micrometer alumina 1 kg; 3.5-5 micrometer alumina 1 kg.

[0075] Silica, Hubei Huifu E-commerce Co., Ltd., Model: HL-450, 10 kg, Particle size 45 nanometers.

[0076] Sodium dioctyl sulfonate, Shanghai Huijun Chemical Co., Ltd., Model: OT-75.

[0077] Triethanolamine borate, Dexu New Materials (Guangzhou) Co., Ltd., Model: DX621.

[0078] Glycerol, Shandong Defa Chemical Co., Ltd., Model: Glyceryl Glycerol 011.

[0079] Polyacrylamide, Henan Saike Environmental Protection Technology Co., Ltd., Model: Ionic, 25 kg.

[0080] Amine oxide, Zhengzhou Juepai Chemical Products Co., Ltd., Model: LAO-30.

[0081] Sodium tripolyphosphate, Anhui Weimao Biotechnology Co., Ltd., Model: STPP, 25 kg.

[0082] Example 1

[0083] Using glass (PMMA, polymethyl methacrylate) from cable car cabins that have been in use for more than 10 years as a base, the base is cut into several pieces of the same size as templates.

[0084] Step 1: Cleaning

[0085] Rinse the sample surface with clean water, then spray with a neutral nano-active agent solution, spraying evenly from top to bottom. Next, use a cleaning bear paw glove to wipe from left to right, followed by rinsing. The rinsing sequence is from top to bottom, moving in one direction.

[0086] Step 2, First Polishing Treatment

[0087] Weigh out 9.65% silicon carbide, 11.15% alumina, 9.40% silicon oxide, 1.80% cleaning agent, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster by mass percentage. Add the weighed components to the deionized water using a high-speed disperser to fully blend and homogenize the raw materials, forming a polishing emulsion. The resulting first polishing agent has a total mass of 1 kg. The silicon carbide uses two particle sizes, 0.5 μm and 1 μm, with a mass ratio of 1:1. The alumina has a particle size of 1 μm, and the silicon oxide has a particle size of 45 nm.

[0088] The polishing machine operates at 1500-2000 rpm, using a short-wool polishing disc. At the start of polishing, the polishing disc should be held at a 15-degree angle to the glass surface. Appropriate downward pressure should be applied during polishing. The polishing time is 3 minutes.

[0089] Step 3, First Polishing

[0090] For deep scratches, use a small-diameter polisher with 600-grit wet sandpaper to carefully polish along the scratch lines. Maintain consistent pressure and direction to effectively remove the scratches while minimizing the spread and creating a smooth surface.

[0091] Step 4, Second Polishing

[0092] Use a polishing machine with a 6-8 inch sandpaper disc and 1500 grit sandpaper. Polish horizontally or vertically back and forth to completely cover the 600 grit sandpaper marks.

[0093] Step 5, Third Polishing

[0094] Use a polishing machine with a 6-8 inch sandpaper disc and 2000 grit sandpaper. Polish horizontally or vertically back and forth to completely cover the 1500 grit sandpaper marks.

[0095] Step Six: Second Polishing Process

[0096] Weigh out 6.25% silicon carbide, 13.75% alumina, 75.00% deionized water, 1.25% rust remover, 1.56% lubricant, 1.25% emulsifier, 0.63% thickener, and 0.31% pH adjuster by weight percentage. Add the weighed components to the deionized water using a high-speed disperser to fully blend and homogenize the raw materials, forming a polishing emulsion. This yields a second polishing agent with a total mass of 1 kg, containing silicon carbide particles of 5 μm and alumina particles of 5 μm.

[0097] Using an eccentric polisher with a long wool pad, remove sandpaper marks and polishing streaks left from previous processes. Apply a small amount of the second polishing compound each time during polishing, adding it multiple times to avoid dry polishing. Polish for three minutes. Apply appropriate downward pressure during polishing, reducing the thickness of the long wool pad by one-third. This maximizes the contact area between the polishing pad and the glass, resulting in the highest efficiency. Use a crisscross polishing pattern, first horizontally then vertically, alternating between horizontal and vertical passes several times to remove sandpaper marks.

[0098] Step 7, Third Polishing Process

[0099] Weigh out 10.25% silicon carbide, 11.75% alumina, 10% silicon oxide, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster by weight percentage. Add the weighed components to the deionized water using a high-speed disperser to fully blend and homogenize the raw materials, forming a polishing emulsion. This yields a third polishing agent with a total mass of 1 kg, wherein the silicon carbide particle size is 1 μm, the alumina particle size is 1 μm, and the silicon oxide particle size is 45 nm.

[0100] Use an eccentric polisher with a short wool pad and a third polishing compound to remove glare and haze, restoring the mirror-like effect of the acrylic glass. During polishing, use a figure-eight polishing path, first polishing horizontally in a figure-eight pattern, then vertically in a figure-eight pattern, to remove glare. Polish for three minutes. During polishing, keep the glass surface temperature below 60℃ to avoid surface gelling and capillary cracks caused by excessive temperature.

[0101] Step 8: Inspect the surface condition of the glass made of organic materials, checking for scratches, sand marks, glare, etc., and whether the light transmittance meets the standards.

[0102] Example 2

[0103] The difference from Example 1 is that in step two, the particle size of silicon carbide is 0.5 μm, the particle size of alumina is 1 μm, and the particle size of silicon oxide is 45 nm. In step six, the second polishing agent is composed of 72.5 g silicon carbide, 127.5 g alumina, 750 g deionized water, 12.5 g rust remover, 15.6 g lubricant, 12.5 g emulsifier, 6.3 g thickener, and 3.1 g pH adjuster. The polishing time is 15 minutes.

[0104] Example 3

[0105] The difference from Example 1 is that in step six, the second polishing agent is composed of 82.5g silicon carbide, 117.5g alumina, 750g deionized water, 12.5g rust remover, 15.6g lubricant, 12.5g emulsifier, 6.3g thickener, and 3.1g pH adjuster. The polishing time is 15 minutes.

[0106] Example 4

[0107] The difference from Example 1 is that in step six, the second polishing agent is composed of 92.5g silicon carbide, 107.5g alumina, 750g deionized water, 12.5g rust remover, 15.6g lubricant, 12.5g emulsifier, 6.3g thickener, and 3.1g pH adjuster. The polishing time is 15 minutes.

[0108] Comparative Example 1

[0109] The difference from Example 1 is that in step two, the first polishing agent is composed of 10.00% silicon carbide, 11.50% aluminum oxide, 9.75% silicon oxide, 0.75% cleaning agent, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener and 0.50% pH adjuster, resulting in a first polishing agent with a total mass of 1 kg.

[0110] Comparative Example 2

[0111] The difference from Example 1 is that in step two, the first polishing agent is composed of 9.90% silicon carbide, 11.40% aluminum oxide, 9.65% silicon oxide, 1.05% cleaning agent, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster, resulting in a first polishing agent with a total mass of 1 kg.

[0112] Comparative Example 3

[0113] The difference from Example 1 is that in step two, the first polishing agent is composed of 9.75% silicon carbide, 11.25% aluminum oxide, 9.50% silicon oxide, 1.50% cleaning agent, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster, resulting in a first polishing agent with a total mass of 1 kg.

[0114] Comparative Example 4

[0115] The difference from Example 1 is that in step six, the second polishing agent is composed of 10.00% silicon carbide, 22.00% alumina, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster, resulting in a second polishing agent with a total mass of 1 kg.

[0116] Comparative Example 5

[0117] The difference from Example 1 is that in step six, the second polishing agent is composed of 8.75% silicon carbide, 19.25% alumina, 65.00% deionized water, 1.75% rust remover, 2.19% lubricant, 1.75% emulsifier, 0.88% thickener, and 0.43% pH adjuster, resulting in a second polishing agent with a total mass of 1 kg.

[0118] Comparative Example 6

[0119] The difference from Example 1 is that in step six, the second polishing agent is composed of 7.50% silicon carbide, 16.50% alumina, 70.00% deionized water, 1.50% rust remover, 1.88% lubricant, 1.50% emulsifier, 0.75% thickener, and 0.37% pH adjuster, resulting in a second polishing agent with a total mass of 1 kg.

[0120] Comparative Example 7

[0121] The difference from Example 1 is that in step six, the second polishing agent is composed of 5.00% silicon carbide, 11.00% alumina, 80% deionized water, 1.00% rust remover, 1.25% lubricant, 1.00% emulsifier, 0.50% thickener, and 0.25% pH adjuster, resulting in a second polishing agent with a total mass of 1 kg.

[0122] Comparative Example 8

[0123] The difference from Example 1 is that in step seven, the third polishing agent is composed of 9.25% silicon carbide, 10.75% aluminum oxide, 12% silicon oxide, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster, resulting in a third polishing agent with a total mass of 1 kg.

[0124] Comparative Example 9

[0125] The difference from Example 1 is that in step seven, the third polishing agent is composed of 10.25% silicon carbide, 12.75% aluminum oxide, 9% silicon oxide, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster, resulting in a third polishing agent with a total mass of 1 kg.

[0126] Comparative Example 10

[0127] The difference from Example 1 is that in step seven, the third polishing agent is composed of 11.25% silicon carbide, 13.75% aluminum oxide, 5% silicon oxide, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster, resulting in a third polishing agent with a total mass of 1 kg.

[0128] Comparative Example 11

[0129] The difference from Example 1 is that in step seven, the third polishing agent is composed of 9.25% silicon carbide, 10.75% alumina, 12% polycrystalline diamond, 60.00% deionized water, 2.00% rust remover, 2.50% lubricant, 2.00% emulsifier, 1.00% thickener, and 0.50% pH adjuster, resulting in a third polishing agent with a total mass of 1 kg.

[0130] Comparative Example 12

[0131] The difference from Example 1 is that the first polishing process in step two is missing.

[0132] Comparative Example 13

[0133] The difference from Example 1 is that the second polishing process in step six is ​​missing.

[0134] The samples obtained after the first polishing treatment in Examples 1-2 and Comparative Examples 1-3 were observed and compared.

[0135] Check the sample for any oil stains or other dirt residue and compare it with the changes before polishing, dividing it into 5 levels: very obvious, obvious, average, not obvious, and no change.

[0136] The comparison results are shown in Table 1 below.

[0137] Table 1

[0138]

[0139] The comparative results show that the difference before and after the first polishing treatment in Examples 1 and 2 is very obvious. Stubborn stains and oil stains were completely removed, and no secondary damage was caused to the glass substrate. In contrast, Comparative Examples 1-3 showed obvious stain residue after the first polishing treatment, indicating a poor first polishing effect.

[0140] The samples from Example 1 and Comparative Examples 4-7 that underwent the second polishing treatment were observed and compared. The approximate number of fiber marks left on the samples was checked and rated as: many, more, few, less, none.

[0141] See Figures 2 to 6 , Figures 2 to 5 These are the samples after the second polishing treatment, as shown in Comparative Examples 4-7. Figure 6 This is the sample after the second polishing treatment in Example 1.

[0142] The comparison results are shown in Table 2 below.

[0143] Table 2

[0144] model Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Example 1 Fiber Stain Rating many More few none none

[0145] The comparative test results showed that the samples in Comparative Examples 4-6 had obvious fiber marks, while Comparative Example 7, although not showing obvious fiber marks, still had sand marks that had not been completely removed. Example 1 showed the best results, effectively removing sand marks and leaving no obvious fiber marks.

[0146] In Examples 2-4, the thickness of the samples after the second polishing treatment was measured using a thickness gauge before and after grinding. The measurement results are shown in Table 3.

[0147] Table 3

[0148] model Example 2 Example 3 Example 4 Thickness before grinding 3892.14um 3890.18um 3890.20um Thickness after grinding 3892.13um 3890.17um 3890.17um Difference (cutting amount) 0.01um 0.01um 0.03um

[0149] Comparative test results show that the sanding marks on the samples of Examples 2-4 were basically removed. Furthermore, Example 4 left no long wool fiber marks and had the smallest thickness, indicating that this formula has the strongest cutting force.

[0150] The transmittance of the samples after the third polishing treatment in Example 1 and Comparative Examples 8-11 was measured using a transmittance meter. The measurement results are shown in Table 4.

[0151] Table 4

[0152] model Example 1 Comparative Example 8 Comparative Example 9 Comparative Example 10 Comparative Example 11 Before polishing 70 69 69 69 70 After polishing 90 83 85 80 77

[0153] Comparative test results show that the sample obtained by Example 1 not only achieves a mirror effect, but also has the best light transmittance.

[0154] A comparison of the repaired samples from Example 1 and Comparative Example 12 reveals that, due to the lack of a first polishing treatment, the sample in Comparative Example 12, after sanding, has more surface scratches compared to the sample in Example 1 after sanding. Subsequent second and third polishing treatments are less effective at removing newly generated scratches.

[0155] By comparing the repaired samples of Example 1 and Comparative Example 13, it can be seen that, due to the lack of a second polishing treatment, the surface sand marks of the sample of Comparative Example 13 after the third polishing treatment were not completely removed compared to the sample of Example 1 after the third polishing treatment.

[0156] In this embodiment of the invention, the term "multiple" refers to two or more, unless otherwise explicitly defined. The terms "install," "connect," and "fix" should be interpreted broadly. For example, "connect" can mean a fixed connection, a detachable connection, or an integral connection. Those skilled in the art can understand the specific meaning of the above terms in this embodiment of the invention based on the specific circumstances.

[0157] In the description of the embodiments of the present invention, it should be understood that the terms "upper" and "lower" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or unit referred to must have a specific orientation or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of the present invention.

[0158] In the description of this specification, the terms "an embodiment," "a preferred embodiment," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0159] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. For those skilled in the art, the embodiments of the present invention can have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the embodiments of the present invention should be included within the protection scope of the embodiments of the present invention.

Claims

1. A method for repairing glass made of organic materials, characterized in that, include: Clean with a cleaning solution to remove surface stains; The first polishing treatment is performed with the first abrasive to remove residual stains and aged surface layers; Use sandpaper of different grits to sand in order of increasing grit; A second polishing process is performed using a second abrasive to remove sanding marks formed by sandpaper sanding; A third polishing process is performed using a third abrasive to remove glare patterns; The first abrasive comprises the following components by mass percentage: silicon carbide 9.55%-9.70%, alumina 11.05%-11.20%, silicon oxide 9.30%-9.45%, cleaning agent 1.70%-2.10%, rust remover 1.90%-2.10%, lubricant 2.40%-2.55%, emulsifier 1.90%-2.10%, thickener 0.95%-1.10%, pH adjuster 0.45%-0.55%, with the balance being deionized water; the particle size of the silicon carbide and alumina is 0.5-1 μm, and the particle size of the silicon oxide is 30-80 nm; The second abrasive comprises the following components by mass percentage: 16%-22% abrasive particles, 1.00%-1.40% rust remover, 1.25%-1.70% lubricant, 1.00%-1.40% emulsifier, 0.50%-0.70% thickener, 0.25%-0.35% pH adjuster, with the balance being deionized water. The abrasive particles comprise silicon carbide and alumina. The mass percentage of the abrasive particles in the second abrasive is as follows: 8.75%-9.50% silicon carbide and 10.50%-11.25% alumina. The particle size of the silicon carbide and the alumina is 3.5-5 μm. The third abrasive comprises the following components by mass percentage: silicon carbide 9.70%-10.30%, alumina 11.50%-12.00%, silicon oxide 9.50%-10.50%, rust remover 1.90%-2.10%, lubricant 2.40%-2.55%, emulsifier 1.90%-2.10%, thickener 0.95%-1.10%, pH adjuster 0.45%-0.55%, with the balance being deionized water; the particle size of the silicon carbide and alumina is 0.5-1 μm, and the particle size of the silicon oxide is 30-80 nm.

2. The method for repairing glass using organic materials according to claim 1, characterized in that, In the first polishing process, the polishing machine rotates at 1500-2000 rpm, the polishing disc is a short wool disc, and the polishing disc is kept at a 15-degree angle to the glass surface.

3. The method for repairing glass made of organic materials according to claim 1, characterized in that, Use sandpaper of different grits, and sand in order of increasing grit, including: For deep scratches, use 600-grit wet sandpaper to sand along the scratch lines; Use 1500-grit sandpaper to completely cover the 600-grit sandpaper marks during sanding; Use 2000-grit sandpaper to completely cover the 1500-grit sandpaper marks during sanding.

4. The method for repairing glass made of organic materials according to claim 3, characterized in that, When sanding with 1500-grit or 2000-grit sandpaper, sand back and forth horizontally or vertically.

5. The method for repairing glass made of organic materials according to claim 1, characterized in that, In the second polishing process, an eccentric polishing machine is used, and a long wool disc is used for polishing. During the polishing process, the applied pressure reduces the thickness of the long wool disc by 1 / 3, and a grid-shaped polishing trajectory is used, with alternating horizontal and vertical polishing.

6. The method for repairing glass made of organic materials according to claim 1, characterized in that, In the third polishing process, an 8-shaped polishing trajectory is used, and the glass surface temperature is controlled below 60°C during the polishing process.

Citation Information

Patent Citations

  • Method for polishing glass substrate

    CN104487395A

  • Preparation method for anti-dazzle glass

    CN105436998A