Sintering aid-coated barium titanate-based thermosensitive ceramic and method for manufacturing the same
By coating barium lead titanate-based thermistors with a core-shell structured sintering aid, the problems of power attenuation and voltage breakdown in barium titanate-based ceramics during long-term energized applications are solved, achieving ceramic densification and improved voltage resistance, making it suitable for electric vehicle heating equipment.
Patent Information
- Application Number
- CN202510065663.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-01-16
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-01-16
AI Technical Summary
Existing barium titanate-based thermistors suffer from severe power attenuation during long-term energized applications, pose a significant risk of voltage breakdown, and exhibit poor density, making it difficult to simultaneously maintain excellent PTC effect and voltage withstand performance.
A core-shell structured sintering aid is used to coat barium lead titanate-based thermistors. The core layer is composed of barium carbonate, lead tetroxide, etc., and the shell layer is composed of silica sol, etc. It is prepared by ball milling, spray drying, calcination and sintering processes to refine the grains and promote densification.
While maintaining the excellent PTC effect, it significantly improves the voltage resistance and density of ceramics, and enhances the stability and service life of ceramics.
Smart Images

Figure CN119874354B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of materials science and technology, specifically to a sintering aid-coated lead barium titanate-based thermistor ceramic and its preparation method. Background Technology
[0002] Barium titanate (BaTiO3) ceramics are a representative ferroelectric material with a typical perovskite lattice structure. Pure barium titanate is an excellent insulating material, with a resistivity exceeding 10 Ω·cm at room temperature. 12 Ω·cm, relative permittivity is 10 4 BaTiO3 is an important class of functional ceramic materials. The PTC (positive temperature coefficient) effect of BaTiO3 was first discovered by Philips in the Netherlands in the 1950s. Introducing trace amounts of rare earth elements into BaTiO3 leads to a higher concentration of conduction band carriers after ionization, thereby increasing the material's conductivity and causing it to become semiconductive, with a resistivity of 10⁻⁶. 1 ~10 2 A semiconductor with a resistance of Ω·cm is called a valence-controlled semiconductor. The relationship between the resistance of a semiconductor and its temperature is called the PTC effect.
[0003] Barium titanate (BaTiO3) thermistor ceramics, based on semiconductor donor doping, exhibit positive temperature coefficient (PTC) resistivity. Due to their excellent thermoelectric properties, low manufacturing cost, high heating efficiency, and easily adjustable resistivity and Curie temperature, they have been widely used in various technological applications over the past few decades, such as self-regulating heating elements, overcurrent protection, and temperature sensors. In recent years, with the trend of electric vehicles replacing internal combustion engine vehicles to address environmental pollution, PTC elements have found new applications as the main heating devices in electric vehicles. However, this new application area requires different and customized performance characteristics. Since heating elements account for a major portion of energy consumption, the most prominent problem in current applications is that prolonged energization leads to severe power decay in ceramic elements and poses some risk of voltage breakdown. Therefore, it is necessary to effectively adjust the room temperature resistivity, resistivity, and withstand voltage of PTCs.
[0004] To optimize the PTC performance of barium titanate-based PTC ceramics and improve the stability of ceramic materials, scholars both domestically and internationally have focused on studying the effects of doping and sintering processes on the performance of barium titanate-based PTC ceramics. Cheng et al., by doping BaTiO3 with Nb and simultaneously modifying the sintering process, prepared PTC ceramics with a room temperature resistivity of only 0.14 Ω and a resistance increase ratio greater than 10. 3Low room temperature resistivity PTC ceramics; Li Yanyan et al. studied the effect of different donor Nb doping amounts on the properties of barium titanate-based ceramic materials. Experiments showed that with the increase of Nb₂O₅ doping amount, the room temperature resistivity of the ceramic first decreased and then increased, with the lowest room temperature resistivity observed when the donor Nb doping amount was 0.5 mol%. Zhiyu et al. studied the relationship between semiconductivity and sintering process, lead vacancies, barium vacancies, and donor and acceptor impurities in (Ba,Pb)TiO₃-based high-temperature PTC semiconductor ceramics, focusing on the influence of introducing acceptor impurity Mn on the semiconductivity of the material. Ding et al. prepared a ceramic with a room temperature resistivity of only 14 Ω and a resistance-to-weight ratio of 10 by changing the Mn content and continuously improving the sintering temperature and holding time. 5 A high-performance PTC effect ceramic with a temperature coefficient of approximately 22% was synthesized. Zhong Zhiyong employed a two-step synthesis method, introducing liquid-phase additives (Al2O3-SiO2-TiO2) to increase the density of the ceramic material. The resulting PTC ceramic exhibited a breakdown voltage greater than 900V and a rise-resistance ratio reaching 10. 3 above.
[0005] Although barium titanate-based thermistors have been extensively studied, current research indicates that low concentrations of liquid-phase additives and sintering aids result in poor density and insufficient voltage withstand performance. While studies have found that increasing the concentration of liquid-phase additives and adding higher concentrations of sintering aids can enhance the voltage withstand performance, related research shows that increasing the concentration of liquid-phase additives within the ceramic leads to increased resistivity, affecting the semiconductorization process and the PTC effect. Therefore, improving the voltage withstand performance of barium titanate-based thermistors while maintaining good PTC performance, and simultaneously preserving good sintering properties, is key to their wider application. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a sintering aid-coated lead barium titanate-based thermistor ceramic and its preparation method. This method refines the ceramic grains while promoting ceramic densification, thereby effectively improving the ceramic's voltage withstand performance while maintaining its excellent PTC effect.
[0007] To achieve the above objectives, the present invention provides the following technical solution: a sintering aid-coated barium lead titanate-based thermistor ceramic, characterized in that it has a core-shell structure; the molar composition of the raw materials in its core layer is as follows: barium carbonate 29-46 parts, lead tetroxide 2-7 parts, calcium carbonate 0.1-3 parts, strontium carbonate 0.1-4 parts, zirconium oxide 0.1-5 parts, tin oxide 0.1-8 parts, and titanium dioxide 49.4-49.93 parts. The shell contains 0.02-0.3 parts manganese oxide and 0.05-0.3 parts niobium pentoxide. The molar composition of the raw materials is as follows: 0.05-1 parts silica sol, 0.01-0.2 parts aluminum compounds, 0.01-0.2 parts calcium compounds, 0.05-0.5 parts sodium compounds, 0.05-0.5 parts potassium compounds, 0.01-0.5 parts boric acid, and 0.01-0.2 parts magnesium compounds.
[0008] As a preferred embodiment, the aluminum compound is one or more of aluminum nitrate, aluminum chloride, and aluminum acetate; the calcium compound is one or more of calcium nitrate, calcium chloride, and calcium acetate; the sodium compound is one or more of sodium nitrate, sodium chloride, and sodium acetate; the potassium compound is one or more of potassium nitrate, potassium chloride, and potassium acetate; and the magnesium compound is one or more of magnesium nitrate, magnesium chloride, and magnesium acetate.
[0009] A method for preparing lead barium titanate-based thermistor ceramics coated with sintering aids as described above includes the following steps:
[0010] (1) Weigh a certain amount of barium carbonate, lead tetroxide, calcium carbonate, strontium carbonate, zirconium oxide, tin oxide, titanium dioxide, manganese oxide, and niobium pentoxide according to the proportion of the core layer raw materials. Then, place the above substances together with anhydrous ethanol in a ceramic ball mill jar, add zirconium oxide grinding balls at the same time, and ball mill. Place the ball-milled slurry in an oven at 80°C and dry for 4 to 6 hours. Then place it in an alumina crucible and keep it at 950 to 1050°C for 2 to 4 hours. After cooling, obtain lead barium titanate-based powder.
[0011] (2) Weigh a certain amount of silica sol, aluminum compound, calcium compound, sodium compound, potassium compound, boric acid and magnesium compound according to the proportion of shell raw materials, and then dissolve the above compounds in deionized water to obtain a deionized water solution of 0.5 to 3 mol / L.
[0012] (3) The lead barium titanate-based powder prepared in step (1) and the deionized aqueous solution prepared in step (2) are placed together in a ball mill for ball milling, and then spray dried; the spray-dried powder is placed in an alumina crucible and calcined at 1000-1100℃ for 3-6 hours.
[0013] (4) The calcined powder is placed in a ball mill jar, and at the same time, a 5% polyvinyl alcohol aqueous solution is added at twice the mass of the powder. After ball milling and mixing, the mixture is spray granulated to obtain granulated powder.
[0014] (5) The above granulated powder is dry-pressed and then kept at 300-500°C for 4-10 hours to remove the glue. Then, the temperature is raised to 1250-1350°C and kept for 2-4 hours to sinter, thereby obtaining the sintering aid-coated lead barium titanate-based thermistor ceramic of the present invention.
[0015] The beneficial effects of this invention are as follows: The core-shell structure prepared by this invention, with lead barium titanate-based powder as the core and sintering aid precursor as the shell, allows the sintering aid precursor to be uniformly coated on the surface of the lead barium titanate-based powder. The Ca, Sr, Zr, Sn and other elements added to the lead barium titanate-based powder refine the grains, while the sintering aid in the shell refines the ceramic grains and promotes the densification of the ceramic. Thus, while maintaining the excellent PTC effect of the ceramic, the voltage withstand performance of the ceramic is effectively improved. Attached Figure Description
[0016] Figure 1 Scanning electron microscope image of the lead barium titanate-based thermistor ceramic prepared in this invention. Detailed Implementation
[0017] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] Example 1:
[0019] Weigh out 37 parts barium carbonate, 6 parts lead tetroxide, 1 part calcium carbonate, 1 part strontium carbonate, 1 part zirconium oxide, 4 parts tin oxide, 49.65 parts titanium dioxide, 0.15 parts manganese oxide, and 0.2 parts niobium pentoxide according to the molar ratio. Place the above substances together with anhydrous ethanol in a ceramic ball mill jar, add zirconium oxide grinding balls at the same time, and ball mill. Place the ball-milled slurry in an oven at 80°C and dry for 5 hours. Then place it in an alumina crucible and keep it at 1000°C for 3 hours. After cooling, lead barium titanate-based powder is obtained.
[0020] Weigh out 0.5 parts silica sol, 0.1 parts aluminum nitrate, 0.02 parts calcium nitrate, 0.06 parts sodium nitrate, 0.12 parts potassium nitrate, 0.05 parts boric acid, and 0.05 parts magnesium nitrate according to the molar ratio, and then dissolve them in deionized water to obtain a 2 mol / L deionized water solution.
[0021] The prepared lead-barium titanate-based powder was ball-milled together with a deionized aqueous solution in a ball mill, followed by spray drying. The spray-dried powder was then placed in an alumina crucible and calcined at 1050°C for 4 hours. The calcined powder was then placed in a ball mill jar, and 5% polyvinyl alcohol aqueous solution (by mass) was added at twice the powder mass. After ball milling and mixing, the mixture was spray-granulated to obtain granulated powder. The granulated powder was then dry-pressed, and then debinded at 400°C for 8 hours. Subsequently, the temperature was raised to 1290°C and held for 3 hours for sintering to obtain sintering aid-coated lead-barium titanate-based thermistor ceramic.
[0022] The scanning electron microscope image of the lead-barium titanate-based thermistor ceramic prepared in this example is shown below. Figure 1 As shown.
[0023] The ceramic sample was polished on both sides, coated with ohmic silver paste, and kept at 550℃ for 30 min to complete electrode preparation. Subsequently, the ceramic sample was subjected to resistance-temperature test and withstand voltage test, and its performance parameters are shown in Table 1.
[0024] Example 2:
[0025] Weigh out 33.5 parts barium carbonate, 7 parts lead tetroxide, 3 parts calcium carbonate, 0.5 parts strontium carbonate, 2 parts zirconium oxide, 4 parts tin oxide, 49.4 parts titanium dioxide, 0.3 parts manganese oxide, and 0.3 parts niobium pentoxide according to the molar ratio. Place the above substances together with anhydrous ethanol in a ceramic ball mill jar, add zirconium oxide grinding balls at the same time, and ball mill. Place the ball-milled slurry in an oven at 80°C and dry for 4 hours. Then place it in an alumina crucible and keep it at 950°C for 4 hours. After cooling, lead barium titanate-based powder is obtained.
[0026] Weigh out 1 part silica sol, 0.2 parts aluminum nitrate, 0.2 parts calcium nitrate, 0.1 parts sodium nitrate, 0.3 parts potassium nitrate, 0.2 parts boric acid, and 0.1 parts magnesium nitrate according to the molar ratio, and then dissolve them in deionized water to obtain a 0.5 mol / L deionized water solution.
[0027] The prepared lead-barium titanate-based powder was ball-milled together with a deionized aqueous solution in a ball mill, followed by spray drying. The spray-dried powder was then placed in an alumina crucible and calcined at 1000°C for 6 hours. The calcined powder was then placed in a ball mill jar, and 5% polyvinyl alcohol aqueous solution (by mass) was added at twice the powder mass. After ball milling and mixing, the mixture was spray-granulated to obtain granulated powder. The granulated powder was then dry-pressed, and then debinded at 500°C for 4 hours. Subsequently, the temperature was raised to 1280°C and held for 4 hours for sintering to obtain sintering aid-coated lead-barium titanate-based thermistor ceramic.
[0028] The ceramic sample was polished on both sides, coated with ohmic silver paste, and kept at 550℃ for 30 min to complete electrode preparation. Subsequently, the ceramic sample was subjected to resistance-temperature test and withstand voltage test, and its performance parameters are shown in Table 1.
[0029] Example 3:
[0030] Weigh out 35.8 parts barium carbonate, 5 parts lead tetroxide, 0.1 parts calcium carbonate, 0.1 parts strontium carbonate, 1 part zirconium oxide, 8 parts tin oxide, 49.6 parts titanium dioxide, 0.2 parts manganese oxide, and 0.2 parts niobium pentoxide according to the molar ratio. Place the above substances together with anhydrous ethanol in a ceramic ball mill jar, add zirconium oxide grinding balls, and ball mill. Place the ball-milled slurry in an oven at 80°C and dry for 6 hours. Then place it in an alumina crucible and keep it at 1050°C for 2 hours. After cooling, lead barium titanate-based powder is obtained.
[0031] Weigh out 0.2 parts silica sol, 0.05 parts aluminum nitrate, 0.01 parts calcium nitrate, 0.1 parts sodium nitrate, 0.2 parts potassium nitrate, 0.1 parts boric acid, and 0.05 parts magnesium nitrate according to the molar ratio, and then dissolve them in deionized water to obtain a 3 mol / L deionized water solution.
[0032] The prepared lead-barium titanate-based powder was ball-milled together with a deionized aqueous solution in a ball mill, followed by spray drying. The spray-dried powder was then placed in an alumina crucible and calcined at 1100°C for 3 hours. The calcined powder was then placed in a ball mill jar, and a 5% polyvinyl alcohol aqueous solution was added at twice the powder mass. After ball milling and mixing, the mixture was spray-granulated to obtain granulated powder. The granulated powder was then dry-pressed, and then debinded at 300°C for 10 hours. Subsequently, the temperature was raised to 1320°C and held for 2 hours for sintering to obtain sintering aid-coated lead-barium titanate-based thermistor ceramic.
[0033] The ceramic sample was polished on both sides, coated with ohmic silver paste, and kept at 550℃ for 30 min to complete electrode preparation. Subsequently, the ceramic sample was subjected to resistance-temperature test and withstand voltage test, and its performance parameters are shown in Table 1.
[0034] Table 1 Electrical properties of the lead barium titanate-based thermistor ceramics prepared in this invention
[0035]
Claims
1. A sintering aid-coated lead-barium titanate-based thermistor ceramic, characterized in that: It has a core-shell structure; the molar composition of the raw materials in its core layer is as follows: barium carbonate 29-46 parts, lead tetroxide 2-7 parts, calcium carbonate 0.1-3 parts, strontium carbonate 0.1-4 parts, zirconium oxide 0.1-5 parts, tin oxide 0.1-8 parts, titanium dioxide 49.4-49.93 parts, manganese oxide 0.02-0.3 parts, and niobium pentoxide 0.05-0.3 parts; the molar composition of the raw materials in its shell layer is as follows: silica sol 0.05-1 part, aluminum compounds 0.01-0.2 parts, calcium compounds 0.01-0.2 parts, sodium compounds 0.05-0.5 parts, potassium compounds 0.05-0.5 parts, boric acid 0.01-0.5 parts, and magnesium compounds 0.01-0.2 parts.
2. The sintering aid-coated barium lead titanate-based thermistor ceramic according to claim 1, characterized in that: The aluminum compound is one or more of aluminum nitrate, aluminum chloride, and aluminum acetate; the calcium compound is one or more of calcium nitrate, calcium chloride, and calcium acetate; the sodium compound is one or more of sodium nitrate, sodium chloride, and sodium acetate; the potassium compound is one or more of potassium nitrate, potassium chloride, and potassium acetate; and the magnesium compound is one or more of magnesium nitrate, magnesium chloride, and magnesium acetate.
3. A method for preparing lead barium titanate-based thermistor ceramics coated with the sintering aid as described in claim 1, comprising the following steps: (1) Weigh a certain amount of barium carbonate, lead tetroxide, calcium carbonate, strontium carbonate, zirconium oxide, tin oxide, titanium dioxide, manganese oxide, and niobium pentoxide according to the proportion of the core layer raw materials. Then, place the above substances together with anhydrous ethanol in a ceramic ball mill jar, add zirconium oxide grinding balls at the same time, and ball mill. Place the ball-milled slurry in an oven at 80°C and dry for 4 to 6 hours. Then place it in an alumina crucible and keep it at 950 to 1050°C for 2 to 4 hours. After cooling, obtain lead barium titanate-based powder. (2) Weigh a certain amount of silica sol, aluminum compound, calcium compound, sodium compound, potassium compound, boric acid and magnesium compound according to the proportion of shell raw materials, and then dissolve the above compounds in deionized water to obtain a deionized water solution of 0.5 to 3 mol / L. (3) The lead barium titanate-based powder prepared in step (1) and the deionized aqueous solution prepared in step (2) are placed together in a ball mill for ball milling, and then spray dried; the spray-dried powder is placed in an alumina crucible and calcined at 1000-1100℃ for 3-6 hours. (4) The calcined powder is placed in a ball mill jar, and a 5% polyvinyl alcohol aqueous solution is added at twice the mass of the powder. After ball milling and mixing, the mixture is spray granulated to obtain granulated powder. (5) The above granulated powder is dry-pressed and then kept at 300-500℃ for 4-10 hours to remove the glue. Then, the temperature is raised to 1250-1350℃ and kept for 2-4 hours to sinter, thus obtaining the sintering aid-coated lead barium titanate-based thermistor ceramic.
Citation Information
Patent Citations
Method of producing fine-particle multicomponent glass powders for use as a glass flow for producing layers and decorations on glass, glass ceramic or ceramic
US5837025A