Image recording method and image recording apparatus

By controlling the concentration viscosity and heating drying parameters of white ink, and combining inkjet and heating processes, the problem of insufficient concealment and adhesion of white images on non-permeable substrates was solved, achieving high-quality white image recording.

CN119894685BActive Publication Date: 2026-11-24FUJIFILM CORP
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
CN202380066891.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-09-21
Filing Date
2023-09-05
Publication Date
2026-11-24
Estimated Expiration
2043-09-05

AI Technical Summary

Technical Problem

Existing technologies for recording white images via inkjet printing suffer from insufficient concealment and adhesion, especially when recording on non-permeable substrates. It is difficult to simultaneously achieve both high coverage and concealment performance and good adhesion to the substrate.

Method used

By controlling the concentration viscosity of white ink, the heating and drying rate, and the warm air speed during the drying process, combined with inkjet printing and heating and drying procedures, the effective adhesion and coverage of white ink on non-permeable substrates can be ensured. This specifically includes the use of inkjet printheads and heating and drying devices.

Benefits of technology

This technology enables white images recorded on non-permeable substrates to exhibit excellent concealment and adhesion, improving the coverage and hiding performance of white images and their adhesion to the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119894685B_ABST
    Figure CN119894685B_ABST
Patent Text Reader

Abstract

An image recording method includes a recording step of applying white ink containing water, white pigment and resin to a surface of a non-permeable substrate by inkjet printing and heating and drying the applied white ink to record a white image. When the viscosity of the concentrated ink obtained by concentrating the white ink to 30% by mass is set as X mPa·s and the heating rate from the start of heating and drying to 5 seconds is set as Y °C / s, the product of X and Y is 30 to 280.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an image recording method and an image recording apparatus. Background Technology

[0002] Various studies have been conducted on image recording methods and devices in the past.

[0003] For example, in Patent Document 1, the following printing method is disclosed as a method for manufacturing printed matter to obtain high-quality reverse-printed printed matter.

[0004] In the printing method disclosed in Patent Document 1, a first processing liquid containing a coagulant that causes colored ink and white ink to coagulate is applied to a non-permeable medium. An image is printed by applying colored ink to the non-permeable medium to which the first processing liquid has been applied, and white ink is applied to the non-permeable medium to which the colored ink has been applied. Here, when the combined amount of colored ink and white ink applied exceeds a threshold, a second processing liquid containing at least a coagulant that causes white ink to coagulate is applied to the non-permeable medium after the application of colored ink and before the application of white ink.

[0005] Furthermore, in Patent Document 2, the following recording method is disclosed as a recording method that ensures lamination resistance in the back printing mode of transparent flexible packaging film.

[0006] The recording method disclosed in Patent Document 2 is a recording method for recording on a recording medium used to laminate the recording surface to be recorded. It includes: a non-white ink adhesion step, in which a water-based non-white ink composition containing a non-white pigment is adhered to the recording medium; a white ink adhesion step, in which a water-based white ink composition containing a white pigment is adhered to the recording medium that has undergone the non-white ink adhesion step; and a transparent ink adhesion step, in which a transparent ink composition containing a resin is adhered to the recording medium that has undergone the white ink adhesion step.

[0007] Furthermore, in Patent Document 3, the following inkjet printer is disclosed as an inkjet printer capable of performing both surface printing and back printing using water-based inks while continuously conveying a roll of printing substrate at high speed.

[0008] The inkjet printer disclosed in Patent Document 3 includes: a first white ink printhead that sprays white water-based ink onto the surface of a roll-shaped printing substrate during surface printing; a first roller-type drying unit that dries the white water-based ink during surface printing; a second white ink printhead that sprays white water-based ink onto the surface of a roll-shaped printing substrate during back printing; and a second roller-type drying unit that dries the white water-based ink during back printing.

[0009] Patent Document 1: International Publication No. 2020 / 137323

[0010] Patent Document 2: Japanese Patent Application Publication No. 2021-17005

[0011] Patent Document 3: International Publication No. 2019 / 131204 Summary of the Invention

[0012] The technical problem to be solved by the invention

[0013] However, sometimes there is a need to further improve the concealment and adhesion of the recorded white image in image recording methods that use inkjet technology to apply white ink containing water, white pigment and resin to one side of a non-permeable substrate and then heat-dry the applied white ink.

[0014] Here, the concealment of a white image refers to the ability to cover and hide the color of the substrate on which the white image is recorded (e.g., a non-porous substrate, a colored image recorded before the white image, etc. The same applies hereinafter). The adhesion of a white image refers to the adhesion of the white image relative to the substrate on which the white image is recorded.

[0015] The present invention was made in view of this situation, and its object is to provide an image recording method and an image recording apparatus that can record white images with excellent concealment and adhesion when white ink containing water, white pigment and resin is applied to one surface of a non-permeable substrate by inkjet printing and the applied white ink is heated and dried to record a white image.

[0016] means for solving technical problems

[0017] The present invention includes the following methods.

[0018] <1> An image recording method, comprising:

[0019] The recording process involves applying white ink containing water, white pigment, and resin to one surface of a non-porous substrate using an inkjet printer, and then heating and drying the applied white ink to record a white image.

[0020] When the viscosity of the concentrated ink obtained by concentrating white ink to a mass reduction of 30% is set as X mPa·s, and the heating rate from the start of heating and drying to 5 seconds is set as Y °C / s, the product of X and Y is 30 to 280.

[0021] <2> According to the image recording method described in <1>, wherein,

[0022] The product of X and Y is between 40 and 200.

[0023] <3> The image recording method according to <1> or <2>, wherein,

[0024] Heating and drying are carried out by blowing warm air. When the value obtained by dividing the wind speed of the warm air in m / s units by the temperature of the warm air in ℃ units is set as Z, the product of X and Z is 2.0 to 10.0.

[0025] <4> According to the image recording method described in <3>, wherein,

[0026] The product of X and Z is 3.5 to 7.5.

[0027] <5> The image recording method according to any one of <1> to <4>, wherein,

[0028] The value obtained by dividing the thickness of the white ink applied to one side of the non-permeable substrate after heat drying by the thickness of the white ink applied to one side of the non-permeable substrate before heat drying is 0.10 to 0.20.

[0029] <6> The image recording method according to any one of <1> to <5>, wherein,

[0030] The thickness of the white ink applied to one side of a non-permeable substrate after heat drying is 1.30 μm to 1.80 μm. <7> The image recording method according to any one of <1> to <6>, wherein,

[0031] The recording process also includes a step of conveying a non-permeable substrate coated with white ink via a conveying component in a configuration where the conveying component contacts the white ink.

[0032] Following the recording process is a winding process that involves winding up a non-permeable substrate with the recorded white image.

[0033] The average contact pressure between the conveyor and the white ink from the application of white ink to the winding of the non-permeable substrate is 750 N / m. 2 ~4000N / m 2 .

[0034] <8> The image recording method according to any one of <1> to <7>, wherein,

[0035] The recording process also includes the process of applying a colored ink containing water, pigments and resin to one side of a non-permeable substrate by inkjet printing to record a colored image.

[0036] <9> According to the image recording method described in <8>, wherein,

[0037] The colored image is recorded before the white image and positioned between the non-porous substrate and the white image.

[0038] <10> The image recording method according to any one of <1> to <9> further includes, prior to the recording step, a step of applying a pretreatment liquid containing water and a coagulant to one surface of a non-permeable substrate.

[0039] In the recording process, white ink is applied to an area on a surface that has been pretreated with the liquid to record a white image.

[0040] <11> An image recording apparatus for the image recording method described in any one of <1> to <10>, the image recording apparatus comprising:

[0041] An inkjet head is used to apply the aforementioned white ink to one surface of a non-porous substrate; and

[0042] A heating and drying apparatus for heating and drying the aforementioned white ink.

[0043] The product of X and Y is 30 to 280.

[0044] Invention Effects

[0045] According to one embodiment of the present invention, an image recording method and an image recording apparatus are provided, which can record white images with excellent concealment and adhesion when applying white ink containing water, white pigment and resin to one surface of a non-permeable substrate by inkjet printing and heating and drying the applied white ink to record a white image. Attached Figure Description

[0046] Figure 1 This is a diagram that conceptually illustrates an example of an image recording apparatus used in implementing the image recording method of the present invention. Detailed Implementation

[0047] In this invention, the numerical range represented by “~” indicates the range included by taking the values ​​recorded before and after “~” as the minimum and maximum values, respectively.

[0048] In the numerical ranges described in this specification, the upper or lower limit value recorded in a certain numerical range can be replaced with the upper or lower limit value of other numerical ranges described in different stages. Furthermore, the upper or lower limit value recorded in a certain numerical range described in this specification can also be replaced with the values ​​shown in the embodiments.

[0049] In this invention, the amount of each component in the composition, when there are multiple substances corresponding to each component in the composition, means the total amount of the multiple substances present in the composition, unless otherwise stated.

[0050] In this invention, a combination of two or more preferred methods is a more preferred method.

[0051] In this invention, the term "process" includes not only independent processes, but also processes that can achieve their intended purpose, even if they cannot be clearly distinguished from other processes.

[0052] In this invention, the term "image" refers to the ink film itself when no pretreatment liquid is used, and to the laminated film of the pretreatment liquid film and the ink film when a pretreatment liquid is used.

[0053] In this invention, "image recording" refers to the formation of an image.

[0054] The concept of "image" in this invention also includes solid images.

[0055] In this invention, the description of "applying ink to one surface of a substrate" includes a method of directly applying ink to one surface of a substrate, and a method of directly applying ink to the surface of layer A when layer A is formed on one surface of a substrate, for example.

[0056] In this invention, unless otherwise specified, "upstream side" refers to the upstream side of the transport direction of the non-permeable substrate, and unless otherwise specified, "downstream side" refers to the downstream side of the transport direction of the non-permeable substrate.

[0057] [Image recording method]

[0058] The image recording method of the present invention (hereinafter also referred to as the "recording method") includes:

[0059] The recording process involves applying white ink containing water, white pigment, and resin to one side (hereinafter referred to as the "front side" or "recording side") of a non-porous substrate using an inkjet printer, and then heating and drying the applied white ink to record a white image.

[0060] When the viscosity of the concentrated ink obtained by concentrating white ink to a mass reduction of 30% is set as X mPa·s, and the heating rate from the start of heating and drying to 5 seconds is set as Y °C / s, the product of X and Y is 30 to 280.

[0061] According to the recording method of the present invention, it is possible to record white images with excellent concealment (i.e., the property of covering and hiding the color of the substrate) and adhesion (i.e., adhesion to non-permeable substrates).

[0062] In detail, in the recording method of the present invention, when the product of X and Y (hereinafter also referred to as "product (X*Y)") is 30 or more, the concealment of the obtained white image is improved, and when the product (X*Y) is 280 or less, the tightness of the obtained white image is improved.

[0063] The reason why the concealment of a white image is improved by multiplying (X*Y) by 30 or more is as follows.

[0064] X (i.e., the viscosity of the concentrated ink obtained by concentrating white ink to a 30% mass reduction at 32°C) is a viscosity simulating the viscosity of white ink during heat drying. It is believed that if X is too small, white pigments tend to precipitate in the film formed by the white ink (hereinafter also referred to as the white ink film), resulting in a thinner white ink film and reduced concealment of the white image.

[0065] Furthermore, it is believed that if Y (i.e., the heating rate from the start of heating and drying to 5 seconds later) is too small, the drying (i.e., the evaporation of the solvent) will be slower, and the white pigment will easily precipitate in the white ink film, thus reducing the concealment of the white image.

[0066] In response to these tendencies, it is believed that by setting the product (X*Y) to 30 or higher, the precipitation of white pigment in the white ink film is suppressed, thereby ensuring the concealment of the obtained white image.

[0067] The reason for the improved fit of the white image obtained by multiplying (X*Y) by 280 or less is as follows.

[0068] It is believed that as X increases, it is beneficial to the concealment of white images, but the thickness of the white ink film increases and the film quality tends to decrease, thus the adhesion of the white image tends to decrease.

[0069] Furthermore, it is believed that when Y is too large, drying becomes too fast, which easily leads to skin formation on the white ink film. The drying inside the white ink film is insufficient, and the adhesion of the white image tends to decrease.

[0070] In response to these tendencies, it is believed that by setting the product (X*Y) to 280 or less, the skinning of the white ink film, insufficient internal drying, and reduced film quality can be suppressed. As a result, the adhesion of the obtained white image (adhesion to non-permeable substrates) can be ensured.

[0071] <Product (X*Y)>

[0072] As described above, in the recording method of the present invention, the product (X*Y) is 30 to 280.

[0073] The concealment of the white image is improved by multiplying (X*Y) by 30 or more.

[0074] By having a product (X*Y) of 280 or less, the density of the resulting white image is improved.

[0075] The product (X*Y) is preferably between 40 and 200.

[0076] The concealment of the white image is further improved by multiplying (X*Y) by 40 or more.

[0077] By setting the product (X*Y) to below 200, the tightness of the resulting white image is further improved.

[0078] In the product (X*Y), "X" represents the viscosity (in mPa·s) of the concentrated ink obtained by concentrating the white ink to a 30% mass reduction at 32°C.

[0079] Here, "concentration" refers to the removal of a portion of the solvent (i.e., water and, if present, water-soluble organic solvents, as in the case of white ink. The same applies hereinafter.) from the white ink.

[0080] That is, the concentrated ink mentioned above is an ink obtained by removing (e.g., distilling away) 30% of the solvent from the white ink relative to the total mass of the white ink.

[0081] The viscosity of concentrated ink at 32°C is measured using a viscometer (e.g., the TV-22 viscometer manufactured by TOKI SANGYO CO.,LTD.).

[0082] In the recording method of the present invention, by setting the concentration (i.e., solvent removal) of the white ink used to obtain "X" to "reduction of 30%", the accuracy of the relationship between the product (X*Y) and the effect (concealment and tightness of the white image) is improved.

[0083] It is argued that if the degree of concentration (i.e., solvent removal) is set to, for example, "reduction of less than 20%" instead of "reduction of 30%", the fluidity of the white ink is not lost, and the accuracy of the relationship between the product (X*Y) and the effect is insufficient.

[0084] It is argued that if the degree of concentration (i.e., solvent removal) is set to, for example, "reduction of more than 40%" instead of "reduction of 30%", it is sometimes difficult to determine the difference in the fluidity of white ink, and the accuracy of the relationship between the product (X*Y) and the effect is insufficient.

[0085] The "X" in the product (X*Y) is preferably 10.0 to 20.0, more preferably 10.0 to 19.0, and even more preferably 11.0 to 17.0.

[0086] In the product (X*Y), "Y" represents the heating rate (in °C / s) from the start of the heating and drying process until 5 seconds have elapsed.

[0087] The heating rate refers to the rate at which the surface temperature of the white ink film undergoes heat drying increases.

[0088] The surface temperature of the white ink film was measured using a non-contact thermometer (e.g., the FT-H20 manufactured by KEYENCE CORPORATION).

[0089] In this invention, by defining “Y” as the heating rate from the start of heating and drying until “5 seconds” have elapsed, the accuracy of the relationship between the product (X*Y) and the effect is improved.

[0090] If Y is defined as being shorter than "5 seconds" (e.g., "less than 3 seconds"), the accuracy of the heating rate is considered insufficient.

[0091] When Y is defined as being longer than "5 seconds" (e.g., "more than 7 seconds"), there will be a case of temperature passivation, and the accuracy of the speed is also considered insufficient.

[0092] The "Y" in the product (X*Y) is preferably 1.0 to 25.0, more preferably 1.5 to 20.0, and even more preferably 2.0 to 15.0.

[0093] <Record Process>

[0094] The recording process involves applying white ink containing water, white pigment, and resin to the front side of a non-permeable substrate using an inkjet method, and then heating and drying the applied white ink to record a white image.

[0095] (Non-permeable substrate)

[0096] In this invention, the non-permeability of the non-permeable substrate refers to the property that the water absorption rate after 24 hours is less than 2.5%, as measured according to ASTM D570-98 (2018). Here, the "%" used as the unit of water absorption rate is based on mass. The aforementioned water absorption rate is preferably less than 1.0%, more preferably less than 0.5%.

[0097] Materials that can be used as non-permeable substrates include, for example, glass, metals (e.g., aluminum, zinc, copper, etc.) and resins (e.g., polyvinyl chloride, cellulose diacetate, cellulose triacetate, cellulose propionate, cellulose butyrate, cellulose acetate butyrate, cellulose nitrate, polyethylene terephthalate, polyethylene, polystyrene, polypropylene, polycarbonate, polyvinyl acetal, nylon, acrylic resin, etc.).

[0098] The non-permeable substrate is preferably made of resin. That is, the non-permeable substrate is preferably a non-permeable substrate.

[0099] From a general perspective, the preferred materials for non-permeable substrates are polypropylene, polyethylene, polyethylene terephthalate, nylon, acrylic resin, or polyvinyl chloride.

[0100] The shape of the non-permeable substrate is preferably sheet (film) or plate. Examples of non-permeable substrates with this shape include glass plates, metal plates, resin sheets (resin films), paper laminated with plastic, paper laminated or vapor-deposited with metal, and plastic sheets (plastic films) laminated or vapor-deposited with metal.

[0101] As a non-permeable substrate made of resin, examples include resin sheets (resin films), and more specifically, flexible packaging materials for packaged foods and floor guide panels in large retail stores.

[0102] In addition to sheet-like (film-like) or plate-like non-permeable substrates, textiles (fabrics) and non-woven fabrics formed from non-permeable fibers can also be cited as examples of non-permeable substrates.

[0103] The thickness of the non-permeable substrate is preferably 0.1 μm to 1,000 μm, more preferably 0.1 μm to 800 μm, and even more preferably 1 μm to 500 μm.

[0104] Surface treatment can be applied to at least one of the front and back sides of a non-permeable substrate.

[0105] Examples of surface treatments include corona treatment, plasma treatment, flame treatment, heat treatment, abrasion treatment, light irradiation treatment (e.g., UV treatment), but are not limited to these. Corona treatment can be performed, for example, using a corona treatment machine (product name "PS-10S", manufactured by Shinko Electric & Instrumentation Co., Ltd.).

[0106] The surface treatment conditions can be selected appropriately based on the type of non-permeable substrate.

[0107] Furthermore, the surface energy of the back side of the non-permeable substrate can be adjusted by whether or not a surface treatment is performed on the back side of the non-permeable substrate and by adjusting the conditions under which the surface treatment is performed, thereby adjusting ΔE and the ΔE / P ratio.

[0108] Non-permeable substrates can be transparent non-permeable substrates.

[0109] Here, transparency means that the transmittance of visible light with wavelengths of 400nm to 700nm is 80% or more (preferably 90% or more).

[0110] When the non-permeable substrate is a transparent non-permeable substrate, the image can be easily visually identified from the back side of the non-permeable substrate.

[0111] For example, when the non-permeable substrate is a transparent non-permeable substrate, and when recording is performed on the non-permeable substrate in a manner in which patterned images such as characters and graphics, i.e. colored images, and white images (e.g., solid images) as background images are arranged sequentially when viewed from the non-permeable substrate side, it is easy to visually identify the colored images (e.g., patterned images such as characters and graphics) with white images (e.g., solid images) as backgrounds through the non-permeable substrate from the image back side of the non-permeable substrate.

[0112] In this invention, "coloring" in coloring inks and coloring pigments refers to color (e.g., cyan, magenta, yellow, etc.) or black (hereinafter also referred to as Black).

[0113] [White ink]

[0114] White ink contains water, white pigment, and resin.

[0115] The following is an explanation of the white ink.

[0116] -water-

[0117] White ink contains water.

[0118] The water content relative to the total amount of white ink is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 50% by mass or more.

[0119] The upper limit of the water content relative to the total amount of white ink can be appropriately determined based on the content of other components, for example, 99% by mass, preferably 95% by mass, and more preferably 90% by mass.

[0120] -White pigment-

[0121] White ink contains at least one white pigment.

[0122] Examples of inorganic pigments that can be used as white pigments include titanium dioxide, barium sulfate, calcium carbonate, silicon dioxide, zinc oxide, zinc sulfide, mica, talc, and pearl.

[0123] The preferred white pigment is titanium dioxide, barium sulfate, calcium carbonate, or zinc oxide, with titanium dioxide being more preferred.

[0124] From the viewpoint of concealment, the average primary particle size of the white pigment is preferably 150 nm or more, more preferably 200 nm or more. Furthermore, from the viewpoint of ink ejectibility, the average primary particle size of the white pigment is preferably 400 nm or less, more preferably 350 nm or less.

[0125] Here, concealment refers to the ability to cover and hide a substrate that forms a white image (e.g., the front side of a non-permeable substrate or a colored image recorded on the front side before the white image).

[0126] In this invention, the average primary particle size of the white pigment is a value measured using a transmission electron microscope (TEM). Specifically, it is the value obtained by selecting any 50 white pigments present in the field of view observed by the TEM, measuring the primary particle size of each of the 50 pigments, and averaging the results. The transmission electron microscope is the JEOL Ltd. 1200EX transmission electron microscope.

[0127] From the viewpoint of image density and ejectibility, when the ink contains white pigment, the content of white pigment relative to the total amount of ink is preferably 2% to 25% by mass, more preferably 5% to 25% by mass, and even more preferably 10% to 20% by mass.

[0128] -Resin-

[0129] White ink contains at least one type of resin.

[0130] The resin in white ink contributes to the film-forming properties of white ink (i.e., the ability to form a white ink film).

[0131] The weight-average molecular weight (Mw) of the resin is preferably 1,000 to 300,000, more preferably 2,000 to 200,000, and even more preferably 5,000 to 100,000.

[0132] In this invention, unless otherwise stated, weight-average molecular weight (Mw) refers to the value determined by gel permeation chromatography (GPC).

[0133] In the determination by gel permeation chromatography (GPC), the apparatus used was an HLC-8020GPC (TOSOH CORPORATION), with three TSKgel Super Multipore HZ-H columns (4.6 mm ID × 15 cm, TOSOH CORPORATION) used as the column and THF (tetrahydrofuran) as the eluent. The determination conditions were set as follows: sample concentration 0.45% by mass, flow rate 0.35 ml / min, sample injection volume 10 μl, and determination temperature 40 °C, using an RI detector.

[0134] The calibration curves were prepared using eight samples from TOSOH Corporation's "Standard Samples TSK standard, polystyrene": "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000" and "n-propylbenzene".

[0135] As a resin, pigment dispersion resins, which are used as pigment dispersants, can be cited as an example.

[0136] As a resin, resin particles can also be cited.

[0137] White inks may contain at least one pigment dispersion resin.

[0138] Pigment dispersion resin is a resin that has the function of dispersing pigments.

[0139] Pigment dispersion resins can be random copolymers or block copolymers.

[0140] Pigment dispersion resins can have cross-linked structures.

[0141] Inks can be prepared using pigment dispersions containing pigments and pigment dispersing resins.

[0142] Regarding pigment dispersion resins, for example, known polymer dispersants such as those described in paragraphs 0029 to 0106 of International Publication No. 2021 / 221069 can be used.

[0143] When the white ink contains pigment dispersion resin, the ratio of the pigment content to the pigment dispersion resin content in the ink, based on a mass basis, is preferably 1:0.04 to 1:3, more preferably 1:0.05 to 1:1, and even more preferably 1:0.05 to 1:0.5.

[0144] When the white ink contains pigment dispersion resin, the content of pigment dispersion resin relative to the total amount of white ink is preferably 0.1% to 10% by mass, more preferably 0.3% to 5% by mass, and even more preferably 0.5% to 2.5% by mass.

[0145] White ink may contain at least one type of resin particle.

[0146] The resin constituting the resin particles is preferably a water-insoluble resin. "Water-insoluble" in water-insoluble resin refers to the property that its solubility in 100g of distilled water at 25°C is less than 2g.

[0147] The volume average particle size of the resin particles is preferably 1 nm to 300 nm, more preferably 3 nm to 200 nm, and even more preferably 5 nm to 150 nm.

[0148] In this invention, the volume average particle size refers to the value measured using a laser diffraction / scattering particle size analyzer.

[0149] As a measuring device, an example is the particle size distribution measuring device "Microtrac MT-3300II" (manufactured by Nikkiso Co., Ltd.).

[0150] The resin particles are preferably selected from at least one of the following groups: acrylic resin particles, ester resin particles, mixtures of acrylic resin particles and ester resin particles, composite particles containing acrylic resin and ester resin, styrene acrylic resin particles, and polyurethane resin particles.

[0151] In this invention, acrylic resin refers to a polymer (homopolymer or copolymer) containing at least one raw material monomer selected from the group consisting of acrylic acid, derivatives of acrylic acid (e.g., acrylates), methacrylic acid, and derivatives of methacrylic acid (e.g., methacrylates).

[0152] From the viewpoint of further improving the abrasion resistance of the image, the glass transition temperature (Tg) of the resin particles is preferably 50°C to 250°C, more preferably 50°C to 150°C.

[0153] Here, the glass transition temperature (Tg) of the resin particles is determined by actual measurement. For the method of determining Tg, please refer to paragraph 0111 of Japanese Patent Application Publication No. 2015-25076.

[0154] Regarding resin particles, for example, see paragraphs 0038 to 0114 of International Publication No. 2021 / 192720 and paragraphs 0109 to 0120 of Japanese Patent Application Publication No. 2015-25076.

[0155] When the white ink contains resin particles, the content of resin particles in the white ink relative to the total amount of white ink is preferably 1% to 20% by mass, more preferably 2% to 15% by mass, and even more preferably 2% to 10% by mass.

[0156] -Water-soluble organic solvents-

[0157] White inks preferably contain at least one water-soluble organic solvent.

[0158] This ensures the stability of the inkjet output.

[0159] The water-soluble organic solvent contained in white ink can be one type or two or more types.

[0160] In this invention, "water-soluble" in "water-soluble organic solvent" refers to the property of dissolving more than 1g of water at 25°C in 100g of water.

[0161] There are no restrictions on the types of water-soluble organic solvents that can be contained in white inks. For example:

[0162] Monools with 1 to 4 carbon atoms;

[0163] 1,2-Ethylene glycol (also known as ethylene glycol), 1,3-propanediol (also known as propylene glycol), 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 2-buten-1,4-diol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, 1,2-octanediol, 1,2-hexanediol, 1,2-pentanediol, 4-methyl-1,2-pentanediol, and other diols;

[0164] Triols such as glycerol, 1,2,6-hexanetriol, and trimethylolpropane;

[0165] Ethylene glycol monoalkyl ethers, propylene glycol monoalkyl ethers, and other alkylene glycol monoalkyl ethers;

[0166] Diethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, dipropylene glycol, polyoxyethylene polyoxypropylene glycol, and other polyalkylene glycols;

[0167] Diethylene glycol monoalkyl ethers, triethylene glycol monoalkyl ethers, tripropylene glycol monoalkyl ethers, polyoxypropylene glycerol ethers, and other polyalkylene glycol ethers; and

[0168] 2-Pyrrolidone, N-methyl-2-pyrrolidone;

[0169] wait.

[0170] From the viewpoint of ejection stability, the water-soluble organic solvent in the white ink preferably contains at least one selected from the group consisting of glycols and alkylene glycol monoalkyl ethers.

[0171] The content of water-soluble organic solvent relative to the total amount of white ink is preferably 10% to 40% by mass, more preferably 15% to 30% by mass.

[0172] -surfactant-

[0173] White ink may contain at least one surfactant.

[0174] Examples of surfactants include nonionic surfactants, cationic surfactants, anionic surfactants, and betaine surfactants.

[0175] As a preferred surfactant, acetylene glycol-based surfactants, which are a type of nonionic surfactant, can be cited as an example.

[0176] As an acetylene glycol-based surfactant, for example, the acetylene glycol-based surfactant described in paragraphs 0070 to 0080 of International Publication No. 2017 / 149917 can be used.

[0177] Examples of acetylene glycol surfactants include:

[0178] Polyalkylene adducts (preferably polyethylene oxide adducts) of 2,4,7,9-tetramethyl-5-decyn-4,7-diol

[0179] Polyalkylene oxide adducts (preferably polyethylene oxide adducts) of 3,6-dimethyl-4-octyne-3,6-diol

[0180] Polyalkylene adducts (preferably polyethylene oxide adducts) of 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol

[0181] Polyalkylene adduct of 2,5-dimethyl-3-hexyne-2,5-diol (preferably a polyoxyethylene adduct)

[0182] wait.

[0183] Commercially available acetylene glycol surfactants include: the Surfynol series (e.g., Surfynol 420, Surfynol 440, Surfynol 465, Surfynol 485), OLFINE series (e.g., OLFINE E1010, OLFINE E1020), and Dynol series (e.g., Dynol 604) manufactured by Air Products Ltd. or Nissin Chemical Co., Ltd.; and ACETYLENOL manufactured by Kawaken Fine Chemicals Co., Ltd., etc.

[0184] Commercially available acetylene glycol surfactants are also supplied by companies such as The Dow Chemical Company and General Aniline & Film Corp.

[0185] Examples of surfactants include compounds listed on pages 37-38 of Japanese Patent Application Publication No. 59-157636 and Research Disclosure No. 308119 (1989). Furthermore, examples include fluorinated (fluorinated alkyl) surfactants and silicone surfactants described in Japanese Patent Application Publication Nos. 2003-322926, 2004-325707, and 2004-309806.

[0186] When white ink contains surfactants, the surfactant content in the white ink can be appropriately adjusted taking into account the surface energy of the white image to be recorded.

[0187] The surfactant content in the white ink is preferably 0.01% to 5% by mass relative to the total amount of white ink, more preferably 0.05% to 3% by mass, and even more preferably 0.1% to 2% by mass.

[0188] -Other ingredients-

[0189] White ink may contain other ingredients besides those mentioned above.

[0190] Other ingredients include, for example, known additives such as silica compounds (e.g., silica compounds described in paragraphs 0058 to 0075 of Japanese Patent No. 5430316), urea, urea derivatives, waxes, anti-fading agents, emulsion stabilizers, penetration enhancers, ultraviolet absorbers, preservatives, antifungal agents, pH adjusters, defoamers, viscosity modifiers, dispersion stabilizers, and chelating agents.

[0191] -Physical properties-

[0192] From the viewpoint of improving ejection stability, the pH (25°C) of the white ink is preferably 7 to 10, more preferably 7.5 to 9.5. The pH of the ink can be determined using the same method as that used for the pH of the pretreatment solution.

[0193] The viscosity (at 32°C) of the white ink is preferably 0.5 mPa·s to 30 mPa·s, more preferably 2 mPa·s to 20 mPa·s, even more preferably 2 mPa·s to 15 mPa·s, and even more preferably 3 mPa·s to 10 mPa·s.

[0194] The viscosity of white ink is measured using a viscometer (e.g., the TV-22 viscometer manufactured by TOKI SANGYO CO.,LTD.).

[0195] The surface tension (at 25°C) of the white ink is preferably below 60 mN / m, more preferably 20 mN / m to 50 mN / m, and even more preferably 25 mN / m to 40 mN / m.

[0196] Surface tension was measured using a surface tension meter at 25°C, for example, using an automated surface tension meter (product name "CBVP-Z") manufactured by Kyowa Interface Science Co., Ltd., and measured by the plate method.

[0197] (Applying white ink)

[0198] The recording process includes applying white ink to the front side of a non-porous substrate using an inkjet printing method.

[0199] There are no particular restrictions on the ejection method of white ink based on inkjet technology. It can be any of the known methods, such as charge control method that uses electrostatic attraction to eject ink, on-demand inkjet method (pressure pulse method) that uses the vibration pressure of piezoelectric elements, acoustic inkjet method that converts electrical signals into sound beams to irradiate ink and uses radiation pressure to eject ink, and thermal inkjet method (Bubble Jet (registered trademark)) that heats ink to form bubbles and uses the resulting pressure.

[0200] As an inkjet printing method, the method described in Japanese Patent Application Publication No. 54-59936, namely the inkjet recording method, is particularly effective. In this inkjet recording method, the ink undergoes a rapid volume change under the influence of heat energy, and the force generated by this change in state propels the ink out of the nozzle. The method described in paragraphs 0093 to 0105 of Japanese Patent Application Publication No. 2003-306623 is also applicable as an inkjet printing method.

[0201] Applying white ink to the front side of an inkjet-based non-permeable substrate by ejecting white ink from the nozzle of the inkjet head.

[0202] As for inkjet heads, there are reciprocating methods where a short, serial head scans and records simultaneously across the width of the medium being recorded (i.e., a non-permeable substrate; the same applies below), and linear methods where a line head arranges recording elements corresponding to the entire area of ​​one side of the medium being recorded.

[0203] In the inline method, by scanning the recording medium in a direction intersecting the arrangement direction of the recording elements, images can be recorded on the entire surface of the recording medium. The inline method eliminates the need for a transport system such as a carriage, which is required for scanning with short strip-shaped nozzles as in the reciprocating method. Furthermore, compared to the reciprocating method, the inline method eliminates the need for carriage movement and complex scanning control of the recording medium; only the recording medium moves. Therefore, the linear method achieves higher image recording speeds compared to the reciprocating method.

[0204] Applying white ink is preferably done using an inkjet head with a resolution of 300 dpi or higher (more preferably 600 dpi or higher, and even more preferably 800 dpi or higher). Here, dpi is an abbreviation for dots per inch, and 1 inch is 2.54 cm.

[0205] From the viewpoint of obtaining high-definition images, the amount of white ink ejected is preferably 1 pL (picoliter) to 10 pL, more preferably 1.5 pL to 6 pL.

[0206] (Drying of white ink)

[0207] In the recording process, white ink applied to the front side of a non-permeable substrate is heated and dried to obtain a white image.

[0208] There are no particular limitations on the heating and drying methods for white inks. Examples include infrared (IR) drying, warm air blowing (i.e., warm air drying, such as a dryer), and heating drying based on heating devices (e.g., heaters, hot plates, heated rollers, furnaces, etc.).

[0209] As a heating and drying method, it is also possible to combine two or more of these methods.

[0210] Heat drying can be performed by heating the white ink from at least one side of the front and back sides of the non-permeable substrate.

[0211] The heating temperature for drying white ink is preferably 35°C or higher, more preferably 40°C or higher, even more preferably 50°C or higher, and even more preferably 60°C or higher.

[0212] There is no particular limit to the upper limit of the heating temperature, but it is preferably 100°C, and more preferably 90°C.

[0213] There is no particular limitation on the heating time for drying white ink, but it is preferably 1 to 180 seconds, more preferably 1 to 120 seconds, and even more preferably 1 to 60 seconds.

[0214] In the heating and drying of white ink, the rate of temperature rise of the surface of the white ink from the start of heating and drying until 5 seconds have elapsed is "Y" in the aforementioned product (X*Y).

[0215] The range of the product (X*Y) and the preferred range of “Y” are as described above.

[0216] The heating and drying of white ink is preferably carried out by blowing warm air (i.e., warm air drying).

[0217] As a result, the abrasion resistance of white images is further improved.

[0218] -Product(X*Z)-

[0219] In warm air drying, when the value obtained by dividing the wind speed of warm air in m / s units by the temperature of warm air in ℃ units is set as "Z", the product of the aforementioned "X" (i.e., the viscosity of the concentrated ink obtained by concentrating white ink to a mass reduction of 30% at 32℃ (in mPa·s)) and "Z" (hereinafter also referred to as "product (X*Z)") is preferably 0.5 to 18.0, more preferably 1.0 to 15.0, even more preferably 2.0 to 10.0, and even more preferably 3.5 to 7.5.

[0220] When the product (X*Z) is 0.5 or higher, the abrasion resistance of the white image is further improved.

[0221] When the product (X*Z) is below 18.0, the abrasion resistance of the white image is further improved.

[0222] The value of "Z" is preferably 0.04 to 1.20, more preferably 0.10 to 1.00, and even more preferably 0.15 to 0.80.

[0223] -Comparison of [Dry Film Thickness / Wet Film Thickness]-

[0224] In this invention, the value obtained by dividing the film thickness of the white ink applied to the front side of the non-permeable substrate after heat drying (hereinafter also referred to as "dry film thickness" or "A"; in μm) by the film thickness of the white ink applied to the front side of the non-permeable substrate before heat drying (hereinafter also referred to as "wet film thickness" or "B"; in μm) (hereinafter also referred to as "ratio [dry film thickness / wet film thickness]" or "A / B") is preferably 0.10 to 0.30, more preferably 0.10 to 0.25, and even more preferably 0.10 to 0.20.

[0225] When the ratio of dry film thickness to wet film thickness is 0.10 or higher, the concealment of the white image is further improved.

[0226] When the ratio of dry film thickness to wet film thickness is below 0.30, the adhesion of the white image is further improved.

[0227] The wet film thickness of white ink is the film thickness of the white ink (i.e., white ink film) applied to the front side of a non-permeable substrate before heat drying.

[0228] The wet film thickness of white ink is calculated based on the amount of ink ejected from the inkjet head [pL / pixel] and the resolution, expressed in μm and given as a value with two decimal places.

[0229] The dry film thickness of white ink is the film thickness after the white ink film has been heated and dried.

[0230] In other words, the dried film thickness of the white ink is the same as the film thickness of the white image.

[0231] The thickness of the dried film was determined by taking a cross-sectional scanning electron microscope (SEM) image (10,000x magnification) of the image recorder (i.e., a non-permeable substrate with a white image). The thickness of the dried film was measured in μm to two decimal places.

[0232] In the case where the recording method of the present invention includes the winding process described later, the dry film thickness of the white ink is measured by unwinding the image recorder (i.e., a non-permeable substrate with a white image) from the image recorder wound through the winding process and using it as the film thickness of the white image on the unwound image recorder.

[0233] The dry film thickness of the white ink is preferably 0.60 μm to 2.50 μm, more preferably 0.80 μm to 2.00 μm, even more preferably 1.00 μm to 2.00 μm, and even more preferably 1.30 μm to 1.80 μm.

[0234] When the dry film thickness of the white ink is greater than 0.60 μm, the concealment of the white image is further improved.

[0235] When the dry film thickness of the white ink is less than 2.50 μm, the adhesion of the white image is further improved.

[0236] The recording process may also include a process of conveying a non-permeable substrate to which the white ink has been applied via a conveying component in a configuration in which the conveying component comes into contact with the white ink.

[0237] In this case, the non-permeable substrate can be conveyed through a conveying component (e.g., described later) that contacts the white ink (i.e., the front side of the non-permeable substrate). Figure 1 The conveying roller T1 and the conveying components (e.g., described later) that contact the back side of the non-permeable substrate. Figure 1The conveyor roller T2 in the middle is used for this purpose.

[0238] Furthermore, the conveying based on the conveying component can be carried out not only in the recording process, but also throughout the entire recording method of the present invention.

[0239] The recording process further includes a step of conveying a non-permeable substrate to which the white ink has been applied via a conveying member in a configuration where the conveying member contacts the white ink. Furthermore, in the case where the recording method of the present invention includes a winding step of winding up the non-permeable substrate to which the white image has been recorded after the recording step, the average contact surface pressure between the conveying member and the white ink (i.e., the white ink film) from the application of the white ink to the winding up of the non-permeable substrate is preferably 375 N / m. 2 ~4500N / m 2 More preferably 500 N / m 2 ~4500N / m 2 The preferred value is 750 N / m. 2 ~4000N / m 2 .

[0240] When the average contact surface pressure is 375 N / m 2 At the above levels, the transportability of non-permeable substrates is further improved.

[0241] When the average contact surface pressure is 4500 N / m 2 In the following cases, the reduction in film thickness of the white image due to contact with the conveying component can be suppressed, resulting in further improvement in the concealment of the white image.

[0242] Here, when there is only one conveying component in contact with the white ink film, the average contact surface pressure between the conveying component and the white ink film is equal to the contact surface pressure between that one conveying component and the white ink film.

[0243] When there are multiple conveying components in contact with the white ink film, the average contact surface pressure between the conveying components and the white ink film refers to the arithmetic mean of the contact surface pressures between each conveying component and the white ink film.

[0244] When a conveyor roller is used as a conveying component, the contact pressure between the conveyor roller and the white ink film is determined by dividing the tension (N / m) of the non-permeable substrate conveyed by the conveyor roller by the roller radius (m).

[0245] (Record of a colored image)

[0246] The recording process may also include the process of recording a colored image by applying a colored ink containing water, coloring pigments and resin to the front side of a non-permeable substrate using an inkjet method.

[0247] According to this method, it is possible to record multicolor images containing white and colored images on the front side of a non-permeable substrate.

[0248] In this method, only one type of coloring ink can be used to record only one type of colored image (e.g., one of cyan, magenta, yellow and black images), or two or more types of coloring ink can be used to record two or more colored images (e.g., two or more of cyan, magenta, yellow and black images).

[0249] The preferred method for applying colored ink is the same as the preferred method for applying white ink.

[0250] In the recording process, the colored ink applied to the front side of the non-permeable substrate can be heated and dried as needed to obtain a colored image. The preferred method for heating and drying the colored ink in this case is the same as the preferred method for heating and drying the white ink.

[0251] The colored image can be recorded before or after the white image.

[0252] One method of recording a colored image before a white image is, for example, placing the colored image (e.g., a patterned image such as characters or graphics) between the front side of a non-porous substrate and a white image (e.g., a solid image). This method allows for visual identification of the colored image (e.g., a patterned image such as characters or graphics) against a white image (e.g., a solid image) through the non-porous substrate from the back side of the substrate.

[0253] As a method of recording a colored image after a white image, an example is a method in which a colored image (e.g., a patterned image such as characters or graphics) is disposed on a white image (e.g., a solid image). This method is a way of visually recognizing a colored image (e.g., a patterned image such as characters or graphics) on an upper layer as a background of a white image (e.g., a solid image) on an lower layer side from the front side of a non-permeable substrate.

[0254] From the viewpoint of more effectively utilizing the recording method of the present invention, regarding the colored image, it is preferable to record it before the white image and to position it between the front side of the non-porous substrate and the white image.

[0255] -Coloring Inks-

[0256] Coloring inks used to record colored images contain water, coloring pigments (i.e., colored or black pigments), and resin.

[0257] Regarding the preferred method for coloring ink, except for the type of pigment, it is the same as the preferred method for white ink described above.

[0258] Coloring pigments can be either commercially available organic or inorganic pigments.

[0259] As coloring pigments, examples include those described in Seishiro Itō's "Encyclopedia of Pigments" (published in 2000), W. Herbst and K. Hunger's "Industrial Organic Pigments," Japanese Patent Application Publication Nos. 2002-12607, 2002-188025, 2003-26978, and 2003-342503.

[0260] Furthermore, the coloring pigment can be a water-insoluble pigment that can be dispersed in water by a dispersant, or it can be a self-dispersing pigment.

[0261] Self-dispersible pigments are pigments that can be dispersed in water even without the use of a dispersant.

[0262] Self-dispersible pigments are, for example, compounds selected from the group consisting of hydrophilic groups such as carbonyl, hydroxyl, carboxyl, sulfonyl, and phosphate groups and their salts, which are directly or chemically bonded to the pigment surface via other groups.

[0263] From the viewpoint of the concentration of the colored image and the ejectibility of the colored ink, the content of the colored pigment in the colored ink relative to the total amount of the colored ink is preferably 1% to 20% by mass, more preferably 1% to 15% by mass, and even more preferably 1% to 10% by mass.

[0264] <Pretreatment solution application process>

[0265] The recording method of the present invention may further include a step of applying a pretreatment liquid containing water and a coagulant to the front side of a non-permeable substrate (hereinafter also referred to as the "pretreatment liquid application step") before the recording step.

[0266] In this case, during the recording process, the aforementioned white image is recorded by applying the white ink to the area on the front side that has been treated with the pretreatment liquid using an inkjet method.

[0267] According to the method including the pretreatment liquid application process, the components of white ink are coagulated by the action of the coagulant pre-applied to the front side, which is beneficial in terms of the image quality of white images.

[0268] In methods that include the pretreatment liquid application process, in addition to white images, the aforementioned colored images may also be recorded.

[0269] In this case, the aforementioned colored ink is applied to the area on the front side that has been pretreated with the ink by inkjet printing to record the colored image. As a result, the components of the colored ink are agglomerated by the action of a coagulant, thus improving the image quality and other aspects of the colored image.

[0270] As mentioned above, the colored image can be recorded on the upper side of the white image (the side away from the non-permeable substrate) or on the lower side of the white image (the side closer to the non-permeable substrate, i.e., between the front of the non-permeable substrate and the white image), preferably on the lower side of the white image.

[0271] (Pretreatment solution)

[0272] The pretreatment solution contains water and coagulant.

[0273] -water-

[0274] The pretreatment solution contains water.

[0275] The water content relative to the total amount of the pretreatment liquid is preferably 50% by mass or more, and more preferably 60% by mass or more.

[0276] While the upper limit of water content depends on the amount of other components, it is preferably 90% by mass or less, and more preferably 80% by mass or less, relative to the total amount of pretreatment liquid.

[0277] -Flocculant-

[0278] The pretreatment solution contains at least one coagulant.

[0279] The coagulant in the pretreatment solution causes the components in the ink to coagulate on the front side of the non-permeable substrate. This improves the image quality.

[0280] The coagulant is preferably selected from at least one of the group consisting of organic acids, polyvalent metal compounds, metal complexes and cationic polymers.

[0281] As a coagulant, the coagulant described in paragraphs 0122 to 0130 of International Publication No. 2020 / 195360 is preferred.

[0282] The preferred methods for organic acids, polyvalent metal compounds, metal complexes, and cationic polymers that can be used as coagulants are described below.

[0283] --Organic acids--

[0284] Organic acids can be exemplified by organic compounds having acidic groups.

[0285] Examples of acidic groups include phosphate, phosphonic acid, hypophosphonic acid, sulfate, sulfonic acid, sulfinic acid, and carboxyl groups.

[0286] From the perspective of ink coagulation speed, the acidic group is preferably a phosphate group or a carboxyl group, and more preferably a carboxyl group.

[0287] Preferably, at least a portion of the acidic groups dissociate in the pretreatment solution.

[0288] Examples of organic compounds containing a carboxyl group include (meth)acrylic acid, poly(meth)acrylic acid, acetic acid, formic acid, benzoic acid, ethylene glycol, malonic acid, malic acid (preferably DL-malic acid), maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, citric acid, tartaric acid, phthalic acid, 4-methylphthalic acid, lactic acid, pyrrolidone carboxylic acid, pyranone carboxylic acid, pyrrolic carboxylic acid, furan carboxylic acid, pyridine carboxylic acid, coumaric acid, thiophene carboxylic acid, and nicotinic acid.

[0289] From the viewpoint of ink coagulation speed, organic compounds with carboxyl groups are preferably carboxylic acids with a valence of 2 or higher (hereinafter also referred to as polycarboxylic acids), and more preferably dicarboxylic acids.

[0290] Specifically, the polycarboxylic acid is preferably malonic acid, malic acid, maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, tartaric acid, 4-methylphthalic acid, or citric acid, and more preferably malonic acid, malic acid, tartaric acid, succinic acid, glutaric acid, pimelic acid, adipic acid, or citric acid.

[0291] The organic acid is preferably low in pKa (e.g., 1.0 to 5.0). Thus, the surface charge of particles such as pigments and resin particles in inks that are dispersed and stabilized by weakly acidic functional groups such as carboxyl groups is reduced by contact with organic acids with lower pKa, thereby reducing dispersion stability.

[0292] The organic acid is preferably low in pKa, highly soluble in water, and has a valence of 2 or higher. Furthermore, the organic acid is more preferably high in the pH region where it has a lower pKa than the functional group (e.g., carboxyl group) that disperses and stabilizes the particles in the ink.

[0293] --Polyvalent metal compounds--

[0294] As examples of polyvalent metal compounds, polyvalent metal salts can be cited.

[0295] Examples of polyvalent metal salts include organic acid polyvalent metal salts and inorganic acid polyvalent metal salts.

[0296] As a polyvalent metal salt of an organic acid, a polyvalent metal salt of the aforementioned organic acid (e.g., formic acid, acetic acid, benzoic acid, etc.) is preferred.

[0297] As polyvalent metal salts of inorganic acids, polyvalent metal salts of nitrates, polyvalent metal salts of hydrochloric acid, or polyvalent metal salts of thiocyanate are preferred.

[0298] Examples of polyvalent metal salts include salts of alkaline earth metals (e.g., magnesium, calcium) from Group 2 of the periodic table, salts of transition metals (e.g., lanthanum) from Group 3 of the periodic table, salts of metals (e.g., aluminum) from Group 13 of the periodic table, and salts of lanthanides (e.g., neodymium).

[0299] As a multivalent metal salt, calcium salt, magnesium salt, or aluminum salt are preferred, with calcium salt or magnesium salt being more preferred.

[0300] As a polyvalent metal compound, a polyvalent metal salt of an organic acid is preferred, and a calcium salt or a magnesium salt of an organic acid is more preferred.

[0301] Preferably, at least a portion of the polyvalent metal compound dissociates into polyvalent metal ions and counterions in the pretreatment solution.

[0302] --Metal complex--

[0303] The metal complex preferably contains at least one metal element selected from the group consisting of zirconium, aluminum and titanium.

[0304] The metal complex preferably contains at least one metal complex with a ligand selected from the group consisting of acetate, acetylacetonate, methyl acetoacetate, ethyl acetoacetate, octanediol, butoxyacetylacetonate, lactate, ammonium lactate and triethanolamine.

[0305] Metal complexes are commercially available. Various organic ligands, especially multidentate ligands capable of forming metal chelating catalysts, are commercially available. Therefore, metal complexes can be prepared by combining commercially available organic ligands with metals.

[0306] --Catonic polymers--

[0307] The cationic polymer is preferably a homopolymer, copolymer, or condensation polymer of a cationic monomer having primary to tertiary amino or quaternary ammonium groups. As a cationic polymer, it can be used in either the form of a water-soluble polymer or a water-insoluble polymer (i.e., latex particles).

[0308] Examples of cationic polymers include polyvinylpyridine salts, polyalkylaminoethyl acrylates, polyalkylaminoethyl methacrylates, polyvinylimazoles, polyethyleneimine, polybiguanidines, polyguanidines, polyallylamines, and their derivatives.

[0309] From the viewpoint of the viscosity of the pretreatment solution, a low weight-average molecular weight of the cationic polymer is preferred. When the pretreatment solution is applied to a non-permeable substrate by inkjet printing, a weight-average molecular weight of 1,000 to 500,000 is preferred, more preferably 1,500 to 200,000, and even more preferably 2,000 to 100,000. A weight-average molecular weight of 1,000 or higher is advantageous from the viewpoint of coagulation rate. A weight-average molecular weight of 500,000 or lower is advantageous from the viewpoint of ejection reliability. However, this is not a limitation when the pretreatment solution is applied to a non-permeable substrate by methods other than inkjet printing.

[0310] The content of coagulant in the pretreatment liquid relative to the total amount of the pretreatment liquid is preferably 0.1% to 40% by mass, more preferably 0.1% to 30% by mass, even more preferably 1% to 20% by mass, and even more preferably 1% to 10% by mass.

[0311] -Resin-

[0312] The pretreatment solution may contain at least one type of resin.

[0313] The resin in the pretreatment solution contributes to the film-forming properties of the pretreatment solution (i.e., the film-forming properties based on the pretreatment solution).

[0314] As the resin in the pretreatment solution, the same resin (e.g., resin particles) as the resin in the ink can be used.

[0315] There are no particular restrictions on the resin content in the pretreatment solution.

[0316] The resin content relative to the total amount of the pretreatment solution is preferably 0.5% to 30% by mass, more preferably 1% to 20% by mass, and especially preferably 1% to 15% by mass.

[0317] -Water-soluble organic solvents-

[0318] The pretreatment solution may contain at least one water-soluble organic solvent.

[0319] As a water-soluble organic solvent in the pretreatment solution, the same solvent that can be used as the water-soluble organic solvent that the ink may contain can be used.

[0320] -additive-

[0321] Inks may contain additives such as surfactants, water-soluble resins, co-sensitizers, UV absorbers, antioxidants, anti-fading agents, conductive salts, and alkaline compounds, depending on the requirements.

[0322] -Physical properties-

[0323] The pH of the pretreatment solution is preferably 2.0 to 7.0, more preferably 2.0 to 4.0. The pH of the pretreatment solution is determined by the same method as that used for the pH of the ink.

[0324] From the viewpoint of the coatability of the pretreatment solution, the viscosity of the pretreatment solution is preferably 0.5 mPa·s to 10 mPa·s, more preferably 1 mPa·s to 5 mPa·s. The viscosity is the value measured using a viscometer at 25°C. The viscosity of the pretreatment solution is measured using the same method as the viscosity of the ink.

[0325] The surface tension of the pretreatment liquid is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The surface tension is a value measured at 25°C. The surface tension of the pretreatment liquid is measured using the same method as that used for the surface tension of the ink.

[0326] (Method for applying pretreatment solution)

[0327] The method of applying the pretreatment solution is not particularly limited, and well-known methods such as coating, immersion, and inkjet recording can be cited.

[0328] As a coating method, known coating methods include those using bar coaters, die coaters, air knife coaters, blade coaters, bar coaters, knife coaters, extrusion coaters, and reverse roller coaters.

[0329] (Drying of the pretreatment solution)

[0330] The pretreatment liquid application process may include a process of drying the pretreatment liquid applied to the front side of a non-permeable substrate.

[0331] There are no particular limitations on the drying method used as a pretreatment liquid; for example, the same method exemplified as the drying method for white ink can be applied.

[0332] The preferred range of drying conditions (e.g., heating temperature and heating time) for the pretreatment solution is the same as the preferred range of drying conditions for the white ink.

[0333] <Winding Process>

[0334] The recording method of the present invention may include a winding process of winding up a non-permeable substrate on which a white image is recorded.

[0335] Regarding the winding process, there are no particular limitations, and it can be carried out using a known winding device that includes a winding core.

[0336] The recording method of the present invention may also include other steps besides those described above.

[0337] <Image Recording Device>

[0338] The image recording apparatus used in the image recording method of the present invention includes:

[0339] An inkjet head is used to apply the aforementioned white ink to one surface of the aforementioned non-permeable substrate; and

[0340] A heating and drying apparatus for heating and drying the aforementioned white ink.

[0341] In this image recording device,

[0342] The product of X and Y is 30 to 280.

[0343] The image recording apparatus described above can achieve the same effect as the image recording method of the present invention described above.

[0344] <An example of an image recording device>

[0345] Figure 1 This is a diagram that conceptually illustrates an example of an image recording apparatus used in the image recording method of the present invention.

[0346] like Figure 1 As shown, the image recording apparatus involved in this example is an example of an image recording apparatus equipped with a transport mechanism for transporting non-permeable substrates in a roll-to-roll manner. The apparatus is as follows: a non-permeable substrate A1, which is rolled into a roll shape, is unwound by an unwinding device R1. The unwound non-permeable substrate A1 is transported in the direction of the arrow under tension, and is sequentially passed through a pretreatment liquid application device P1, a pretreatment liquid drying zone DP1, a first inkjet head IJ1, a first drying zone D1, a second inkjet head IJ2, and a second drying zone D2. Then, it is transported by transport rollers T1 and T2, which are transport components, and finally, it is wound up by a winding device R2.

[0347] The non-permeable substrate A1 can be conveyed under tension. Furthermore, the tension can vary depending on the position of the conveying direction, or it can be the same tension.

[0348] The image recording apparatus described in this example may include a tension adjustment mechanism for adjusting the tension of a non-permeable substrate.

[0349] Examples of tension adjustment mechanisms include:

[0350] A powder brake is installed in the unwinding device R1 and / or the winding device R2.

[0351] Tension adjustment rollers (dancer rollers) installed along the conveying path; and

[0352] A control device (e.g., a tension controller) that controls tension by adjusting various conditions of the image recording device.

[0353] wait.

[0354] In addition, due to Figure 1 This is a conceptual diagram, thus simplifying the transport path of the non-permeable substrate A1. It is shown as the non-permeable substrate A1 being transported in one direction between the unwinding device R1 and the transport roller T1, but the transport path of the non-permeable substrate A1 can of course be curved.

[0355] As a conveying method for non-permeable substrate A1, various web conveying methods such as cylinders and rolls can be appropriately selected.

[0356] Relative to the unwinding device R1 used for unwinding the non-permeable substrate A1, on the downstream side of the conveying direction of the non-permeable substrate A1, from the upstream side of the conveying direction of the non-permeable substrate A1, a pretreatment liquid application device P1, a pretreatment liquid drying zone DP1, a first inkjet head IJ1, a first drying zone D1, a second inkjet head IJ2, a second drying zone D2, a transport roller T1, and a transport roller T2 are arranged in sequence.

[0357] The pretreatment liquid is applied by the pretreatment liquid application device P1, the first inkjet head IJ1 and the second inkjet head IJ2 respectively.

[0358] At this time, at least one of the following can be performed: heating and drying of the pretreatment liquid in the pretreatment liquid drying zone DP1, heating and drying of the first ink in the first drying zone D1, and heating and drying of the second ink in the second drying zone D2.

[0359] In the first drying zone D1, in addition to the heating and drying of the first ink, the pretreatment liquid can also be heated and dried.

[0360] In the second drying zone D2, in addition to the heating and drying of the second ink, the heating and drying of the pretreatment liquid and / or the heating and drying of the first ink can also be carried out. In this case, at least one of the pretreatment liquid drying zone DP1 and the first drying zone D1 can be omitted.

[0361] Furthermore, if the non-permeable substrate is passed through each drying zone while the temperature of each drying zone is set to room temperature, the heating and drying in each drying zone can be omitted.

[0362] In this example, the first ink is either a coloring ink for recording a colored image or a white ink for recording a white image, and the second ink is the other of the aforementioned coloring ink and white ink.

[0363] Coloring inks contain water, coloring pigments, and resins.

[0364] White ink contains water, white pigment, and resin.

[0365] The white ink used in the image recording method of the present invention can be used as the first ink in this example, or it can be used as the second ink in this example.

[0366] Relative to the pretreatment liquid application device P1, on the upstream side, a surface treatment section (not shown) may be provided for performing surface treatment (preferably corona treatment) on at least one of the front (i.e., image recording surface) and back (i.e., image non-recording surface) of the non-permeable substrate A1.

[0367] Furthermore, a cooling zone may be provided downstream of the second drying zone D2 to cool the recorded multicolor image (i.e., a multicolor image including a white image and a colored image).

[0368] The first inkjet head IJ1 and the second inkjet head IJ2 can be reciprocating inkjet heads, but from the viewpoint of high-speed image recording, it is preferable to have a row head with multiple nozzles arranged in the width direction of the non-permeable substrate A1 in the shape of a long strip film.

[0369] The first inkjet head IJ1 and the second inkjet head IJ2 can each be a single unit or multiple units.

[0370] As an example of the combination of the first inkjet head IJ1 and the second inkjet head IJ2, the following combination can be given: the first inkjet head IJ1 is four inkjet heads corresponding to the four colors of cyan, magenta, yellow and black (note: these four inkjet heads are arranged along the transport direction of the non-permeable substrate), and the second inkjet head IJ2 is one inkjet head corresponding to white (i.e., white).

[0371] Furthermore, as another example of the combination of the first inkjet head IJ1 and the second inkjet head IJ2, the following combination can also be given: the first inkjet head IJ1 is one inkjet head corresponding to white (i.e., white), and the second inkjet head IJ2 is four inkjet heads corresponding to the four colors of cyan, magenta, yellow and black (Note: these four inkjet heads are arranged along the transport direction of the non-permeable substrate).

[0372] In inkjet recording using the image recording device described in this example,

[0373] First, the non-permeable substrate A1, which is wound into a roll shape, is unwound by the unwinding device R1.

[0374] The released non-permeable substrate A1 is conveyed along the direction of the arrow in the block under tension.

[0375] The pretreatment liquid is applied to the non-permeable substrate A1 using the pretreatment liquid application device P1.

[0376] Next, the pretreatment solution is dried at the pretreatment solution drying zone DP1 as needed.

[0377] Next, the first ink (i.e., either colored ink or white ink) is applied through the first inkjet head IJ1.

[0378] Next, the first ink is dried in the first drying zone D1 as needed.

[0379] Next, the second ink (i.e., the other of the colored ink and white ink) is applied through the second inkjet head IJ2.

[0380] Next, the second ink is dried in the second drying zone D2 as needed.

[0381] Thus, a multicolor image can be obtained, which includes a first image (i.e., either the colored image or the white image) derived from the first ink and a second image (i.e., the other of the colored image or the white image) derived from the second ink.

[0382] Next, the obtained multicolor images are cooled as needed, and the non-permeable substrate A1 on which the multicolor images are recorded is conveyed to the winding device R2 by the conveying rollers T1 and T2, which are the conveying components, and finally wound up by the winding device R2.

[0383] In conveying rollers T1 and T2, conveying roller T1 is configured to contact the front side of non-permeable substrate A1 to convey non-permeable substrate A1, and conveying roller T2 is configured to contact the back side of non-permeable substrate A1 to convey non-permeable substrate A1.

[0384] The conveyor roller T1 is an example of a conveying member configured to contact the white ink between the application of the white ink and the winding of the non-permeable substrate A1. In the image recording apparatus described in this example, there may also be conveying members configured to contact the white ink other than the conveyor roller T1.

[0385] The preferred range of average contact pressure between the transport component and the white ink from the application of white ink to the winding of the non-permeable substrate is as described above.

[0386] In addition, the application and drying of the pretreatment solution in this example can be omitted.

[0387] Furthermore, in this example, it is possible to record only the white image instead of the colored image.

[0388] Example

[0389] The following are embodiments of the present invention, but the present invention is not limited to the following embodiments.

[0390] <Preparation of Pretreatment Solution>

[0391] The pretreatment solution was prepared by mixing the following components.

[0392] -Composition of the pretreatment solution-

[0393] Glutaric acid (coagulant)

[0394] ...6.1% by weight

[0395] Propylene glycol (PG) [water-soluble organic solvent]

[0396] ...20% by mass

[0397] • OLFINE E1010 (manufactured by Nissin Chemical Co., Ltd.) [surfactant]

[0398] ...0.5% by mass

[0399] ·SUPER FLEX 500M (DKS Co., Ltd.) [Aqueous dispersion of urethane resin particles]

[0400] ...7.0% of mass

[0401] Triisopropanolamine (pH adjuster)

[0402] ...0.2% by mass

[0403] • BYK024 (BYK Corporation) [Defoamer]

[0404] ...0.01% by mass

[0405] Ultrapure water

[0406] ...the pretreatment solution becomes 100% by mass as a whole.

[0407] <Preparation of White Ink>

[0408] (Preparation of white ink W1)

[0409] White ink W1 was prepared by mixing the following ingredients.

[0410] -Composition of white ink W1-

[0411] • The following white pigment dispersion 1

[0412] ...17% by mass based on the content of white pigment.

[0413] Propylene glycol (PG) [water-soluble organic solvent]

[0414] ...28% by mass

[0415] Propylene glycol monomethyl ether (PGmME) [water-soluble organic solvent]

[0416] ...5% by mass

[0417] • OLFINE E1010 (manufactured by Nissin Chemical Co., Ltd.) [acetylene glycol-based surfactant]

[0418] ...0.60% by mass

[0419] • BYK-3450 (BYK Corporation) [Silicone-based surfactant]

[0420] ...0.75% by mass

[0421] • BYK024 (BYK Corporation) [Defoamer]

[0422] ...0.02% by mass

[0423] SOLSPERSE 43000 (manufactured by The Lubrizol Corporation) [Polymer Dispersant]

[0424] ...0.75% by mass

[0425] Joncryl JDX-6180 (manufactured by BASF) [water-soluble polymer]

[0426] ...1.1% by mass

[0427] • PVP-K15 (Polyvinylpyrrolidone K15)

[0428] ...0.12% by mass

[0429] • SNOWTEX XS (manufactured by Nissan Chemical Corporation) [Colloidal silica dispersion]

[0430] ...based on the content of colloidal silica particles, it is 0.1% by mass.

[0431] ·water

[0432] ...the white ink constitutes a 100% mass surplus.

[0433] (Preparation of white pigment dispersion 1 (containing block polymer dispersant))

[0434] -Synthesis of Block Polymer Dispersant 1-

[0435] Referring to Synthesis Example 8 of Japanese Patent Application Publication No. 2015-83688, a block polymer dispersant 1 was synthesized as a pigment dispersant for white pigment dispersion 1. Details are shown below.

[0436] Add to a reaction apparatus consisting of a 1L separable flask equipped with a stirrer, reflux condenser, thermometer, and nitrogen inlet pipe.

[0437] Diethylene glycol dimethyl ether (266 parts by weight; polymerization solvent)

[0438] 2-Iodo-2-cyanopropane (6.2 parts by mass; polymerization initiator compound),

[0439] Methyl methacrylate (MMA) (120 parts by weight; monomer),

[0440] Acrylic acid (AA) (28.8 parts by weight; monomer),

[0441] Cyclohexyl methacrylate (CHMA) (67.2 parts by weight; monomer),

[0442] Azobis(dimethyl)isovalerate (7.9 parts by weight) and

[0443] 2-tert-butyl-4,6-dimethylphenol (0.7 parts by weight; catalyst),

[0444] Nitrogen gas was passed through the mixture while it was being stirred.

[0445] Next, the temperature of the mixture in the reaction apparatus (reaction temperature) was raised to 70°C and polymerization was carried out for 3 hours to obtain a polymerization solution A containing MMA / AA / CHMA copolymer.

[0446] Three hours later, a portion of the above-mentioned polymerization solution A was sampled and the solid content was measured, which was 42.0% by mass, confirming that most of the monomers had been polymerized.

[0447] Furthermore, the molecular weight of the MMA / AA / CHMA copolymer was determined by GPC, and the weight-average molecular weight (Mn) was 7,500.

[0448] The acid value of this MMA / AA / CHMA copolymer is 101.0 mg KOH / g.

[0449] Next, a mixture of benzyl methacrylate (BzMA) (35.2 parts by mass; monomer) and V-65 (0.3 parts by mass; free radical generator) was added to the above polymerization solution A, and the mixture was polymerized at 70°C for 3 hours to obtain polymerization solution B containing block polymer dispersant 1.

[0450] Here, the block polymer dispersant 1 is a block polymer containing an MMA / AA / CHMA copolymer, i.e., block A, and a BzMA homopolymer, i.e. block B.

[0451] The solid content of the obtained polymerization solution B was determined to be 43.2% by mass, confirming that most of the monomers had been polymerized.

[0452] Furthermore, the block polymer dispersant 1 has a Mw of 8,500 and an acid value of 89.3 mg KOH / g.

[0453] Preparation of White Pigment Dispersion 1

[0454] The block polymer dispersant 1 (136.4 parts by mass), butylcarbitol (163.6 parts by mass), and CI Pigment White 6 (trade name "JR-405", rutile titanium dioxide particles, manufactured by TAYCA CORPORATION) (450 parts by mass), used as a white pigment, were blended and stirred using a disperser. Then, the white pigment was thoroughly dispersed using a horizontal media disperser to obtain an oily pigment dispersion. The average particle size of the white pigment dispersed in the oily pigment dispersion was 290 nm. The viscosity of the oily pigment dispersion was 86.3 mPa·s.

[0455] Next, while stirring the above-mentioned oily pigment dispersion (700 parts by weight) using a disperser, a mixture of potassium hydroxide (4.0 parts by weight) and water (341 parts by weight) was slowly added to it and neutralized. Then, the white pigment was thoroughly dispersed using a horizontal media disperser to obtain a pigment dispersion.

[0456] Next, the obtained pigment dispersion was subjected to ultrafiltration using a cross-flow ultrafiltration (UF) apparatus (manufactured by Sartorius) with a flow rate of 600 mL / min flowing into deion-exchanged water. The liquid temperature was maintained at 25°C, and ultrafiltration was performed 10 times, with each cycle consisting of one volume of the prepared liquid. After adding deion-exchanged water, a white pigment dispersion 1 with a concentration of 45% by mass and a block polymer dispersant 1 concentration of 3.7% by mass was obtained.

[0457] (Preparation of white ink W2)

[0458] In the preparation of the white ink, NEOCRYL A1091 (manufactured by Covestro Coating Resins) [an aqueous dispersion of styrene-acrylic resin particles] (0.75% by mass based on the content of styrene-acrylic resin particles) was added. Otherwise, white ink W2 was prepared in the same manner as white ink W1.

[0459] (Preparation of white ink W3)

[0460] In the preparation of the white ink, NEOCRYL A1091 (manufactured by Covestro Coating Resins) [an aqueous dispersion of styrene-acrylic resin particles] (1.85% by mass based on the content of styrene-acrylic resin particles) was added, and Joncryl JDX-6180 (manufactured by BASF) was not used. Otherwise, white ink W3 was prepared in the same manner as white ink W1.

[0461] (Preparation of white ink W4)

[0462] Instead of white pigment dispersion 1 (containing block polymer dispersant), white pigment dispersion 2 (containing random polymer dispersant) was used. Otherwise, white ink W4 was prepared in the same manner as white ink W2.

[0463] (Preparation of white pigment dispersion 2 (containing random polymer dispersant))

[0464] -Synthesis of Random Polymer Dispersant 1-

[0465] Add 965 g of dipropylene glycol to a 5000 mL three-necked flask equipped with a stirrer and cooling tube, and heat to 85 °C under a nitrogen atmosphere.

[0466] The following were prepared respectively:

[0467] Solution I was obtained by dissolving 640 g of benzyl methacrylate, 340 g of methacrylic acid, and 19.94 g of 2-mercaptopropionic acid in 370.28 g of dipropylene glycol; and

[0468] Solution II was obtained by dissolving 17.69 g of tert-butyl peroxide (2-ethylhexanoate) (product name "PERBUTYL O", manufactured by NOF CORPORATION) in 221.17 g of dipropylene glycol.

[0469] Solution I was added dropwise to the three-necked flask over 4 hours, and solution II was added dropwise over 5 hours. After the additions were completed, the mixture was allowed to react further for 2 hours. 1 H-NMR confirmed the disappearance of the monomer.

[0470] The obtained reaction solution was heated to 70°C, and 248.02 g of 50% potassium hydroxide aqueous solution was added to it. Then, 107.48 g of dipropylene glycol and 75.52 g of pure water were added and stirred to obtain a 37% solution of random polymer dispersant 1.

[0471] pass 1 ¹H-NMR confirmed the structural units constituting the obtained random polymer dispersant 1. Furthermore, the weight-average molecular weight (Mw) was determined by GPC. The obtained random polymer dispersant 1 has a weight-average molecular weight (Mw) of 8400 and an acid value of 221.7 mg KOH / g.

[0472] Preparation of White Pigment Dispersion 2 (containing random polymer dispersant) -

[0473] Random polymer dispersant 1 (150 parts by mass) was dissolved in water to prepare a polymer solution with a concentration of 25% by mass.

[0474] The above polymer solution was mixed with 96 parts by mass of CI Pigment White 6 (trade name "JR-405", rutile titanium dioxide particles, manufactured by TAYCA Co., Ltd.) as a white pigment and 270 parts by mass of water to obtain a mixture. A potassium hydroxide aqueous solution was added to the obtained mixture to adjust the pH to 8.7 after neutralization.

[0475] Next, the neutralized mixture was dispersed for 3 hours using a bead mill (bead diameter: 0.1 mmφ, zirconia beads). This yielded a white pigment dispersion A (uncrosslinked dispersion) PD1, in which white pigment was dispersed by pigment dispersant P1.

[0476] Next, the obtained white pigment dispersion (uncrosslinked dispersion) PD1 was ultrafiltered using an ultrafiltration apparatus (cross-flow ultrafilter (UF), manufactured by Sartorius) with 600 mL of deion-exchanged water flowing in at a rate of 1 minute. The liquid temperature was maintained at 25°C, and three ultrafiltration cycles were performed, with each cycle consisting of one volume of the prepared liquid. Deion-exchanged water was added to the ultrafiltered liquid to obtain white pigment dispersion 2 with a white pigment concentration of 45% by mass and a random polymer dispersant 1 concentration of 3.6% by mass.

[0477] <Viscosity Determination of White Ink and Concentrated Ink>

[0478] The viscosity (X) of each of the white inks W1 to W4 and the concentrated ink were measured. The thickening rate (%) was calculated based on the viscosity and the concentrated ink viscosity.

[0479] These results are shown in Table 1.

[0480] These viscosities were measured using a TV-22 viscometer manufactured by Toki Sangyo Co., Ltd., at 32°C.

[0481] Furthermore, the concentrated ink is prepared as follows: white ink is heated and the solvent (i.e., water and water-soluble organic solvents) is removed by distillation until the mass is reduced by 30%.

[0482] [Table 1]

[0483]

[0484] <Preparation of Coloring Inks>

[0485] As coloring inks, cyan ink, black ink, magenta ink and yellow ink were prepared.

[0486] Each ink was prepared by mixing the components shown in the following ink compositions.

[0487] -Composition of cyan ink-

[0488] • APD4000 Cyan (manufactured by Fujifilm Imaging Colorants Ltd.) [Cyan Pigment Dispersion]

[0489] ...with a cyan pigment content of 4.0% by mass

[0490] Propylene glycol monomethyl ether (PGmME) [water-soluble organic solvent]

[0491] ...3% by mass

[0492] Propylene glycol (PG) [water-soluble organic solvent]

[0493] ...20% by mass

[0494] Neocryl A-1105 (manufactured by DSM) [Acrylic resin particle dispersion]

[0495] ...5.0% by mass, based on the content of resin particles.

[0496] • OLFINE E1010 (manufactured by Nissin Chemical Co., Ltd.) [acetylene glycol-based surfactant]

[0497] ...1.0% of mass

[0498] • BYK3450 (manufactured by BYK Corporation) [Silicone-based surfactant]

[0499] ...1.0% of mass

[0500] ·PVPK15 (Polyvinylpyrrolidone K15)

[0501] ...0.15% by mass

[0502] ST-XS (manufactured by Nissan Chemical Corporation) [Colloidal silica dispersion]

[0503] ...based on the content of colloidal silica particles, it is 0.05% by mass.

[0504] ·water

[0505] ...the ink as a whole becomes 100% by mass of the remainder.

[0506] -Composition of black ink-

[0507] • APD4000 Black (manufactured by Fujifilm Imaging Colorants Ltd.)

[0508] ...4.0% by weight, based on pigment content.

[0509] Propylene glycol (PG) [water-soluble organic solvent]

[0510] ...20% by mass

[0511] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0512] ...1.0% of mass

[0513] Neocryl A-1105 (Acrylic Resin Particle Dispersion) (Manufactured by DSM)

[0514] ...5.0% by mass, based on the content of resin particles.

[0515] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0516] ...1.0% of mass

[0517] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0518] ...1.0% of mass

[0519] ·PVPK15 (Polyvinylpyrrolidone K15)

[0520] ...0.15% by mass

[0521] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0522] ...based on the content of colloidal silica particles, it is 0.05% by mass.

[0523] ·water

[0524] ...the ink as a whole becomes 100% by mass of the remainder.

[0525] -Composition of magenta ink-

[0526] • APD4000 Magenta (manufactured by Fujifilm Imaging Colorants Ltd.)

[0527] ...5.0% by weight, based on pigment content.

[0528] Propylene glycol (PG) [water-soluble organic solvent]

[0529] ...20% by mass

[0530] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0531] ...1.0% of mass

[0532] Neocryl A-1105 (Acrylic Resin Particle Dispersion) (Manufactured by DSM)

[0533] ...5.0% by mass, based on the content of resin particles.

[0534] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0535] ...1.0% of mass

[0536] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0537] ...1.0% of mass

[0538] ·PVPK15 (Polyvinylpyrrolidone K15)

[0539] ...0.15% by mass

[0540] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0541] ...based on the content of colloidal silica particles, it is 0.05% by mass.

[0542] ·water

[0543] ...the ink as a whole becomes 100% by mass of the remainder.

[0544] -Preparation of Yellow Ink-

[0545] ·APD4000 Yellow (manufactured by Fujifilm Imaging Colorants Ltd.)

[0546] ...4.0% by weight, based on pigment content.

[0547] Propylene glycol (PG) [water-soluble organic solvent]

[0548] ...20% by mass

[0549] Propylene glycol monomethyl ether (water-soluble organic solvent)

[0550] ...1.0% of mass

[0551] Neocryl A-1105 (Acrylic Resin Particle Dispersion) (Manufactured by DSM)

[0552] ...5.0% by mass, based on the content of resin particles.

[0553] •Olfine E1010 (an acetylene glycol-based surfactant manufactured by Nissin Chemical Co., Ltd.)

[0554] ...1.0% of mass

[0555] • BYK3450 (a silicone-based surfactant manufactured by BYK Corporation)

[0556] ...1.0% of mass

[0557] ·PVPK15 (Polyvinylpyrrolidone K15)

[0558] ...0.15% by mass

[0559] ST-XS (Colloidal Silica Dispersion) (Manufactured by Nissan Chemical Corporation)

[0560] ...based on the content of colloidal silica particles, it is 0.05% by mass.

[0561] ·water

[0562] ...the ink as a whole becomes 100% by mass of the remainder.

[0563] <Preparation of Image Recording Device>

[0564] As an image recording device, the aforementioned [equipment / device] is prepared. Figure 1 The image recording device shown.

[0565] A concave plate coating machine was used as the pretreatment liquid application device P1.

[0566] The drying method in the pretreatment liquid drying zone DP1 is set to warm air drying.

[0567] As the first inkjet head IJ1, four inkjet heads—a cyan inkjet head, a magenta inkjet head, a yellow inkjet head, and a black inkjet head—are arranged in this order from the upstream side (i.e., upstream of the direction of transport of the non-permeable substrate).

[0568] The IJ2, as the second inkjet head, is equipped with an inkjet head for white inkjet printing.

[0569] All inkjet heads and ink ejection conditions are as follows.

[0570] • Inkjet head: Uses a 1200dpi (dots per inch, 1 inch is 2.54cm) / 20-inch width piezo full line head (total number of nozzles 2048).

[0571] • Ink ejection volume: Set to 3.0 pL.

[0572] • Drive frequency: Set to 30kHz.

[0573] The drying method in both the first drying zone D1 and the second drying zone D2 is set to warm air drying. The drying method in the second drying zone D2 is configured to be switchable between infrared (IR) drying and heated drum drying.

[0574] Both conveyor rollers T1 and T2 are made of aluminum rollers (0.05m radius) that have undergone anodizing (almite treatment).

[0575] <Preparation of Non-Opermeable Substrates>

[0576] As a non-permeable substrate, a polyethylene terephthalate (PET) substrate "Taiko polyester film (25 μm thick)" manufactured by FUTAMURA CHEMICAL CO.,LTD. was prepared.

[0577] The “Taiko Polyester Film (25μm Thickness)” is a roll of a long strip of PET substrate with a thickness of 25μm and a width of 800mm.

[0578] [Experiment Nos. 1-44]

[0579] <Image Recording>

[0580] Using the aforementioned image recording apparatus, the aforementioned pretreatment liquid, and the aforementioned white ink as the second ink, inkjet recording was performed to obtain a non-permeable substrate with a white image, i.e., an image recording object.

[0581] In this image recording, the coloring inks used as the first ink (i.e., cyan ink, black ink, magenta ink, and yellow ink) were not used.

[0582] As the second ink, any one of the aforementioned white inks W1 to W4 was used (refer to Tables 2 and 3).

[0583] First, the non-permeable substrate is unwound from the roll using the unwinding device R1.

[0584] The released non-permeable substrate is conveyed under tension.

[0585] The gravure coating machine, which serves as the pretreatment liquid application device P1, applies the pretreatment liquid to the front side of the conveyed non-permeable substrate.

[0586] Next, the pretreatment solution is dried at the pretreatment solution drying zone DP1.

[0587] Next, white ink, serving as the second ink, is applied through the second inkjet head IJ2.

[0588] Next, the white ink, which was used as the second ink, was dried in the second drying zone D2.

[0589] Through the above operations, a white image is recorded on the front side of the conveyed non-permeable substrate, resulting in a non-permeable substrate with a white image, i.e., an image recording object.

[0590] Next, the obtained image recording is conveyed by conveyor rollers T1 and T2, and then wound up by the winding device R2.

[0591] In the above inkjet recording, the transport speed of the non-permeable substrate was set to 50 m / min.

[0592] The amount of pretreatment solution administered was set at 3.0 g / m³. 2 .

[0593] The drying conditions for the pretreatment liquid were set as follows: warm air temperature 80℃, warm air velocity 20m / s, and drying time 3 seconds.

[0594] The application amount of the second ink (white ink) is set at 3.0 g / m. 2 .

[0595] The drying method and conditions (i.e., heating rate, and the temperature and pressure of the warm air) for the second ink (white ink) are shown in Tables 2 and 3. The drying time is fixed at 40 seconds.

[0596] The heating rate was defined as the rate at which the surface temperature rose from the start of the heating and drying process until 5 seconds had elapsed. The heating rate was determined by measuring the surface temperature of the white ink applied to the front side of the non-permeable substrate.

[0597] <Determination of Dry Film Thickness and Wet Film Thickness>

[0598] The film thickness (wet film thickness (μm); B) of the white ink on the front side of the non-permeable substrate after the white ink is applied by the second inkjet head IJ2 and before drying in the second drying zone D2 is calculated based on the amount of ink ejected from the inkjet head [pL / pixel] and the resolution, in μm, as a value with two decimal places.

[0599] Furthermore, the film thickness (dry film thickness (μm); A) of the white ink on the front side of the non-permeable substrate was measured in μm, with two decimal places, by unwinding the image recorder after it was wound up and taking a cross-sectional SEM image (magnification 10,000x) of the unwound image recorder.

[0600] The value (A / B) is obtained by dividing the dry film thickness (A) by the wet film thickness (B).

[0601] These results are shown in Tables 2 and 3.

[0602] <Contact surface pressure with conveyor roller T1>

[0603] By dividing the tension (N / m) of the non-permeable substrate at the location of the conveyor roller T1 by the radius of the conveyor roller T1 (i.e., 0.05m), the contact pressure (N / m) between the white image and the conveyor roller T1 was calculated. 2 ).

[0604] The results are shown in Tables 2 and 3.

[0605] <Evaluation>

[0606] The following evaluation was performed on the white image obtained through the above image recording.

[0607] The results are shown in Tables 2 and 3.

[0608] In the remarks column of Tables 2 and 3, “Ex.” and “Com.” respectively represent the examples and comparative examples (the same applies to Tables 4 and thereafter).

[0609] (concealment)

[0610] An image recording was placed on the black portion of a concealment rate test strip (JIS compliant) manufactured by TP Giken Co., Ltd. with the white image in contact with the black portion of the image recording, and the concealment power (%) of the white image was measured. The concealment power was measured using x-rite eXact Advanced from X-Rite, Inc. (see https: / / www.xrite.co.jp / allproduct / qa / 99-exact / 588-pqa0111.html).

[0611] In the following evaluation criteria, the highest level of concealment is A.

[0612] -Evaluation criteria for concealment-

[0613] A: Concealment rate is above 56.0%.

[0614] B: Concealment rate is 54.5% or higher but less than 56.0%.

[0615] C: Concealment rate is above 53.0% and less than 54.5%.

[0616] D: Concealment capability less than 53.0%.

[0617] (Seamless fit)

[0618] For the white images in the above image recordings, a cross-hatch test was performed according to ISO 2409 (cross-cut method), and the image fit was evaluated according to the following evaluation criteria.

[0619] In the following evaluation criteria, the highest grade for image fit is "A".

[0620] In this 100-grid test, 25 square grids, each 1 mm in size, were formed with a 1 mm cutting interval.

[0621] In the following evaluation criteria, the percentage (%) of cells stripped is a value obtained by the following formula. The total number of cells in the following formula is 25.

[0622] Percentage of cells stripped (%) = [(Number of cells stripped) / (Total number of cells)] × 100

[0623] In the following evaluation criteria, the highest level of fit is A.

[0624] -Evaluation criteria for tightness-

[0625] A: The percentage of grid cells stripped is between 0% and 5%.

[0626] B: The percentage of grid cells stripped (%) is more than 5% and less than 15%.

[0627] C: The percentage of grids that are stripped is greater than 15% and less than 35%.

[0628] D: The percentage of cells stripped exceeds 35%.

[0629] (In-surface unevenness)

[0630] The concealment power (%) of the white image was measured at 10 points along the width direction of the aforementioned image record using the aforementioned concealment power measurement method. The maximum and minimum values ​​of the concealment power at the 10 points were determined, and the value obtained by subtracting the minimum value from the maximum value was set as Δ. Based on the value of Δ, the in-plane inhomogeneity of the white image was evaluated according to the following evaluation criteria.

[0631] In the following evaluation criteria, the highest level of in-plane non-uniformity suppression is A.

[0632] -Evaluation criteria for in-plane non-uniformity-

[0633] A: Δ is less than 1.0

[0634] B: Δ is greater than 1.0 and less than 2.0

[0635] C: Δ is greater than 2.0 and less than 3.0

[0636] D: Δ is 3.0 or higher

[0637] (Abrasion resistance)

[0638] The white image in the aforementioned image record was repeatedly rubbed with a paperweight wrapped with friction paper. OK TopKote 104 (manufactured by OOji Paper Co., Ltd.) was used as the friction paper. The rubbing operation was performed with a weighted intensity of 4.0 N.

[0639] The color shift from the solid image to the rubbed paper was observed with the naked eye, and the abrasion resistance of the image was evaluated according to the following evaluation criteria.

[0640] In the following evaluation criteria, the highest grade for abrasion resistance of the image is "A".

[0641] -Evaluation criteria for wear resistance-

[0642] A: At the point when 200 rubbing operations were completed, no color shift from the solid image to the rubbing paper was visually detected.

[0643] B: At the point when 200 rubbing operations were completed, a color shift from the solid image to the rubbing paper was visually recognized, but at the point when 100 rubbing operations were completed, a color shift from the solid image to the rubbing paper was not visually recognized.

[0644] C: At the point when 100 rubbing operations were completed, a color shift from the solid image to the rubbing paper was visually recognized, but at the point when 20 rubbing operations were completed, a color shift from the solid image to the rubbing paper was not visually recognized.

[0645] D: At the point when 20 rubbing operations are completed, a color shift from the white image to the rubbing paper is visually recognized.

[0646] [Experiment numbers 101-106]

[0647] The white ink shown in Table 4 was used as the white ink, and the amount of white ink applied was adjusted so that the wet film thickness (μm) was the value shown in Table 4. Otherwise, the same operation as in test number 2 was performed.

[0648] The results are shown in Table 4.

[0649] [Experiment numbers 201-228]

[0650] The conditions for drying the warm air (temperature and wind speed) were changed as shown in Table 5. Otherwise, the same operations as in test number 2 were performed.

[0651] The results are shown in Table 5.

[0652] [Experiment numbers 301-306]

[0653] By adjusting the tension applied to the non-permeable substrate, the contact surface pressure between the white image and the conveyor roller T1 was changed as shown in Table 6. Otherwise, the same operation as in test number 2 was performed.

[0654] The results are shown in Table 6.

[0655] [Table 2]

[0656]

[0657] [Table 3]

[0658]

[0659] [Table 4]

[0660]

[0661] [Table 5]

[0662]

[0663] [Table 6]

[0664]

[0665] As shown in Tables 2 to 6, the white images exhibit superior concealment compared to the comparative examples (Com.) with a product (X*Y) of 30 to 280. From Test No. 1 (Comparative Example) and Test Nos. 2, 5, 9, and 13 (all Examples), it can be seen that, regardless of the drying method, an improved concealment effect can be achieved by having a product (X*Y) of 30 or higher.

[0666] Furthermore, the white images in each embodiment (Ex.) exhibited superior adhesion compared to the comparative examples (Com.) where the product (X*Y) exceeded 280. As can be seen from test number 44 (comparative example) and test numbers 32, 36, 40, and 43 (all examples), improved adhesion can be achieved by having a product (X*Y) of 280 or less, regardless of the drying method.

[0667] For example, a comparison between test number 2 and test number 3 shows that when the product (X*Y) is above 40, the concealment of the white image is further improved.

[0668] For example, a comparison between test number 33 and test number 34 shows that when the product (X*Y) is less than 200, the fit of the white image is further improved.

[0669] For example, the comparison of test numbers 8, 12 and 16 shows that when the heating and drying method is warm air drying, the abrasion resistance of the white image is further improved compared with the heating and drying methods of IR drying and heated drum drying.

[0670] For example, a comparison between test number 205 and test number 206 shows that when the heating and drying method is warm air drying, the abrasion resistance of the white image is further improved when the product (X*Z) is 2.0 or higher.

[0671] For example, a comparison between test number 214 and test number 215 shows that when the heating and drying method is warm air drying, the in-plane non-uniformity of the white image is further suppressed when the product (X*Z) is less than 10.0.

[0672] For example, a comparison between test number 209 and test number 210 shows that when the heating and drying method is warm air drying, the abrasion resistance of the white image is further improved when the product (X*Z) is 3.5 or higher.

[0673] For example, a comparison between test number 215 and test number 216 shows that when the heating and drying method is warm air drying, the in-plane non-uniformity of the white image is further suppressed when the product (X*Z) is below 7.5.

[0674] For example, a comparison between test number 11 and test number 12 shows that when the value of A / B, obtained by dividing the dry film thickness of the white ink by the wet film thickness, is below 0.20, the adhesion of the white image is further improved.

[0675] For example, a comparison between test number 29 and test number 30 shows that when the dry film thickness of the white ink is greater than 1.30 μm, the concealment of the white image is further improved.

[0676] For example, a comparison between test number 28 and test number 32 shows that when the dry film thickness of the white ink is less than 1.80 μm, the adhesion of the white image is further improved.

[0677] For example, a comparison between test number 305 and test number 306 shows that when the contact pressure between the conveyor roller T1 and the white ink is 4000 N / m... 2 In the following cases, the concealment of white images is further enhanced.

[0678] Additionally, although the evaluation was omitted, the contact pressure between the conveyor roller T1 and the white ink was 750 N / m. 2 At the above time, the conveying performance based on conveyor roller T1 is further improved.

[0679] In the above embodiments, instead of using coloring inks (i.e., cyan ink, black ink, magenta ink, and yellow ink) as the first ink, a pretreatment liquid and white ink as the second ink were used to record a white image.

[0680] In these embodiments, when a colored pattern image (characters, graphics, etc.) is recorded using at least one of a coloring ink (i.e., cyan ink, black ink, magenta ink, and yellow ink) as the first ink, and then a white image (solid image) is recorded as a background image using white ink as the second ink to cover the colored pattern image, a white image with excellent concealment and adhesion can be obtained, similar to the embodiments described above. In this case, when the first ink is set to white ink and the second ink is set to a coloring ink, a white image with excellent concealment and adhesion can also be obtained, similar to the embodiments described above.

[0681] Furthermore, in the above embodiments, even without applying the pretreatment liquid, a white image with excellent concealment and adhesion can be obtained in the same way as in the above embodiments.

[0682] The disclosure of Japanese Patent Application No. 2022-150263, filed on September 21, 2022, is incorporated herein by reference in its entirety.

[0683] All documents, patent applications and technical standards described in this specification are incorporated herein by reference to the same extent as the specific documents, patent applications and technical standards which are incorporated herein by reference.

Claims

1. An image recording method, comprising: The recording process involves applying white ink containing water, white pigment, and resin to one surface of a non-porous substrate using an inkjet printer, and then heating and drying the applied white ink to record a white image. When the white ink is concentrated to a mass reduction of 30% by removing a portion of the solvent, and the viscosity of the concentrated ink obtained at 32°C is set as X mPa·s, and the heating rate from the start of the heating and drying process to 5 seconds is set as Y°C / s, the product of X and Y is 30 to 280. The solvent is water and, in the presence of water, a water-soluble organic solvent. The water solubility of the water-soluble organic solvent refers to its property of dissolving more than 1g of water at 25°C per 100g of water. The non-permeable nature of the non-permeable substrate refers to the property that the water absorption rate is less than 2.5% after 24 hours as determined by ASTM D570-98 (2018), with "%" as the unit of the water absorption rate as the quality standard.

2. The image recording method according to claim 1, wherein, The product of X and Y is 40 to 200.

3. The image recording method according to claim 1, wherein, The heating and drying are carried out by blowing warm air. When the value obtained by dividing the wind speed of the warm air in m / s by the temperature of the warm air in °C is set as Z, the product of X and Z is 2.0 to 10.

0.

4. The image recording method according to claim 3, wherein, The product of X and Z is 3.5 to 7.

5.

5. The image recording method according to claim 1, wherein, The value obtained by dividing the thickness of the white ink applied to one side of the non-permeable substrate after heat drying by the thickness of the white ink applied to one side of the non-permeable substrate before heat drying is 0.10 to 0.

20.

6. The image recording method according to claim 5, wherein, The thickness of the white ink applied to one side of the non-permeable substrate after heat drying is 1.30 μm to 1.80 μm.

7. The image recording method according to claim 1, wherein, The recording process further includes a step of conveying the non-permeable substrate coated with the white ink via a conveying member in a configuration where the conveying member is in contact with the white ink. Following the recording step, a winding step is also included to wind up the non-permeable substrate on which the white image is recorded. The average contact pressure between the conveying component and the white ink from the application of the white ink to the winding of the non-permeable substrate is 750 N / m. 2 ~4000N / m 2 .

8. The image recording method according to claim 1, wherein, The recording process also includes the step of applying a coloring ink containing water, coloring pigments and resin to one surface of the non-permeable substrate by inkjet printing to record a colored image, wherein "coloring" in the coloring ink and the coloring pigments refers to color or black.

9. The image recording method according to claim 8, wherein, The colored image is recorded before the white image and is positioned between the non-permeable substrate and the white image.

10. The image recording method according to claim 1, wherein, Prior to the recording step, the process further includes applying a pretreatment solution containing water and a coagulant to one surface of the non-permeable substrate. In the recording process, the white ink is applied to the area on one surface that has been treated with the pretreatment liquid to record the white image.

11. An image recording apparatus for use in the image recording method according to any one of claims 1 to 10, the image recording apparatus comprising: An inkjet head for applying the white ink to one surface of the non-permeable substrate; and A heating and drying apparatus for heating and drying the applied white ink. The product of X and Y is 30 to 280.

Citation Information

Patent Citations

  • Exhaust gas recirculation controller

    JP1979030316A

  • Recording method and device therefor

    JP1979059936A

  • Color image forming method

    JP1984157636A

  • Photopolymerization composition, photopolymerizable color composition and color filter

    JP2002012607A

  • Actinic energy ray-curable ink-jet ink

    JP2002188025A