A method for manufacturing an antistatic carpet
Conductive fibers were prepared by crosslinking modified polyacrylonitrile with 1-hydroxypyrrole-doped polypyrrole, which solved the problem of static electricity accumulation in acrylic carpets and achieved high washability and excellent antistatic effect, while maintaining the carpet's appearance and flexibility.
Patent Information
- Application Number
- CN202411967737.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-30
AI Technical Summary
Existing acrylic carpets have problems with the generation and accumulation of static electricity, leading to electric shock, fire risk, dust adsorption, and interference with electronic devices. Furthermore, existing antistatic methods affect the appearance of the carpet or have poor washability.
Conductive fibers were prepared using a crosslinking agent of modified polyacrylonitrile and 1-hydroxypyrrole-doped polypyrrole. The 1-hydroxypyrrole-doped polypyrrole was then attached to the side chain of the modified polyacrylonitrile via esterification, and an antistatic carpet was prepared using a wet spinning process.
It meets antistatic standards even after 50 washes, has good flexibility, high color fastness to rubbing, and the conductive fibers do not affect the carpet's appearance. It also has excellent washability and antistatic properties.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of carpets, and specifically relates to a method for preparing an antistatic carpet. Background Technology
[0002] Static electricity is a ubiquitous physical phenomenon with wide-ranging applications, but it can also bring certain negative impacts. In the carpet industry, the presence of static electricity in carpets can lead to several negative consequences, including: 1. Walking on carpets may cause an electric shock sensation, resulting in discomfort and fright; 2. Static discharge may lead to fires and explosions; 3. Static electricity can attract dust and bacteria from the air, and these harmful substances are more likely to accumulate on the carpet surface under the influence of static electricity, affecting human health; 4. Static electricity in carpets may also interfere with the normal operation of electronic devices.
[0003] Acrylic carpets have advantages such as moderate price, good warmth retention, softness and comfort, and easy cleaning, and have broad application prospects in commercial and residential fields. However, acrylic carpets have relatively poor electrical conductivity and weak ability to bind electrons. When acrylic carpets rub against other objects (such as shoe soles, furniture, etc.), electrons are easily transferred between fibers, leading to the accumulation of charge and the generation of static electricity.
[0004] The copolymerization method for preparing antistatic acrylic fibers involves adding comonomers (ethylene monomers containing hydrophilic groups such as hydroxyl, ether, carboxyl, and amide groups) during the monomer polymerization process to increase the hygroscopicity of the acrylic fibers, thereby achieving an antistatic effect. Acrylic fibers prepared by this method have a comfortable feel, good flexibility, and are washable, but their antistatic effect is poor in dry environments.
[0005] The conductive method refers to the co-spinning of acrylic fibers with conductive fibers. The resulting acrylic carpet can conduct away the generated charge, thereby achieving an antistatic effect. This method is not affected by environmental humidity. However, conductive fibers are mostly dark-colored, which is not easy to dye and has poor color fastness, which has a significant impact on the appearance of the product. Conductive fibers also have poor flexibility and are easy to break, so they are not resistant to washing.
[0006] Patent CN117646289B discloses a stain-resistant and antibacterial textile fabric and its preparation method. In this technical solution, polyacrylonitrile fiber is formed by wet spinning of a uniformly mixed functionalized acrylonitrile copolymer, functionalized polypyrrole nanoparticles, 1,3-malondialdehyde, trifluoroacetic acid and dimethyl sulfoxide. Polypyrrole is a conductive polymer material that can form conductive pathways inside the stain-resistant and antibacterial textile fabric, giving it good antistatic properties. However, polypyrrole is a black solid, which has a significant impact on the appearance of the fabric. Polypyrrole has relatively poor flexibility, resulting in a poor hand feel. At the same time, during washing and friction, polypyrrole may break, affecting the antistatic properties. Summary of the Invention
[0007] To address the problems existing in the prior art, this invention provides a method for preparing an antistatic carpet, achieving the following objectives: good antistatic effect, washability, still meeting antistatic standards after 50 washes, good flexibility, high elongation at break, conductive fibers do not affect the appearance and color of the carpet, and high color fastness to rubbing.
[0008] To solve the above technical problems, the technical solution adopted by the present invention is as follows: A method for preparing an antistatic carpet includes the following steps: 1. Preparation of modified polyacrylonitrile Polyacrylonitrile was added to NaOH solution and stirred in a water bath at 60–80°C for 1.5–2.5 h. After cooling to room temperature, the mixture was filtered, and the filter cake was washed with ethanol and deionized water until neutral. Then, it was dried in a drying oven at 50–70°C for 10–14 h to obtain modified polyacrylonitrile. The degree of polymerization of the polyacrylonitrile is 1900–2100; The mass fraction of the NaOH solution is 10-20%; The stirring rate is 70–90 r / min.
[0009] 2. Preparation of 1-hydroxypyrrole-doped polypyrrole Pyrrole was added to anhydrous CaCl2, shaken vigorously for 8–12 min, and then allowed to stand for 5–7 h. Zinc powder and zeolite were then added, and the mixture was distilled under reduced pressure. The fraction at 125–130 °C was collected to obtain pretreated pyrrole. Pretreated pyrrole and 1-hydroxypyrrole were added to deionized water and mixed evenly. Then FeCl3 solution was slowly added dropwise. The mixture was stirred and reacted in an ice-water bath for 22-26 hours. After filtration, the filter cake was washed with deionized water and ethanol alternately 2-4 times. Then it was dried in a drying oven at 55-65℃ for 9-11 hours to obtain 1-hydroxypyrrole-doped polypyrrole. The mass ratio of pyrrole, anhydrous CaCl2, zinc powder, and zeolite is 12–14:1–3:0.6–0.7:0.4–0.6. The mass ratio of the pretreated pyrrole, 1-hydroxypyrrole, deionized water, and FeCl3 solution is 1.5–2.5: 0.08–0.12: 280–320: 0.21–0.26. The FeCl3 solution was added dropwise over a period of 25–35 minutes. The stirring rate is 40–60 r / min; The FeCl3 solution has a mass fraction of 4.4% to 4.9%.
[0010] 3. Preparation of crosslinking agent Cyclohexane hexyl alcohol and gluconic acid were added to deionized water, and then zinc acetate catalyst was added. The mixture was heated to 110-150°C, and the steam was collected. The steam was then introduced into a saturated Na2CO3 solution. After cooling and separation, the upper layer was collected to obtain the esterification product of cyclohexane hexyl alcohol and gluconic acid, i.e., the crosslinking agent. The mass ratio of cyclohexanehexol, gluconic acid, deionized water, and zinc acetate is 14–16:97–99:140–160:2–4.
[0011] 4. Preparation of conductive fibers Modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, and crosslinking agent were added to dimethylamide and crosslinked at 170–190°C for 30–50 min. Then, vacuum defoaming was carried out at 45–55°C to prepare a spinning solution. Conductive fibers were obtained by wet spinning process. The mass ratio of the modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, crosslinking agent, and dimethylamide is 17–19:0.8–1.2:0.06–0.08:95–105.
[0012] 5. Preparation of modified polyacrylonitrile fibers Modified polyacrylonitrile was added to dimethylamide, and vacuum defoaming was carried out at 45-55℃ to prepare a spinning solution. Modified polyacrylonitrile fibers were obtained by wet spinning process. The mass ratio of the modified polyacrylonitrile to dimethylamide is 0.8–1.2:4.5–5.5.
[0013] 6. Spinning yarn and making blankets Conductive fibers and modified polyacrylonitrile fibers are spun into yarn, and the yarn is fed into a carpet loom to obtain an antistatic carpet.
[0014] The yarn comprises 6 to 8 modified polyacrylonitrile fibers and 1 to 3 conductive fibers in each yarn. The antistatic carpet has a warp density of 160-200 threads / cm, a weft density of 350-450 threads / cm, and a pile height of 12-16mm.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. In the process of preparing conductive fibers, the hydroxyl groups in 1-hydroxypyrrole-doped polypyrrole are attached to the side chains of modified polyacrylonitrile through esterification reaction. Therefore, 1-hydroxypyrrole-doped polypyrrole has little effect on the flexibility of the main chain, and the final antistatic carpet has an elongation at break of 57-60%.
[0016] 2. In the process of preparing conductive fibers, the modified polyacrylonitrile in this invention tightly encapsulates the modified polyacrylonitrile containing 1-hydroxypyrrole-doped polypyrrole in a ring-like structure. Therefore, the 1-hydroxypyrrole-doped polypyrrole has no effect on the color and appearance of the antistatic carpet of this invention. The rubbing fastness reaches level 5, and the antistatic effect is good. In the carpet electrostatic performance evaluation simulation human walking test method, the voltage value before washing is 2.15~2.27kV, and the voltage value after 50 washings is 2.66~2.75kV, both of which are lower than 3kV, which meets the antistatic requirements of carpets in general places. Detailed Implementation
[0017] Example 1 1. Preparation of modified polyacrylonitrile Polyacrylonitrile was added to NaOH solution and stirred in a water bath at 70°C for 2 hours. After cooling to room temperature, the mixture was filtered, and the filter cake was washed with ethanol and deionized water until neutral. Then, it was dried in a drying oven at 60°C for 12 hours to obtain modified polyacrylonitrile. The degree of polymerization of the polyacrylonitrile is 2000; The NaOH solution has a mass fraction of 15%. The stirring rate is 80 r / min.
[0018] 2. Preparation of 1-hydroxypyrrole-doped polypyrrole Pyrrole was added to anhydrous CaCl2, shaken vigorously for 10 minutes, and then allowed to stand for 6 hours. Zinc powder and zeolite were then added, and the mixture was distilled under reduced pressure. The fraction at 128°C was collected to obtain pretreated pyrrole. Pretreated pyrrole and 1-hydroxypyrrole were added to deionized water and mixed evenly. Then FeCl3 solution was slowly added dropwise. After stirring and reacting for 24 hours in an ice-water bath, the mixture was filtered. The filter cake was washed three times with deionized water and ethanol alternately. Then it was dried in a drying oven at 60°C for 10 hours to obtain 1-hydroxypyrrole-doped polypyrrole. The mass ratio of pyrrole, anhydrous CaCl2, zinc powder, and zeolite is 13:2:0.7:0.5. The mass ratio of the pretreated pyrrole, 1-hydroxypyrrole, deionized water, and FeCl3 solution is 2:0.1:300:0.24. The FeCl3 solution was added dropwise over a period of 30 minutes. The stirring rate is 50 r / min; The FeCl3 solution has a mass fraction of 4.7%.
[0019] 3. Preparation of crosslinking agent Cyclohexane hexaol and gluconic acid were added to deionized water, and then zinc acetate catalyst was added. The mixture was heated to 130°C, and the steam was collected. The steam was then introduced into a saturated Na2CO3 solution. After cooling and separation, the upper layer was collected to obtain the esterification product of cyclohexane hexaol and gluconic acid, i.e., the crosslinking agent. The mass ratio of cyclohexanehexol, gluconic acid, deionized water, and zinc acetate is 15:98:150:3.
[0020] 4. Preparation of conductive fibers Modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, and crosslinking agent were added to dimethylamide and crosslinked at 180°C for 40 min. Then, vacuum defoaming was performed at 50°C to prepare a spinning solution. Conductive fibers were obtained by wet spinning process. The mass ratio of the modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, crosslinking agent, and dimethylamide is 18:1:0.07:100.
[0021] 5. Preparation of modified polyacrylonitrile fibers Modified polyacrylonitrile was added to dimethylamide, and vacuum defoaming was performed at 50°C to prepare a spinning solution. Modified polyacrylonitrile fibers were obtained by wet spinning process. The mass ratio of the modified polyacrylonitrile to dimethylamide is 1:5.
[0022] 6. Spinning yarn and making blankets Conductive fibers and modified polyacrylonitrile fibers are spun into yarn, and the yarn is fed into a carpet loom to obtain an antistatic carpet.
[0023] The yarn comprises 7 modified polyacrylonitrile fibers and 2 conductive fibers in each yarn. The antistatic carpet has a warp density of 180 threads / cm, a weft density of 400 threads / cm, and a pile height of 14mm.
[0024] Example 2 1. Preparation of modified polyacrylonitrile Polyacrylonitrile was added to NaOH solution and stirred in a water bath at 60°C for 1.5 h. After cooling to room temperature, the mixture was filtered, and the filter cake was washed with ethanol and deionized water until neutral. Then, it was dried in a drying oven at 50°C for 10 h to obtain modified polyacrylonitrile. The degree of polymerization of the polyacrylonitrile is 1900; The NaOH solution has a mass fraction of 10%. The stirring rate is 70 r / min.
[0025] 2. Preparation of 1-hydroxypyrrole-doped polypyrrole Pyrrole was added to anhydrous CaCl2, shaken vigorously for 8 minutes, and then allowed to stand for 5 hours. Zinc powder and zeolite were then added, and the mixture was distilled under reduced pressure. The fraction at 125°C was collected to obtain pretreated pyrrole. Pretreated pyrrole and 1-hydroxypyrrole were added to deionized water and mixed evenly. Then FeCl3 solution was slowly added dropwise. After stirring and reacting for 22 hours in an ice-water bath, the mixture was filtered. The filter cake was washed twice with deionized water and ethanol alternately. Then it was dried in a drying oven at 55°C for 9 hours to obtain 1-hydroxypyrrole-doped polypyrrole. The mass ratio of pyrrole, anhydrous CaCl2, zinc powder, and zeolite is 12:1:0.6:0.4. The mass ratio of the pretreated pyrrole, 1-hydroxypyrrole, deionized water, and FeCl3 solution is 1.5:0.08:280:0.21. The FeCl3 solution was added dropwise over a period of 25 minutes. The stirring rate is 40 r / min; The FeCl3 solution has a mass fraction of 4.4%.
[0026] 3. Preparation of crosslinking agent Cyclohexane hexyl alcohol and gluconic acid were added to deionized water, and then zinc acetate catalyst was added. The mixture was heated to 110°C, and the steam was collected. The steam was then introduced into a saturated Na2CO3 solution. After cooling and separation, the upper layer was collected to obtain the esterification product of cyclohexane hexyl alcohol and gluconic acid, i.e., the crosslinking agent. The mass ratio of cyclohexanehexol, gluconic acid, deionized water, and zinc acetate is 14:97:140:2.
[0027] 4. Preparation of conductive fibers Modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, and crosslinking agent were added to dimethylamide and crosslinked at 170°C for 30 min. Then, vacuum defoaming was performed at 45°C to prepare a spinning solution. Conductive fibers were obtained by wet spinning process. The mass ratio of the modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, crosslinking agent, and dimethylamide is 17:0.8:0.06:95.
[0028] 5. Preparation of modified polyacrylonitrile fibers Modified polyacrylonitrile was added to dimethylamide, and vacuum defoaming was performed at 45°C to prepare a spinning solution. Modified polyacrylonitrile fibers were then obtained using a wet spinning process. The mass ratio of the modified polyacrylonitrile to dimethylamide is 0.8:4.5.
[0029] 6. Spinning yarn and making blankets Conductive fibers and modified polyacrylonitrile fibers are spun into yarn, and the yarn is fed into a carpet loom to obtain an antistatic carpet.
[0030] The yarn comprises 6 modified polyacrylonitrile fibers and 1 conductive fiber in each yarn. The antistatic carpet has a warp density of 160 threads / cm, a weft density of 350 threads / cm, and a pile height of 12mm.
[0031] Example 3 1. Preparation of modified polyacrylonitrile Polyacrylonitrile was added to NaOH solution and stirred in a water bath at 80°C for 2.5 h. After cooling to room temperature, the mixture was filtered, and the filter cake was washed with ethanol and deionized water until neutral. Then, it was dried in a drying oven at 70°C for 14 h to obtain modified polyacrylonitrile. The degree of polymerization of the polyacrylonitrile is 2100; The NaOH solution has a mass fraction of 20%. The stirring rate is 90 r / min.
[0032] 2. Preparation of 1-hydroxypyrrole-doped polypyrrole Pyrrole was added to anhydrous CaCl2, shaken vigorously for 12 minutes, and then allowed to stand for 7 hours. Zinc powder and zeolite were then added, and the mixture was distilled under reduced pressure. The fraction at 130°C was collected to obtain pretreated pyrrole. Pretreated pyrrole and 1-hydroxypyrrole were added to deionized water and mixed evenly. Then FeCl3 solution was slowly added dropwise. After stirring and reacting for 26 hours in an ice-water bath, the mixture was filtered. The filter cake was washed with deionized water and ethanol four times alternately. Then it was dried in a drying oven at 65°C for 11 hours to obtain 1-hydroxypyrrole-doped polypyrrole. The mass ratio of pyrrole, anhydrous CaCl2, zinc powder, and zeolite is 14:3:0.7:0.6. The mass ratio of the pretreated pyrrole, 1-hydroxypyrrole, deionized water, and FeCl3 solution is 2.5:0.12:320:0.26. The FeCl3 solution was added dropwise over a period of 35 minutes. The stirring rate is 60 r / min; The FeCl3 solution has a mass fraction of 4.9%.
[0033] 3. Preparation of crosslinking agent Cyclohexane hexaol and gluconic acid were added to deionized water, and then zinc acetate catalyst was added. The mixture was heated to 150°C, and the steam was collected. The steam was then introduced into a saturated Na2CO3 solution. After cooling and separation, the upper layer was collected to obtain the esterification product of cyclohexane hexaol and gluconic acid, i.e., the crosslinking agent. The mass ratio of cyclohexanehexol, gluconic acid, deionized water, and zinc acetate is 16:99:160:4.
[0034] 4. Preparation of conductive fibers Modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, and crosslinking agent were added to dimethylamide and crosslinked at 190°C for 50 min. Then, vacuum defoaming was performed at 55°C to prepare a spinning solution. Conductive fibers were obtained by wet spinning process. The mass ratio of the modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, crosslinking agent, and dimethylamide is 19:1.2:0.08:105.
[0035] 5. Preparation of modified polyacrylonitrile fibers Modified polyacrylonitrile was added to dimethylamide, and vacuum defoaming was performed at 55°C to prepare a spinning solution. Modified polyacrylonitrile fibers were then obtained using a wet spinning process. The mass ratio of the modified polyacrylonitrile to dimethylamide is 1.2:5.5.
[0036] 6. Spinning yarn and making blankets Conductive fibers and modified polyacrylonitrile fibers are spun into yarn, and the yarn is fed into a carpet loom to obtain an antistatic carpet.
[0037] The yarn comprises 8 modified polyacrylonitrile fibers and 3 conductive fibers in each yarn. The antistatic carpet has a warp density of 200 threads / cm, a weft density of 450 threads / cm, and a pile height of 16mm.
[0038] Comparative Example 1 Based on Example 1, step 4, which prepares 1-hydroxypyrrole-doped polypyrrole, is replaced with the preparation of polypyrrole, omitting the addition of 1-hydroxypyrrole. In step 6, 1-hydroxypyrrole-doped polypyrrole is replaced with polypyrrole, and the remaining steps are the same.
[0039] Comparative Example 2 Based on Example 1, step 5, the preparation of the crosslinking agent, and step 6, the addition of the crosslinking agent are omitted, while the remaining steps are the same.
[0040] Experimental Example 1 The antistatic carpets prepared in Examples 1-3 and Comparative Examples 1-2 were washed 50 times each using GB / T17596-1998. Then, the maximum voltage value of the antistatic carpets within 30 seconds before and after washing was tested using GB / T18044-2000. The test results are shown in Table 1.
[0041] Table 1
[0042] Experimental Example 2 The color fastness to rubbing of the antistatic carpets prepared in Examples 1-3 and Comparative Examples 1-2 was tested according to GB / T14252-2008, and the elongation at break of the antistatic carpets was tested according to GB / T 3923.1-1997. The test results are shown in Table 2.
[0043] Table 2
[0044] The results above show that: The antistatic carpet of the present invention comprises conductive fibers prepared by coating 1-hydroxypyrrole-doped polypyrrole with modified polyacrylonitrile using a crosslinking agent. The side chains of the modified polyacrylonitrile contain multiple carboxyl groups, and the hydroxyl groups in the 1-hydroxypyrrole-doped polypyrrole are attached to the side chains of the modified polyacrylonitrile through an esterification reaction. Therefore, the 1-hydroxypyrrole-doped polypyrrole has little effect on the flexibility of the main chain, and the resulting antistatic carpet has an elongation at break of 57-60%. Compared to Comparative Example 1, because Comparative Example 1 used polypyrrole instead of 1-hydroxypyrrole to dop the polypyrrole, the polypyrrole and polyacrylonitrile main chain were mixed and spun in the conductive fiber. The polypyrrole had poor flexibility, which ultimately led to the breakage of polypyrrole in the conductive fiber during the washing process of the antistatic carpet. After 50 washes, the voltage value was higher than 3kV, the antistatic effect was poor, and the elongation at break was low. The crosslinking agent prepared in this invention has a cyclic polyhydroxy structure. During the preparation of conductive fibers, the modified polyacrylonitrile is in excess. Under the action of the crosslinking agent, the modified polyacrylonitrile tightly encapsulates the modified polyacrylonitrile containing 1-hydroxypyrrole-doped polypyrrole in a cyclic manner. Therefore, the 1-hydroxypyrrole-doped polypyrrole has no effect on the appearance of the antistatic carpet of this invention. The rubbing fastness reaches level 5, and the antistatic effect is good. In the carpet electrostatic performance evaluation simulation human walking test method, the voltage value before washing is 2.15-2.27kV, and the voltage value after 50 washings is 2.66-2.75kV, both of which are lower than 3kV, which meets the antistatic requirements of carpets in general places. Compared to Comparative Example 2, since no crosslinking agent was added during the preparation of the conductive fibers in Comparative Example 2, the polyacrylonitrile had a poor encapsulation effect on 1-hydroxypyrrole-doped polypyrrole. As a result, during the washing or rubbing process, the 1-hydroxypyrrole-doped polypyrrole in the conductive fibers of the antistatic carpet was exposed and broke. After 50 washes, the voltage value was higher than 3kV, indicating poor antistatic effect and low color fastness to rubbing.
Claims
1. A method for preparing an antistatic carpet, characterized in that: The preparation method includes preparing modified polyacrylonitrile, preparing 1-hydroxypyrrole-doped polypyrrole, preparing a crosslinking agent, preparing conductive fibers, preparing modified polyacrylonitrile fibers, spinning and making blankets; The method for preparing 1-hydroxypyrrole-doped polypyrrole is as follows: pyrrole is added to anhydrous CaCl2, shaken for 8-12 min, and allowed to stand for 5-7 h. Then, zinc powder and zeolite are added, and the mixture is distilled under reduced pressure. The fraction at 125-130℃ is collected to obtain pretreated pyrrole. The pretreated pyrrole and 1-hydroxypyrrole are added to deionized water, and then FeCl3 solution is slowly added dropwise. The mixture is stirred and reacted under an ice-water bath for 22-26 h. After filtration, the filter cake is washed with deionized water and ethanol alternately 2-4 times and dried to obtain 1-hydroxypyrrole-doped polypyrrole. The method for preparing the crosslinking agent is as follows: cyclohexanehexol and gluconic acid are added to deionized water, then zinc acetate catalyst is added, the mixture is heated to 110-150°C, the steam is collected, the steam is introduced into a saturated Na2CO3 solution, and after cooling and separation, the upper layer is collected to obtain the esterification product of cyclohexanehexol and gluconic acid, i.e., the crosslinking agent. The method for preparing conductive fibers is as follows: modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, and crosslinking agent are added to dimethylamide, crosslinked at 170-190°C for 30-50 min, and then vacuum defoamed at 45-55°C to prepare a spinning solution. Conductive fibers are then obtained by wet spinning process. The method for preparing modified polyacrylonitrile is as follows: polyacrylonitrile is added to a NaOH solution with a mass fraction of 10-20%, and the mixture is stirred and reacted in a water bath at 60-80°C for 1.5-2.5 hours. After cooling, filtration, washing with ethanol and deionized water, and drying, modified polyacrylonitrile is obtained. The method of spinning and making carpet involves spinning conductive fibers and modified polyacrylonitrile fibers into yarn, and then feeding the yarn into a carpet loom to obtain an antistatic carpet.
2. The method for preparing an antistatic carpet according to claim 1, characterized in that: In the method for preparing 1-hydroxypyrrole-doped polypyrrole, the mass ratio of pyrrole, anhydrous CaCl2, zinc powder, and zeolite is 12–14:1–3:0.6–0.7:0.4–0.6; the mass ratio of pretreated pyrrole, 1-hydroxypyrrole, deionized water, and FeCl3 solution is 1.5–2.5:0.08–0.12:280–320:0.21–0.26; the time for adding FeCl3 solution is 25–35 min; the stirring rate is 40–60 r / min; and the mass fraction of FeCl3 solution is 4.4–4.9%.
3. The method for preparing an antistatic carpet according to claim 1, characterized in that: In the method for preparing the crosslinking agent, the mass ratio of cyclohexanehexyl alcohol, gluconic acid, deionized water, and zinc acetate is 14-16:97-99:140-160:2-4.
4. The method for preparing an antistatic carpet according to claim 1, characterized in that: In the method for preparing conductive fibers, the mass ratio of modified polyacrylonitrile, 1-hydroxypyrrole-doped polypyrrole, crosslinking agent, and dimethylamide is 17-19:0.8-1.2:0.06-0.08:95-105.
5. The method for preparing an antistatic carpet according to claim 1, characterized in that: The method for preparing modified polyacrylonitrile fibers is as follows: modified polyacrylonitrile in a mass ratio of 0.8-1.2:4.5-5.5 is added to dimethylamide, and vacuum defoaming is performed at 45-55°C to prepare a spinning solution. Modified polyacrylonitrile fibers are then obtained by wet spinning process.
6. The method for preparing an antistatic carpet according to claim 1, characterized in that: In the method of spinning and making a carpet, each yarn contains 6 to 8 modified polyacrylonitrile fibers and 1 to 3 conductive fibers; the antistatic carpet has a warp density of 160 to 200 threads / cm, a weft density of 350 to 450 threads / cm, and a pile height of 12 to 16 mm.
Citation Information
Patent Citations
Cellulose fabrics / olypyrrole electrostatic resistance compound material and method of producing the same
CN101182680A
Polyacrylonitrile-based modified material as well as preparation method and application thereof
CN118930750A