A nickel-cobalt-lithium aluminate positive electrode material, a preparation method and application thereof

By employing a stepwise solid-phase mixing and multi-step calcination method, the problem of uneven aluminum ion distribution in lithium nickel cobalt aluminum oxide cathode materials was solved, and NCA materials with high specific capacity and good cycle performance were prepared, making them suitable for lithium-ion batteries.

CN119905498BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311415485.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-27
Publication Date
2026-11-20
Estimated Expiration
2043-10-27

AI Technical Summary

Technical Problem

In existing methods for preparing lithium nickel cobalt aluminum oxide (NCA) cathode materials, the uneven distribution of aluminum ions leads to a loose material structure and poor electrochemical performance. Furthermore, it is prone to generating LiAlO₂ impurity phases, which affects product performance.

Method used

A stepwise solid-phase mixing and multi-step calcination method is adopted. First, nickel hydroxide is mixed with an aluminum source, then with a cobalt source, and finally with a lithium source. Specific heat treatment conditions are used to ensure uniform element distribution and avoid the formation of LiAlO₂ impurity phases.

Benefits of technology

Uniform mixing of lithium nickel cobalt aluminum oxide cathode material was achieved, which improved specific capacity and cycle performance, and ensured the stability of the layered structure and electrochemical performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119905498B_ABST
    Figure CN119905498B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a kind of nickel-cobalt lithium aluminate positive materials and its preparation method and application, the method includes the following steps: S1, nickel hydroxide is mixed with aluminum source first solid phase, obtains first solid material;S2, cobalt source is mixed with the first solid material second solid phase, the mixture material obtained is carried out first heat treatment under the first oxygen-containing atmosphere, obtains second solid material;S3, lithium source is mixed with the second solid material third solid phase, the mixture material obtained is carried out second heat treatment under the second oxygen-containing atmosphere.The method step of the present disclosure is simple, adopts the method of step-by-step solid phase mixing combined with multi-step calcination, by controlling specific feeding sequence and the sequence of solid phase mixing and heat treatment, not only can realize the batch production of any component nickel-cobalt lithium aluminate positive material, but also can promote the uniform mixing of nickel-cobalt aluminum three elements, to obtain specific capacity high, cycle performance good nickel-cobalt lithium aluminate positive material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of ternary material preparation for lithium-ion batteries, specifically to a lithium nickel cobalt aluminum oxide cathode material, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries have been widely used in transportation, communication, energy storage, and other fields. The cathode material is the decisive factor in its electrochemical performance and is a key component of lithium-ion batteries. High-nickel ternary materials have become a hot research topic due to their advantages such as high specific capacity, low overall cost, and stable low-temperature performance. Among them, lithium nickel cobalt aluminum oxide (NCA) is a representative material that has been widely used in the field of new energy vehicles; however, its preparation process still faces certain challenges.

[0003] Currently, there are two main mature methods for preparing NCA. One method involves preparing a nickel-cobalt-aluminum precursor using a co-precipitation method, followed by high-temperature calcination with an appropriate amount of lithium source (e.g., patent CN101262061A). However, due to the significant difference between the precipitation equilibrium constant of aluminum hydroxide and that of nickel hydroxide and cobalt hydroxide, and the fact that aluminum hydroxide dissolves under alkaline conditions, it is difficult for aluminum ions to form a uniform co-precipitate with nickel-cobalt ions. This results in uneven aluminum ion distribution and poor sphericity and a loose structure, thus affecting the electrochemical performance of the cathode material. The other method involves first preparing a nickel-cobalt hydroxide precursor, then mixing it with an aluminum compound to form a coating structure, followed by lithiation and calcination (e.g., patent CN1156910A). However, the subsequently introduced Al₂O₃ or Al(OH)₃ readily forms a LiAlO₂ impurity phase with lithium salt, leading to uneven distribution of elements in the NCA and ultimately affecting product performance. Summary of the Invention

[0004] The purpose of this disclosure is to provide a lithium nickel cobalt aluminum oxide cathode material, its preparation method, and its application.

[0005] To achieve the above objectives, the first aspect of this disclosure provides a method for preparing lithium nickel cobalt aluminum oxide cathode materials, the method comprising the following steps:

[0006] S1. Nickel hydroxide and aluminum source are mixed in a first solid phase to obtain a first solid material;

[0007] S2. Mix the cobalt source with the first solid material in a second solid phase, and subject the resulting mixture to a first heat treatment under a first oxygen-containing atmosphere to obtain the second solid material.

[0008] S3. The lithium source and the second solid material are mixed in a third solid phase, and the resulting mixture is subjected to a second heat treatment in a second oxygen-containing atmosphere.

[0009] Optionally, the aluminum source includes one or more of aluminum hydroxide, aluminum oxide, aluminum carbonate, aluminum oxalate, and aluminum acetate;

[0010] The cobalt source includes one or more of cobalt hydroxide, cobalt oxide, cobalt carbonate, cobalt oxalate, and cobalt acetate;

[0011] The lithium source includes one or more of lithium hydroxide, lithium carbonate, and lithium nitrate.

[0012] Optionally, the first solid-phase mixing, the second solid-phase mixing, and the third solid-phase mixing can be carried out by solid-phase ball milling for 1-5 hours.

[0013] Optionally, in step S2, the first heat treatment method includes calcination, and the conditions of the first heat treatment include: a time of 2-8 hours and a temperature of 400-900℃.

[0014] Optionally, in step S3, the second heat treatment method includes calcination, and the conditions of the second heat treatment include: a time of 10-20 hours and a temperature of 600-850°C.

[0015] Optionally, the first oxygen-containing atmosphere and the second oxygen-containing atmosphere are either an oxygen atmosphere or an air atmosphere, respectively.

[0016] Optionally, the nickel hydroxide has an average particle size of 5-15 μm.

[0017] The second aspect of this disclosure provides a lithium nickel cobalt aluminum oxide cathode material prepared using the method described in the first aspect of this disclosure.

[0018] Optionally, the lithium nickel cobalt aluminum oxide cathode material includes materials with the chemical formula LiNi. 1-x-y Co x Al y For O2 particles, 0.6 ≤ 1 - xy < 1, 0 <x≤0.2,0<y≤0.2。

[0019] This disclosure provides a third aspect of a lithium-ion battery, the lithium-ion battery comprising a positive electrode, an electrolyte and a negative electrode, wherein the positive electrode comprises the lithium nickel cobalt aluminum oxide positive electrode material described in the second aspect of this disclosure.

[0020] Through the above technical solution, this disclosure adopts a step-by-step solid-phase mixing combined with multi-step calcination method. By controlling the specific feeding sequence and the sequence of solid-phase mixing and heat treatment, it can not only realize the mass production of lithium nickel cobalt aluminum oxide cathode materials of arbitrary composition, but also promote the uniform mixing of the three elements of nickel, cobalt and aluminum, thereby obtaining lithium nickel cobalt aluminum oxide cathode materials with high specific capacity and good cycle performance.

[0021] Other features and advantages of this disclosure will be described in detail in the following detailed description section. Attached Figure Description

[0022] The accompanying drawings are provided to further illustrate the present disclosure and form part of the specification. They are used together with the following detailed description to explain the present disclosure, but do not constitute a limitation thereof. In the drawings:

[0023] Figure 1 Electrochemical cycling curve of lithium nickel cobalt aluminum oxide cathode material A3 prepared in Example 3 of this disclosure.

[0024] Figure 2 A scanning electron microscope image of lithium nickel cobalt aluminum oxide cathode material A1 prepared in Example 1 of this disclosure.

[0025] Figure 3 This is a scanning electron microscope image of lithium nickel cobalt aluminum oxide cathode material D1 prepared according to Comparative Example 1 of this disclosure.

[0026] Figure 4 The image shows a scanning electron microscope (SEM) image and elemental distribution map of the second solid material in Embodiment 2 of this disclosure.

[0027] Figure 5 Scanning electron microscope (SEM) image and elemental distribution map of lithium nickel cobalt aluminum oxide cathode material A2 prepared for Example 2 of this disclosure.

[0028] Figure 6 Electrochemical cycling curves of lithium nickel cobalt aluminum oxide cathode materials A1 and D1 prepared in Example 1 and Comparative Example 1 of this disclosure.

[0029] Figure 7 Electrochemical cycling curves of lithium nickel cobalt aluminum oxide cathode materials D3-D6 prepared in Comparative Examples 3-6 of this disclosure. Detailed Implementation

[0030] The specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit this disclosure.

[0031] The first aspect of this disclosure provides a method for preparing lithium nickel cobalt aluminum oxide cathode material, the method comprising the following steps:

[0032] S1. Nickel hydroxide and aluminum source are mixed in a first solid phase to obtain a first solid material;

[0033] S2. Mix the cobalt source with the first solid material in a second solid phase, and subject the resulting mixture to a first heat treatment under a first oxygen-containing atmosphere to obtain the second solid material.

[0034] S3. The lithium source and the second solid material are mixed in a third solid phase, and the resulting mixture is subjected to a second heat treatment in a second oxygen-containing atmosphere.

[0035] This disclosure employs a stepwise mixing and heat treatment method. First, nickel hydroxide is sequentially mixed with an aluminum source and a cobalt source in a solid-state manner. After a first heat treatment, nickel cobalt aluminum oxide is obtained. Then, the nickel cobalt aluminum oxide is mixed with a lithium source in a solid-state manner and subjected to a second heat treatment to obtain lithium nickel cobalt aluminum oxide cathode material. The above method is simple, and the migration of cobalt atoms can drive the migration of aluminum atoms, achieving uniform mixing of elements in the material, avoiding the formation of LiAlO2 impurity phase, improving the stability of the layered structure, and producing cathode material with good sphericity and Li / Ni mixing degree. When used as cathode material for lithium-ion batteries, it has high specific capacity and good cycle performance.

[0036] In this disclosure, in order to achieve uniform mixing, the first solid phase mixing, the second solid phase mixing, and the third solid phase mixing in steps S1, S2, and S3 include solid phase ball milling for 1-5 hours, preferably 2-4 hours; solid phase ball milling can be performed, for example, on a planetary ball mill.

[0037] According to one embodiment of this disclosure, the types of aluminum source, cobalt source, and lithium source are all conventional in the art. For example, the aluminum source includes one or more of aluminum hydroxide, aluminum oxide, aluminum carbonate, aluminum oxalate, and aluminum acetate. When the aluminum source includes two or more, there is no specific limitation on their proportion. The cobalt source includes one or more of cobalt hydroxide, cobalt oxide, cobalt carbonate, cobalt oxalate, and cobalt acetate. When the cobalt source includes two or more, there is no specific limitation on their proportion. The lithium source includes one or more of lithium hydroxide, lithium carbonate, and lithium nitrate. When the lithium source includes two or more, there is no specific limitation on their proportion.

[0038] According to one embodiment of this disclosure, the first oxygen-containing atmosphere and the second oxygen-containing atmosphere are respectively an oxygen atmosphere or an air atmosphere, wherein the definitions of oxygen atmosphere and air atmosphere are conventional in the art.

[0039] According to one embodiment of this disclosure, in step S1, the first heat treatment includes calcination, which can be carried out in a sagger; the conditions of the first heat treatment include: a time of 2-8 hours and a temperature of 400-900°C; preferably, a time of 3-7 hours and a temperature of 500-800°C; at this temperature, metal atoms can migrate effectively, thereby promoting the uniform dispersion of each element.

[0040] According to one embodiment of this disclosure, in step S2, the second heat treatment includes calcination, which can be carried out in a sagger; the conditions of the second heat treatment include: a time of 10-20 hours and a temperature of 600-850°C; preferably, a time of 12-18 hours and a temperature of 700-800°C; the cathode material obtained under these conditions can exhibit good capacity and maintain good stability.

[0041] According to one embodiment of this disclosure, nickel hydroxide has a spherical and / or near-spherical morphology, where spherical and near-spherical are conventional definitions in the art. Preferably, the average particle size of nickel hydroxide is 5-15 μm; this particle size can better exert the performance of the material and meet the market demand for particle size.

[0042] In this disclosure, in steps S1 and S2, the amounts of nickel hydroxide, aluminum source, and cobalt source are adjusted according to the ratio of Ni, Co, and Al in the lithium nickel cobalt aluminum oxide cathode material.

[0043] According to one embodiment of this disclosure, in step S3, the molar ratio of the lithium source (calculated as lithium element) to the second solid material (calculated as the total amount of nickel, cobalt, and aluminum elements) can be, for example, (0.8-1.2):1. The lithium source may be partially lost during solid-phase mixing and heat treatment.

[0044] The second aspect of this disclosure provides a lithium nickel cobalt aluminum oxide cathode material prepared using the method described in the first aspect of this disclosure.

[0045] According to one embodiment of this disclosure, in order to have a high capacity, the lithium nickel cobalt aluminum oxide cathode material comprises LiNi 1-x-y Co x Al y For O2 particles, 0.6 ≤ 1 - xy < 1, 0 <x≤0.2,0<y≤0.2。

[0046] This disclosure provides a lithium-ion battery in a third aspect, the lithium-ion battery comprising a positive electrode, an electrolyte and a negative electrode, wherein the positive electrode comprises the lithium nickel cobalt aluminum oxide positive electrode material described in the second aspect of this disclosure.

[0047] According to one embodiment of this disclosure, the negative electrode is conventional in the art and may include one or more of lithium sheets, carbon materials, and silicon-carbon composite materials.

[0048] According to one embodiment of this disclosure, the electrolyte is conventional in the art, and may include one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, lithium hexafluorophosphate, and dimethyl carbonate.

[0049] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way.

[0050] All raw materials used in the examples were obtained through commercial purchases and, unless otherwise specified, were of analytical grade.

[0051] The scanning electron microscope energy dispersive spectroscopy test instrument was a FEIQUANTA400, and the method was an accelerating voltage of 20 kV.

[0052] The X-ray diffraction pattern was tested using an X-ray powder diffractometer manufactured by Philips, USA. The method used a Cu target anode Kα radiation source with a step width of 0.02°, a scanning speed of 2° / min, and 2θ = 10°-80°.

[0053] Testing method for the chemical formula of cathode materials: inductively coupled plasma mass spectrometry.

[0054] Example 1

[0055] The lithium nickel cobalt aluminum oxide cathode material A1 was prepared using the following steps:

[0056] (1) Spherical nickel hydroxide (average particle size of 8.2 μm) and aluminum hydroxide powder were weighed according to the molar ratio of n(Ni):n(Al)=0.8:0.05, and mixed in a planetary ball mill for 2 hours to obtain the first solid material;

[0057] (2) Weigh out cobalt acetate according to the molar ratio of n(Ni):n(Co)=0.8:0.15 and add it to the first solid material. After mixing in a planetary ball mill for 2 hours, load the resulting mixture into a sagger and perform the first heat treatment under an oxygen atmosphere by calcination at a temperature of 500℃ for 5 hours to obtain the second solid material.

[0058] (3) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.05:1, LiOH·H2O and the second solid material were weighed separately and mixed in a planetary ball mill for 2 hours. The resulting mixture was then placed in a sagger and subjected to a second heat treatment under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material Al, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0059] Example 2

[0060] The lithium nickel cobalt aluminum oxide cathode material A2 was prepared using the following steps:

[0061] (1) Spherical nickel hydroxide (average particle size of 8.2 μm) and aluminum hydroxide powder were weighed according to the molar ratio of n(Ni):n(Al)=0.8:0.05, and mixed in a planetary ball mill for 2 hours to obtain the first solid material;

[0062] (2) Weigh out cobalt acetate according to the molar ratio of n(Ni):n(Co)=0.8:0.15 and add it to the first solid material. After mixing in a planetary ball mill for 2 hours, load the resulting mixture into a sagger and perform the first heat treatment under an oxygen atmosphere by calcination at a temperature of 600℃ for 6 hours to obtain the second solid material.

[0063] (3) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.06:1, LiOH·H2O and the second solid material were weighed separately and mixed in a planetary ball mill for 3 hours. The resulting mixture was then placed in a sagger and subjected to a second heat treatment under an oxygen atmosphere by calcination at 760℃ for 18 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material A2, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0064] Example 3

[0065] The lithium nickel cobalt aluminum oxide cathode material A3 was prepared using the following steps:

[0066] (1) Spherical nickel hydroxide (average particle size of 7.7 μm) and alumina powder were weighed according to the molar ratio of n(Ni):n(Al)=0.7:0.1, and mixed in a planetary ball mill for 2 hours to obtain the first solid material;

[0067] (2) Weigh out cobalt carbonate according to the molar ratio of n(Ni):n(Co)=0.7:0.2 and add it to the first solid material. After mixing in a planetary ball mill for 2 hours, load the resulting mixture into a sagger and perform the first heat treatment under an oxygen atmosphere by calcination at a temperature of 700℃ for 5 hours to obtain the second solid material.

[0068] (3) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.06:1, LiOH·H2O and the second solid material were weighed separately and mixed in a planetary ball mill for 3 hours. The resulting mixture was then placed in a sagger and subjected to a second heat treatment under an oxygen atmosphere by calcination at 760℃ for 18 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material A3, with the chemical formula LiNi. 0.7 Co 0.2 Al 0.1O2.

[0069] Example 4

[0070] The lithium nickel cobalt aluminum oxide cathode material A4 was prepared using the following steps:

[0071] (1) Spherical nickel hydroxide (average particle size of 8.2 μm) and aluminum hydroxide powder were weighed according to the molar ratio of n(Ni):n(Al)=0.8:0.1, and mixed in a planetary ball mill for 2 hours to obtain the first solid material;

[0072] (2) Weigh out cobalt acetate according to the molar ratio of n(Ni):n(Co)=0.8:0.1 and add it to the first solid material. After mixing in a planetary ball mill for 2 hours, load the resulting mixture into a sagger and perform the first heat treatment under an oxygen atmosphere by calcination at a temperature of 800℃ for 6 hours to obtain the second solid material.

[0073] (3) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.08:1, LiOH·H2O and the second solid material were weighed separately and mixed in a planetary ball mill for 3 hours. The resulting mixture was then placed in a sagger and subjected to a second heat treatment under an oxygen atmosphere by calcination at 760℃ for 18 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material A4, with the chemical formula LiNi. 0.8 Co 0.1 Al 0.1 O2.

[0074] Example 5

[0075] Lithium nickel cobalt aluminum oxide cathode material A5 was prepared using the method described in Example 1, except that aluminum hydroxide in step (1) was replaced with aluminum oxide containing an equimolar amount of Al, cobalt acetate in step (2) was replaced with cobalt oxalate containing an equimolar amount of Co, and LiOH·H2O in step (3) was replaced with lithium carbonate containing an equimolar amount of Li. The chemical formula of lithium nickel cobalt aluminum oxide cathode material A5 is LiNi 0.8 Co 0.15 Al 0.05 O2.

[0076] Comparative Example 1

[0077] The lithium nickel cobalt aluminum oxide cathode material D1 was prepared using the following steps:

[0078] (1) Spherical nickel hydroxide (average particle size of 8.2 μm) was placed in a crucible and subjected to the first heat treatment under an oxygen atmosphere by calcination at a temperature of 500 °C for 5 h to obtain the first solid material.

[0079] (2) Weigh the first solid material and aluminum hydroxide powder according to the molar ratio of n(Ni):n(Al)=0.8:0.05, mix them in a planetary ball mill for 2 hours to obtain the second solid material;

[0080] (3) Weigh out cobalt acetate according to the molar ratio of n(Ni):n(Co)=0.8:0.15 and add it to the second solid material. After mixing in a planetary ball mill for 2 hours, the third solid material is obtained.

[0081] (4) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.05:1, LiOH·H2O and the third solid material were weighed separately and mixed in a planetary ball mill for 2 hours. The resulting mixture was then placed in a sagger and subjected to a second heat treatment under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material D1 with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0082] Comparative Example 2

[0083] The lithium nickel cobalt aluminum oxide cathode material D2 was prepared using the following steps:

[0084] (1) Spherical nickel hydroxide (average particle size of 8.2 μm) and cobalt acetate were weighed according to the molar ratio of n(Ni):n(Co)=0.8:0.15, and mixed in a planetary ball mill for 2 hours to obtain the first solid material;

[0085] (2) Weigh aluminum hydroxide powder according to the molar ratio of n(Ni):n(Al)=0.8:0.05 and add it to the first solid material. After mixing in a planetary ball mill for 2 hours, load the resulting mixture into a sagger and perform the first heat treatment under an oxygen atmosphere by calcination at a temperature of 500℃ for 5 hours to obtain the second solid material.

[0086] (3) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.05:1, LiOH·H2O and the second solid material were weighed separately and mixed in a planetary ball mill for 2 hours. The resulting mixture was then placed in a sagger and subjected to a second heat treatment under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material D2, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0087] Comparative Example 3

[0088] The lithium nickel cobalt aluminum oxide cathode material D3 was prepared using the following steps:

[0089] (1) Spherical nickel hydroxide (average particle size of 8.2 μm) and cobalt acetate were weighed according to the molar ratio of n(Ni):n(Co)=0.8:0.15, and mixed in a planetary ball mill for 2 hours to obtain the first solid material;

[0090] (2) Weigh aluminum hydroxide according to the molar ratio of n(Ni):n(Al)=0.8:0.05 and add it to the first solid material. After mixing in a planetary ball mill for 2 hours, the second solid material is obtained.

[0091] (3) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.05:1, LiOH·H2O and the second solid material were weighed separately and mixed in a planetary ball mill for 2 hours. The resulting mixture was then placed in a sagger and heat-treated under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material D3, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0092] Comparative Example 4

[0093] The lithium nickel cobalt aluminum oxide cathode material D4 was prepared using the following steps:

[0094] (1) Spherical nickel hydroxide (average particle size of 8.2 μm) and aluminum hydroxide powder were weighed according to the molar ratio of n(Ni):n(Al)=0.8:0.05, and mixed in a planetary ball mill for 2 hours to obtain the first solid material;

[0095] (2) Weigh out cobalt acetate according to the molar ratio of n(Ni):n(Co)=0.8:0.15 and add it to the first solid material. After mixing in a planetary ball mill for 2 hours, the second solid material is obtained.

[0096] (3) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.05:1, LiOH·H2O and the second solid material were weighed separately and mixed in a planetary ball mill for 2 hours. The resulting mixture was then placed in a sagger and heat-treated under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material D4, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0097] Comparative Example 5

[0098] The lithium nickel cobalt aluminum oxide cathode material D5 was prepared using the following steps:

[0099] (1) According to the molar ratio of n(Ni):n(Co):n(Al)=0.8:0.15:0.05, spherical nickel hydroxide (average particle size of 8.2μm), cobalt acetate and aluminum hydroxide powder were weighed and mixed in a planetary ball mill for 4h to obtain the first solid material;

[0100] (2) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.05:1, LiOH·H2O and the first solid material were weighed separately and mixed in a planetary ball mill for 2 hours. The resulting mixture was then placed in a sagger and heat-treated under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material D5, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0101] Comparative Example 6

[0102] The lithium nickel cobalt aluminum oxide cathode material D6 was prepared using the following steps:

[0103] Spherical nickel hydroxide (average particle size 8.2 μm), cobalt acetate, and aluminum hydroxide powders were weighed according to a molar ratio of n(Ni):n(Co):n(Al) = 0.8:0.15:0.05. LiOH·H₂O was then added to these powders at a molar ratio of n(Li):n(Ni+Co+Al) = 1.05:1 and mixed in a planetary ball mill for 6 hours. The resulting mixture was then placed in a crucible and heat-treated under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material D6, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0104] Comparative Example 7

[0105] The lithium nickel cobalt aluminum oxide cathode material D7 was prepared using the following steps:

[0106] (1) According to the molar ratio of n(Ni):n(Co):n(Al)=0.8:0.15:0.05, spherical nickel hydroxide (average particle size of 8.2μm), cobalt acetate and aluminum hydroxide powder were weighed respectively. After mixing in a planetary ball mill for 4h, the resulting mixture was loaded into a sagger and subjected to the first heat treatment under an oxygen atmosphere by calcination at a temperature of 500℃ for 5h to obtain the first solid material.

[0107] (2) According to the molar ratio of n(Li):n(Ni+Co+Al)=1.05:1, LiOH·H2O and the first solid material were weighed separately and mixed in a planetary ball mill for 2 hours. The resulting mixture was then placed in a sagger and subjected to a second heat treatment under an oxygen atmosphere by calcination at 750℃ for 15 hours. The resulting solid product was then crushed and sieved to obtain lithium nickel cobalt aluminum oxide cathode material D7, with the chemical formula LiNi. 0.8 Co 0.15 Al 0.05 O2.

[0108] The lithium nickel cobalt aluminum oxide cathode material A1 prepared in Example 1 and the lithium nickel cobalt aluminum oxide cathode material D1 prepared in Comparative Example 1 were subjected to scanning electron microscopy (SEM) tests, and the results are as follows: Figure 2 and 3 As shown.

[0109] according to Figure 2 and 3 The results show that the lithium nickel cobalt aluminum oxide cathode material A1 has a better spherical morphology. The only difference between Comparative Example 1 and Example 1 is that the order of the aluminum source mixing step and the heat treatment step are different. As can be seen from the above, it is beneficial to maintain the integrity and spherical morphology of the particles by first performing the aluminum source and cobalt source mixing step and then performing the heat treatment step.

[0110] The second solid material obtained in step (2) of Example 2 was subjected to scanning electron microscopy and elemental distribution imaging. The results are as follows: Figure 4 As shown.

[0111] according to Figure 4 The results show that the nickel, aluminum and cobalt elements in the second solid material are evenly distributed, which is beneficial to the uniform dispersion of elements in the subsequent lithiation heat treatment process.

[0112] The lithium nickel cobalt aluminum oxide cathode material A2 prepared in Example 2 was subjected to scanning electron microscopy and elemental distribution imaging. The results are as follows: Figure 5 As shown.

[0113] according to Figure 5 The results show that the nickel, aluminum and cobalt elements in the lithium nickel cobalt aluminum oxide cathode material prepared by the method of this disclosure are uniformly distributed.

[0114] X-ray diffraction analysis was performed on lithium nickel cobalt aluminum oxide cathode materials A1 and D1-D7. 003 / I 104 The results of the values ​​are shown in Table 1 below.

[0115] Table 1

[0116] Examples / Comparative Examples Sample number <![CDATA[I 003 / I 104 The value]]> Example 1 A1 1.231 Comparative Example 1 D1 1.112 Comparative Example 2 D2 1.154 Comparative Example 3 D3 1.125 Comparative Example 4 D4 1.197 Comparative Example 5 D5 1.093 Comparative Example 6 D6 1.013 Comparative Example 7 D7 1.105

[0117] The intensity ratio of the (003) and (104) crystal planes in the X-ray diffraction pattern is I 003 / I 104 The value of I can be used to describe the Li / Ni mixing degree. 003 / I 104 The larger the value, the smaller the Li / Ni mixing degree. According to the data in Table 1 above, under the same conditions, the ternary material prepared by the method of this disclosure has a low Li / Ni mixing degree. It can be further seen that the mixing order of the materials and the number of heat treatments affect the layered structure stability of the final ternary material, and thus affect the cycle stability of the material.

[0118] Specifically, the difference between Example 1, Comparative Example 2, and Comparative Example 7 lies in the different mixing order of the aluminum source and the cobalt source. According to the data in Table 1, the mixing order of this disclosure can promote the uniform dispersion of elements, thereby improving the stability of the layered structure. The difference between Example 1, Comparative Example 1, and Comparative Example 4 lies in the different number and order of heat treatments. According to the data in Table 1, the number and order of heat treatments of this disclosure can prepare lithium nickel cobalt aluminum oxide cathode material with a stable layered structure.

[0119] Test case

[0120] Electrochemical stability tests were conducted on the lithium nickel cobalt aluminum oxide cathode materials A1, A3, D1, and D3-D6 prepared in the examples and comparative examples. The specific steps are as follows:

[0121] Weigh out the positive electrode material, conductive agent (acetylene black), and binder (polyvinylidene fluoride) according to a mass ratio of 8:1:1, add solvent (N-methylpyrrolidone) and mix evenly. Coat the mixture onto aluminum foil and cut it into sheets to serve as the positive electrode. Then, mix it separately with lithium foil and electrolyte (1 mol·L⁻¹). -1 A lithium-ion half-cell was constructed using LiPF6 (ethylene carbonate / ethyl methyl carbonate / dimethyl carbonate in a mass ratio of 1:1:1) and a separator (Celgard 2300). Electrochemical performance tests were conducted, and the results are as follows: Figure 1 , 6 As shown in Figures 7 and 8.

[0122] Performance testing conditions: charge / discharge voltage range of 2.75-4.3V; charge / discharge rate of 0.1C for the first 4 times, and 0.5C for the 5th time and beyond; test temperature of 25℃.

[0123] The electrochemical cycling curve of a lithium-ion half-cell prepared using lithium nickel cobalt aluminum oxide cathode material A3 prepared in Example 3 is shown below. Figure 1 As shown; according to Figure 1 It can be seen that material A3 exhibits high specific capacity and cycle stability.

[0124] The electrochemical cycling curves of lithium-ion half-cells prepared using lithium nickel cobalt aluminum oxide cathode materials A1 and D1 prepared in Example 1 and Comparative Example 1 are shown below. Figure 6 As shown; according to Figure 6 It can be seen that, compared with D1, A1 exhibits significantly superior discharge specific capacity and cycle retention, further indicating that the method of mixing before heat treatment is beneficial to improving the electrochemical performance of lithium nickel cobalt aluminum oxide cathode materials.

[0125] The electrochemical cycling curves of lithium-ion half-cells prepared using lithium nickel cobalt aluminum oxide cathode materials D3-D6 prepared in Comparative Examples 3-6 are shown below. Figure 7 As shown.

[0126] according to Figure 7 and Figure 1 and 6 The comparison shows that the lithium-ion battery prepared using the lithium nickel cobalt aluminum oxide cathode material prepared by the method of this disclosure has higher specific capacity and better cycle stability.

[0127] The preferred embodiments of this disclosure have been described in detail above with reference to the accompanying drawings. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and these simple modifications all fall within the protection scope of this disclosure.

[0128] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.

[0129] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.

Claims

1. A method for preparing lithium nickel cobalt aluminum oxide cathode material, characterized in that, The method includes the following steps: S1. Nickel hydroxide and aluminum source are mixed in a first solid phase to obtain a first solid material; S2. Mix the cobalt source with the first solid material in a second solid phase, and subject the resulting mixture to a first heat treatment under a first oxygen-containing atmosphere to obtain the second solid material. S3. The lithium source and the second solid material are mixed in a third solid phase, and the resulting mixture is subjected to a second heat treatment in a second oxygen-containing atmosphere. The methods of the first solid-phase mixing, the second solid-phase mixing, and the third solid-phase mixing include solid-phase ball milling.

2. The method according to claim 1, wherein, The aluminum source includes one or more of aluminum hydroxide, aluminum oxide, aluminum carbonate, aluminum oxalate, and aluminum acetate; The cobalt source includes one or more of cobalt hydroxide, cobalt oxide, cobalt carbonate, cobalt oxalate, and cobalt acetate; The lithium source includes one or more of lithium hydroxide, lithium carbonate, and lithium nitrate.

3. The method according to claim 1, wherein, The mixing times for the first solid phase, the second solid phase, and the third solid phase are 1-5 hours, respectively.

4. The method according to claim 1, wherein, In step S2, the first heat treatment method includes calcination, and the conditions of the first heat treatment include: a time of 2-8 hours and a temperature of 400-900℃.

5. The method according to claim 1, wherein, In step S3, the second heat treatment method includes calcination, and the conditions of the second heat treatment include: a time of 10-20 hours and a temperature of 600-850°C.

6. The method according to claim 1, wherein, The first oxygen-containing atmosphere and the second oxygen-containing atmosphere are respectively an oxygen atmosphere or an air atmosphere.

7. The method according to claim 1, wherein, The average particle size of the nickel hydroxide is 5-15 μm.

8. Lithium nickel cobalt aluminum oxide cathode material prepared by any one of claims 1-7.

9. The lithium nickel cobalt aluminum oxide cathode material according to claim 8, wherein, The lithium nickel cobalt aluminum oxide cathode material includes materials with the chemical formula LiNi. 1-x-y Co x Al y For O2 particles, 0.6 ≤ 1 - xy < 1, 0 <x≤0.2,0<y≤0.2。 10. A lithium-ion battery, the lithium-ion battery comprising a positive electrode, an electrolyte, and a negative electrode, characterized in that, The positive electrode comprises the lithium nickel cobalt aluminum oxide positive electrode material as described in claim 8 or 9.

Citation Information

Patent Citations

  • Spherical aluminum-doped nickel cobalt lithium for lithium ion battery and its making method

    CN101262061A

  • High-density lithium ion battery anode material nickel-cobalt lithium aluminate and preparation method thereof

    CN103050686A