A freeze-tolerant gel electrolyte for low temperature metal fuel cells and its preparation method and application
By adding ZnSO₄ and sorbitol to the gel electrolyte, a crystalline structure and hydrogen bonds are formed, solving the problem of freezing of traditional hydrogels at low temperatures and achieving high-efficiency discharge performance of aluminum-air batteries in extreme environments.
Patent Information
- Application Number
- CN202411954021.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-27
AI Technical Summary
Traditional hydrogel electrolytes are prone to freezing at low temperatures, which limits their application in low-temperature environments, especially in extreme conditions such as polar regions, deep seas, and aerospace, where they cannot meet the demand for efficient and sustainable power supply.
ZnSO₄ and sorbitol were used as additives to the polyacrylamide gel matrix. By forming a crystalline structure and hydrogen bonding, the mechanical properties were enhanced and the formation of ice crystals was inhibited, thus preparing a freeze-resistant gel electrolyte.
The mechanical properties and ion transport rate of the gel electrolyte were significantly improved. The aluminum-air battery was able to discharge stably for 100 minutes at -20°C, with a power density of 36.52 mW cm⁻², meeting the application requirements in low-temperature environments.
Smart Images

Figure CN119921035B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal fuel cell technology, and more specifically, to a freeze-resistant gel electrolyte for low-temperature metal fuel cells, its preparation method, and its application. Background Technology
[0002] With the rapid depletion of energy resources and the aggravation of environmental problems, the search for safe and efficient energy storage technologies has become an urgent task. Aluminum-air batteries (AAB) are favored due to their high theoretical discharge voltage (2.7 V) and capacity density (2980 mAh galvanic acid). - ¹) and energy density (8100 Wh gal) - ¹) and its low cost and environmental friendliness have garnered widespread attention, especially in the field of portable power supplies. In aluminum-air batteries, the electrolyte is a core component, and its performance directly affects the battery's electrochemical characteristics. With the continuous growth in energy storage demand and the emergence of diverse application scenarios (such as polar research, deep-sea exploration, high-altitude exploration, and aerospace), the adaptability of energy storage devices to extreme weather conditions has become particularly important. However, traditional aqueous electrolytes are prone to freezing at sub-zero temperatures, which limits their adaptability in low-temperature environments and cannot meet the demand for efficient and sustainable power supply under extreme conditions.
[0003] Gel polymer electrolytes (GPEs), composed of an organic polymer framework and a liquid electrolyte, offer advantages over traditional liquid electrolytes, including reduced leakage, good mechanical properties, and superior electrochemical performance. However, the mechanical properties of traditional hydrogels as battery electrolytes still require further improvement. Furthermore, due to the relatively high freezing point of water, traditional hydrogels inevitably freeze at sub-zero temperatures, limiting ion mobility and electrolyte-electrode interface wettability, thus restricting the application of flexible devices in low-temperature environments.
[0004] In other words, existing hydrogel electrolytes still suffer from insufficient torsion and stretching capacity. Furthermore, their high freezing point and low ion mobility limit their application potential in low-temperature aluminum-air batteries. Summary of the Invention
[0005] To address the problems existing in the prior art, one of the objectives of this invention is to provide a method for preparing a freeze-resistant gel electrolyte for low-temperature metal fuel cells. This freeze-resistant gel electrolyte possesses good mechanical properties such as bendability and stretchability, and has a simple structure, requires no sealing, and is inexpensive. It can significantly improve the low-temperature discharge performance of aluminum-air batteries, which is conducive to promoting the practical application of flexible aluminum-air batteries at low temperatures.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows: A method for preparing a freeze-resistant gel electrolyte for low-temperature metal fuel cells includes the following steps: 1) Dissolve acrylamide in water to obtain solution A; 2) Add the crosslinking agent and initiator to solution A, mix well, and obtain solution B; 3) Add ZnSO4 and sorbitol to solution B in steps, mix and stir evenly under nitrogen atmosphere and room temperature to obtain solution C; 4) Pour solution C into a mold, dry and let it stand, then allow it to swell and absorb alkali to obtain the final product.
[0007] Further, in step 1), the mass concentration of acrylamide in solution A is 20-40%, preferably 30%. After dissolving the acrylamide in water, the solution is magnetically stirred at room temperature (25°C) for 1-2 hours to obtain solution A.
[0008] Further, in step 2), the crosslinking agent is at least one of N,N'-methylenebisacrylamide, N-hydroxymethylacrylamide, hydroxyethyl methacrylate, and diacetone acrylamide; the present invention preferably uses N,N'-methylenebisacrylamide, and the initiator is at least one of potassium persulfate, sodium persulfate, and ammonium persulfate.
[0009] Further, in step 3), the concentration of ZnSO4 in solution C is 0.15-0.25 M, preferably 0.2 M; and the concentration of sorbitol is 0.02-0.06 M, preferably 0.04 M.
[0010] Furthermore, in step 3), the stirring time is 2-4 hours, the rotation speed is 200-400 r / min, and the stirring method is magnetic stirring.
[0011] Further, in step 4), the drying temperature is 60°C, the standing time is 5-8 hours, preferably 6 hours; the swelling and alkali absorption specifically involves soaking in a 4-6 M alkaline solution for swelling and alkali absorption for 5-10 hours.
[0012] The alkaline solution is a KOH solution with a concentration of 5M, and the solution swells and absorbs alkali for 7 hours.
[0013] The second objective of this invention is to provide a freeze-resistant gel electrolyte for low-temperature metal fuel cells prepared by any of the above-mentioned preparation methods.
[0014] Another objective of this invention is to provide the application of the aforementioned freeze-resistant gel electrolyte in metal fuel cells.
[0015] Furthermore, the metal fuel cell is an aluminum-air battery.
[0016] Furthermore, the application specifically refers to the use of metal fuel cells in aluminum-air batteries at temperatures ranging from -10°C to -20°C.
[0017] Specifically, conductive carbon cloth coated with commercial Premetek 20% Pt / C catalyst can be used as the cathode, a high-purity aluminum plate as the anode, and the prepared gel electrolyte as the electrolyte.
[0018] Another objective of this invention is to provide a low-temperature metal fuel cell containing the aforementioned freeze-resistant gel electrolyte.
[0019] This invention provides a freeze-resistant gel polymer electrolyte that selects ZnSO4 as the additive with the best salting-out effect through Hofmeister sequence selection. The SO4²⁻ in ZnSO4… - Ions can polarize water molecules surrounding polyacrylamide, inducing polyacrylamide chains to aggregate and form crystalline structures. These ions act as effective cross-linking points in the hydrogel network, enhancing hydrogen bonding between polyacrylamide chains and significantly improving its mechanical properties. Simultaneously, sorbitol molecules contain six hydroxyl groups, enabling them to effectively bind water molecules through hydrogen bonds, disrupting the interactions between water molecules, inhibiting ice crystal formation, and reducing water activity, thus exhibiting excellent water retention. This water-retention property is due to the OH groups within the gel. - The gel electrolyte provides a near-liquid environment, thereby enhancing ion transport rates. Furthermore, sorbitol forms strong hydrogen bonds with the polyacrylamide three-dimensional framework, further strengthening the gel's mechanical properties and adsorbing onto the aluminum anode surface, effectively mitigating the anode's self-corrosion behavior. The polyacrylamide gel electrolyte with added ZnSO4 and sorbitol significantly improves the electrochemical performance of the aluminum-air battery. At -20°C, the aluminum-air battery assembled using this gel electrolyte exhibits a stable discharge plateau voltage of approximately 1.14 V and can discharge continuously for 100 minutes, meeting the application requirements of aluminum-air batteries in low-temperature environments.
[0020] Compared with the prior art, the present invention has the following advantages: (1) This invention prepares a gel electrolyte by introducing ZnSO4 and sorbitol as additives to the polyacrylamide gel matrix. The prepared gel electrolyte has a dense dendritic framework with uniformly sized micropores arranged regularly between the framework. This structure lays the foundation for the excellent mechanical properties and ion conduction of the gel electrolyte, and the prepared gel electrolyte has the best tensile strength and elongation at break. The antifreeze ability is improved with the addition of sorbitol. The assembled flexible aluminum-air battery achieves a power density of 36.52 mW / cm². -2 The aluminum-air battery assembled with this gel electrolyte at -20°C has a stable discharge platform voltage of approximately 1.14 V and can be continuously discharged for 100 min, which meets the application requirements of low-temperature aluminum-air batteries.
[0021] (2) The low-temperature gel electrolyte of this invention has a simple and easy-to-operate preparation process, uses low-cost raw materials, and meets green environmental protection standards, enabling large-scale mass production and showing good application prospects. The prepared gel electrolyte has a stable structure and excellent electrochemical performance under low-temperature conditions. With the support of this electrolyte, the aluminum-air battery has a stable operating voltage and exhibits excellent low-temperature discharge performance, making it suitable for various applications in low-temperature environments. Attached Figure Description
[0022] Figure 1 These are macroscopic morphological images of different deformations in Embodiment 1 of the present invention; Figure 2 The images shown are SEM images of the gel electrolyte obtained in Example 1 of the present invention, wherein (a) is a cross-sectional view of the gel at 1000x magnification; and (b) is a cross-sectional view of the gel at 2000x magnification. Figure 3 The figures show the tensile test results of Embodiment 1, Comparative Examples 1 and 2 of the present invention. Figure 4 The diagrams show the open-circuit voltage test results of Embodiment 1, Comparative Examples 1 and 2 of the present invention. Figure 5 These are power density test graphs of Embodiment 1, Comparative Examples 1 and 2 of the present invention; Figure 6 The constant current discharge curves of Example 1, Comparative Example 1, and Comparative Example 2 of the present invention at -10°C are shown. Figure 7 The constant current discharge curves of Example 1, Comparative Example 1, and Comparative Example 2 of the present invention at -20°C are shown. Figure 8 The X-ray diffraction patterns of Embodiment 1, Comparative Examples 1 and 2 of the present invention are shown below. Figure 9 The Fourier transform infrared spectra of Embodiment 1, Comparative Examples 1 and 2 of the present invention are shown. Detailed Implementation
[0023] Numerous specific details are set forth in the following description to provide a full understanding of the invention. However, the invention can be practiced in many other ways different from those described herein, and similar modifications can be made by those skilled in the art without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0025] Unless otherwise specified, all materials and reagents used in this invention are available from commercially available products in the field.
[0026] Example 1 A method for preparing a gel electrolyte for low-temperature metal fuel cells, comprising the following steps: Step 1: Weigh 3 g of acrylamide, slowly add the acrylamide powder to 10 ml of deionized water, and stir rapidly with a glass rod. Then place it on a magnetic stirrer and stir for 1 hour to obtain solution A. Step 2: Weigh 1.5 mg of N,N'-methylenebisacrylamide and 30 mg of potassium persulfate, and slowly add them to the prepared solution A. Stir magnetically for 1 h to form a homogeneous mixed solution B. Step 3: Weigh 0.32 g of ZnSO4 powder and slowly add it to the prepared mixed solution B. Then weigh 0.072 g of sorbitol and slowly add it. Stir magnetically for 2-4 h at room temperature (25℃) under a nitrogen atmosphere at a speed of 300 r / min to obtain solution C. Step 4: Pour the prepared solution C into a mold and place it in a constant temperature oven at 60°C for 6 hours to obtain a gel electrolyte.
[0027] Figure 1 The figures show the macroscopic morphology of Embodiment 1 of the present invention under different deformations. As can be seen from the figures, the gel electrolyte obtained in Embodiment 1 can still return to its original intact state after being folded, stretched, and twisted without cracks or damage. This indicates that the gel electrolyte is highly flexible and not easily broken, which can meet the requirements of practical flexible aluminum-air batteries and is suitable for various application scenarios.
[0028] Figure 2 The SEM image of the gel electrolyte prepared in this embodiment shows that it has a dense dendritic framework with uniformly sized micropores arranged regularly between the frameworks; this structure lays the foundation for the excellent mechanical properties and ion conduction of the gel electrolyte.
[0029] Comparative Example 1 Compared with Example 1, Comparative Example 1 provides a method without the addition of ZnSO4 and sorbitol, as follows: Step 1: Weigh 3 g of acrylamide, slowly add the acrylamide powder to 10 ml of deionized water, and stir rapidly with a glass rod. Then place it on a magnetic stirrer and stir for 1 hour to obtain solution A. Step 2: Weigh 1.5 mg of N,N'-methylenebisacrylamide and 30 mg of potassium persulfate, and slowly add them to the prepared solution A. Stir magnetically for 1 h to form a homogeneous mixed solution B. Step 3: Pour the prepared solution B into a mold and place it in a constant temperature oven at 60°C for 6 hours to obtain an additive-free gel electrolyte.
[0030] Comparative Example 2 Compared with Example 1, Comparative Example 2 provides a method for adding ZnSO4 but not sorbitol, as detailed below: Step 1: Weigh 3 g of acrylamide, slowly add the acrylamide powder to 10 ml of deionized water, and stir rapidly with a glass rod. Then place it on a magnetic stirrer and stir for 1 hour to obtain solution A. Step 2: Weigh 1.5 mg of N,N'-methylenebisacrylamide and 30 mg of potassium persulfate, and slowly add them to the prepared solution A. Stir magnetically for 1 h to form a homogeneous mixed solution B. Step 3: Weigh 0.32 g of ZnSO4 powder and slowly add it to the prepared mixed solution B. Stir magnetically for 2-4 h at room temperature (25℃) under a nitrogen atmosphere at a speed of 300 r / min to obtain solution C. Step 4: Pour the prepared solution C into a mold and place it in a constant temperature oven at 60°C for 6 hours to obtain a gel electrolyte containing ZnSO4 additive.
[0031] Performance testing: 1. Mechanical properties The gel electrolytes prepared in Example 1 and Comparative Examples 1-2 were subjected to tensile tests. The specific test method was as follows: the prepared gel was cut into dumbbell shapes with a specification of 20 mm × 5 mm, and the two ends were fixed on a texture analyzer (CTX). The tensile rate was set to 50 mm / min. -1 The maximum stress and strain of the hydrogel were tested at room temperature to evaluate the flexibility and deformation capacity of the gel electrolyte.
[0032] The results are as follows Figure 3 As shown, the gel electrolyte prepared in Example 1 of this invention possesses the best tensile strength and elongation at break. This indicates that the gel electrolyte obtained by simultaneously introducing ZnSO4 and sorbitol can significantly improve its mechanical properties.
[0033] 2. Battery application test A typical embodiment of the present invention provides a method for preparing an aluminum-air battery, as detailed below: Preparation of the aluminum-air battery cathode: Weigh 10 mg of commercial Premetek 20% Pt / C and add it to 10 ml of a mixed solution consisting of deionized water, anhydrous ethanol, and 5% Nafion solution in a volume ratio of 2:2:1. Place the solution in an ultrasonic cleaner and sonicate for 1 h. Use a pipette to evenly coat 200 μL of the solution onto a 1×1 cm plate. -2 Place the sample on a square conductive carbon cloth and heat it on a 50°C heating table for 1 hour. After drying, the sample is obtained.
[0034] Preparation of the anode for an aluminum-air battery: A 5 mm thick aluminum plate was polished using a single-disc continuously variable speed polishing machine, with sandpaper of grades 220#, 600#, and 1000# used in sequence. The polished aluminum plate was then rinsed three times each with deionized water and anhydrous ethanol, and finally dried with a hair dryer using cold air.
[0035] The gel electrolytes prepared in Example 1 and Comparative Examples 1-2 were cut into cylindrical gels with a thickness of 3 mm and a diameter of 16 mm. These were then assembled sequentially in a battery mold in the order of air cathode-gel electrolyte-aluminum anode to obtain an aluminum-air battery. The open-circuit voltage of the aluminum-air battery was tested using a CHI760E electrochemical workstation at a scan rate of 10 mV s. -1 The test duration was 120 seconds; power density testing was performed on the aluminum-air battery, with a scan rate of 10 mV / s. -1 The low-temperature discharge performance of aluminum-air batteries was tested using a Blue Electric testing system and a low-temperature constant temperature test chamber, with a test current density of 1 mA cm⁻¹. -2 .
[0036] Figure 4 The diagram shows the open-circuit voltage test results for Example 1 and Comparative Examples 1 and 2 of the present invention. The initial open-circuit voltages of the aluminum-air batteries prepared in Comparative Examples 1 and 2 were approximately 1.49 V and 1.51 V, respectively, while the open-circuit voltage of the aluminum-air battery assembled with the gel electrolyte in Example 1 increased to 1.53 V, and the overall trend of the open-circuit voltage was stable, indicating that the gel electrolyte with ZnSO4 and sorbitol additives has a higher open-circuit voltage.
[0037] Figure 5 The figures shown are power density test graphs for Example 1 and Comparative Examples 1 and 2 of the present invention. The power densities of the aluminum-air batteries prepared in Comparative Examples 1 and 2 are 17.53 mW / cm², respectively. -2 and 33.29 mW cm -2 The power of the aluminum-air battery assembled using the gel electrolyte of Example 1, which incorporates sorbitol, was further increased to 36.52 mW / cm². -2This further enhances the electrochemical performance of the assembled flexible aluminum-air battery.
[0038] Figure 6 The figure shows the constant current discharge curves of Example 1, Comparative Examples 1 and 2 of the present invention at -10°C. It can be seen from the figure that the aluminum-air battery prepared with pure PAM gel electrolyte in Comparative Example 1 has a discharge time of only 108.8 min, and the aluminum-air battery prepared with ZnSO4 additive in Comparative Example 2 has a discharge time of only 112.7 min, and neither has a stable discharge voltage plateau. However, the aluminum-air battery prepared with ZnSO4 and sorbitol additives in Example 1 has a discharge time increased to 273.0 min, and the voltage remains within the normal range.
[0039] Figure 7 The figure shows the constant current discharge curves of Example 1, Comparative Examples 1 and 2 of the present invention at -20°C. It can be seen from the figure that the aluminum-air battery prepared with pure PAM gel electrolyte in Comparative Example 1 could not discharge. The aluminum-air battery prepared with ZnSO4 added in Comparative Example 2 could discharge normally for 12.2 min, but lacked a stable discharge voltage plateau. In contrast, the aluminum-air battery prepared with ZnSO4 and sorbitol in Example 1 showed a significant increase in discharge time to 99.8 min at -20°C, and exhibited a more stable discharge voltage plateau. This indicates that the gel electrolyte with ZnSO4 and sorbitol additives effectively extended the discharge time of the aluminum-air battery at -20°C.
[0040] Figure 8 The X-ray diffraction patterns of Example 1, Comparative Examples 1 and 2 are shown. The pure PAM gel sample of Comparative Example 1 exhibits broad and diffuse amorphous diffraction peaks. Example 1 after the introduction of ZnSO4 and sorbitol still exhibits broad and diffuse amorphous diffraction peaks, without changing the crystal structure, maintaining the stability of the original PAM three-dimensional framework structure. This gel electrolyte is like a highly absorbent "sponge". After soaking, the electrolyte can penetrate into the gel, providing a fast channel for ion transport.
[0041] Figure 9 The figures shown are Fourier transform infrared spectra of Example 1 and Comparative Examples 1 and 2 of the present invention. In Example 1 and Comparative Examples 1 and 2, peak values at 3343 and 3230 cm⁻¹ can be observed. -1 -NH2 stretching vibration peak, 1659 cm⁻¹ -1 The C=O stretching peak at 1435 cm⁻¹, the CH bending peak at 1435 cm⁻¹, and the CO stretching peak at 1092 cm⁻¹ are all located at 3300 cm⁻¹ after drying. -1The submergence of the -OH stretching vibration peak in water confirms the success of the AM polymerization reaction. In Example 1, where sorbitol and potassium sulfate were introduced, the -NH2 stretching vibration peak and the C=O peak showed a slight blue shift. This is due to the hydrogen bonding interaction between sorbitol and PAM. Furthermore, no new absorption peaks were formed, demonstrating that the addition of the additives did not disrupt the overall stability of the gel structure.
[0042] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0043] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A method for preparing a freeze-resistant gel electrolyte for low-temperature metal fuel cells, characterized in that, Includes the following steps: 1) Dissolve acrylamide in water to obtain solution A, where the mass concentration of acrylamide in solution A is 20-40%; 2) Add the crosslinking agent and initiator to solution A, mix well, and obtain solution B; 3) Add ZnSO4 and sorbitol to solution B in steps, mix and stir evenly under nitrogen atmosphere and room temperature to obtain solution C; in solution C, the concentration of ZnSO4 is 0.15-0.25 M and the concentration of sorbitol is 0.02-0.06 M. 4) Pour solution C into a mold, dry and let it stand, then swell and absorb alkali to obtain the solution; specifically, the swelling and alkali absorption is performed by soaking the solution in a 4-6 M alkaline solution for 5-10 hours.
2. The method for preparing the freeze-resistant gel electrolyte for low-temperature metal fuel cells according to claim 1, characterized in that, In step 1), the mass concentration of acrylamide in solution A is 30%. After dissolving acrylamide in water, the solution is stirred at room temperature for 1-2 hours to obtain solution A.
3. The method for preparing the freeze-resistant gel electrolyte for low-temperature metal fuel cells according to claim 1, characterized in that, In step 2), the crosslinking agent is N,N'-methylenebisacrylamide, and the initiator is potassium persulfate.
4. The method for preparing the freeze-resistant gel electrolyte for low-temperature metal fuel cells according to claim 1, characterized in that, In step 3), the concentration of ZnSO4 in solution C is 0.2 M; the concentration of sorbitol is 0.04 M.
5. The method for preparing the freeze-resistant gel electrolyte for low-temperature metal fuel cells according to claim 1, characterized in that, In step 3), the stirring time is 2-4 hours and the speed is 200-400 r / min.
6. The method for preparing the freeze-resistant gel electrolyte for low-temperature metal fuel cells according to claim 1, characterized in that, In step 4), the drying temperature is 60℃ and the standing time is 5-8h.
7. The method for preparing the freeze-resistant gel electrolyte for low-temperature metal fuel cells according to claim 6, characterized in that, In step 4), the settling time is 6 hours.
8. The freeze-resistant gel electrolyte for low-temperature metal fuel cells prepared by any of the preparation methods of claims 1-7.
9. The application of the freeze-resistant gel electrolyte of claim 8 in a metal fuel cell.
10. The application according to claim 9, characterized in that, The metal fuel cell is an aluminum-air battery.
11. A low-temperature metal fuel cell, characterized in that, It contains the freeze-resistant gel electrolyte as described in claim 8.
Citation Information
Patent Citations
Gel electrolyte for zinc ion battery and preparation method thereof
CN111740172A
Alkaline gel electrolyte for aluminum air battery as well as preparation method and application of alkaline gel electrolyte
CN118299729A