Phosphogypsum-polymer composite material film and preparation method thereof

By mixing anhydrous phosphogypsum with materials such as modifiers and polymers, anhydrous phosphogypsum-polymer composite films are prepared, which solves the problem of low utilization efficiency of phosphogypsum and achieves efficient recycling and good performance of composite films.

CN119931106APending Publication Date: 2025-05-06GUIZHOU INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510069068.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-16
Publication Date
2025-05-06

AI Technical Summary

Technical Problem

In the prior art, the utilization efficiency of phosphogypsum is low, and the treatment method is cumbersome and time-consuming, making it difficult to achieve efficient utilization of phosphogypsum.

Method used

After mixing anhydrous phosphogypsum with modifiers (DOA and oleic acid), polymers, EVA, CPE and antioxidants evenly, anhydrous phosphogypsum-polymer composite film was prepared through a twin-screw extruder and a film blowing mechanism.

Benefits of technology

The efficient recycling and utilization of phosphogypsum is achieved, and the prepared composite film has good mechanical properties and transmittance, complies with national standards, and is simple in process and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119931106A_ABST
    Figure CN119931106A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ardealite utilization, in particular to an ardealite-polymer composite film and a preparation method thereof. The preparation method comprises the following steps: firstly, adding modifiers (DOA and oleic acid) into anhydrous phosphogypsum to modify the anhydrous phosphogypsum, then adding polymer powder, particles, CPE and an antioxidant in proportion, uniformly stirring, and finally, sequentially carrying out melt blending, extrusion, air cooling, granulation and film blowing on an obtained sample. The method disclosed by the invention is simple and easy to implement, a few modifiers are needed, the filling amount of the anhydrous phosphogypsum is large, all numerical values of the prepared composite material film meet national standards, the right-angle tearing strength of the composite material film is 75 KN / m or above, the mechanical property is good, the transmittance is (83.12-86.61), the haze is (44.9-77), and the film has good permeability. The obtained anhydrous phosphogypsum-polymer composite film is high in strength, can be used for manufacturing agricultural plastic mulching films and greenhouse films after being subjected to process adjustment, and has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of phosphogypsum utilization, and specifically to a phosphogypsum-polymer composite film and a preparation method thereof. Background Art

[0002] Phosphogypsum is a common industrial waste residue in the production of phosphoric acid. It is a solid waste formed by treating phosphate ore with sulfuric acid. It contains a large amount of insoluble impurities, such as quartz, apatite, insoluble P 2 O 5 , eutectic P 2 O 5 , fluoride and fluorine, aluminum, magnesium phosphorus, sulfate, and water-soluble P 2 O 5 Soluble impurities such as fluorine, phosphorus, phosphorus, and phosphorus, as well as trace amounts of radioactive elements, can cause pollution to water, air, and soil environments. The random discharge and accumulation of phosphogypsum not only occupies a large amount of land, but also pollutes the atmospheric environment, soil, and water resources in which we live. The treatment and utilization of phosphogypsum is imminent.

[0003] Most of the existing methods using phosphogypsum as a filling material use phosphogypsum to replace the original filling powder or use a polymer to wrap phosphogypsum to make a composite material masterbatch with certain special properties to achieve phosphogypsum recycling and have certain economic value. The present invention uses phosphogypsum as a filler to prepare anhydrous phosphogypsum-polymer composite film. Compared with other methods, the present invention has the advantage that the cost of the present invention is comparable to that of other methods and the economic benefits are higher.

[0004] For example, patent application CN118074026A discloses a polymer modified phosphogypsum alloy bridge and its manufacturing method. This method uses phosphogypsum as filler to make alloy bridges, solving the problem that existing plastic cable bridges are prone to corrosion and damage. However, this method has a small market demand and low utilization rate, and the amount of phosphogypsum that can be processed is small.

[0005] For example, patent application CN114536828A discloses a method for processing modified anhydrous phosphogypsum plastic pipes. This method uses phosphogypsum to replace calcium carbonate, talcum powder, kaolin, mica and other powders as fillers for plastic pipes, but the pipe market is basically saturated and has a small market share.

[0006] For example, patent application CN114316632A discloses a method for preparing a polymer-coated phosphogypsum composite masterbatch. This method requires first converting phosphogypsum into hydroxylated phosphogypsum, which is a cumbersome and time-consuming process, and the actual production cost is high, which is not conducive to the efficient use of phosphogypsum.

[0007] Therefore, finding new directions and specific methods for the utilization of phosphogypsum is the current key research object. Summary of the invention

[0008] In order to solve the above technical problems existing in the prior art, the present application provides a phosphogypsum-polymer composite film and a preparation method thereof, which are as follows:

[0009] A method for preparing a phosphogypsum-polymer composite film comprises the following steps:

[0010] S1. Weigh anhydrous phosphogypsum, DOA and oleic acid, mix well and set aside;

[0011] S2. Add polymer powder, polymer particles, CPE (chlorinated polyethylene), EVA (plasticizer) and antioxidant to the sample prepared in S1 in sequence and mix well for later use;

[0012] S3. The sample obtained in S2 was added to a twin-screw extruder for melt blending, extrusion, air cooling and pelletizing to obtain anhydrous phosphogypsum - polymer composite particles;

[0013] S4. Add the anhydrous phosphogypsum-polymer composite material particles obtained in S3 into a film blowing machine for film blowing to obtain an anhydrous phosphogypsum-polymer composite material film.

[0014] Furthermore, the mass ratio of the anhydrous phosphogypsum to DOA is 1:0.01-0.03.

[0015] Furthermore, the particle size of the anhydrous phosphogypsum in S1 is ≥800 mesh.

[0016] Furthermore, the amount of oleic acid added in S1 is 0.5% to 1% of the weight of the raw materials.

[0017] Furthermore, the polymer in S2 is one or more of PE, PP, PVC, PA, PU, ​​PC mixed in any proportion.

[0018] Furthermore, the mass ratio of anhydrous phosphogypsum to polymer powder in S2 is 1:0.5-2, and the mass ratio of anhydrous phosphogypsum to polymer particles is 1:1.5-7.

[0019] Furthermore, the amount of CPE added in S2 is 1% to 4% of the configured raw materials.

[0020] Furthermore, the amount of EVA added in S2 is 8% to 10% of the configured raw materials.

[0021] Furthermore, the amount of antioxidant added in S2 is 0.4% to 1% of the prepared raw materials.

[0022] By adopting the preparation method of the phosphogypsum-polymer composite film, a composite film can be prepared, all values ​​of which meet the national standards, the right-angle tear strength of the composite film is above 75KN / m, the mechanical properties are good, the transmittance (83.12-86.61), and the haze (44.9-77) of the film have good permeability.

[0023] Compared with the prior art, the technical effects created by this application are embodied in:

[0024] The present application provides a process for preparing a phosphogypsum-polymer composite film, which comprises uniformly mixing anhydrous phosphogypsum with a modifier (DOA and oleic acid), a polymer, EVA, CPE and an antioxidant to obtain an anhydrous phosphogypsum-polymer composite film. The present application can effectively improve the recycling efficiency of phosphogypsum and provide an additional option for agricultural films. The method of the present application is simple and easy to implement, has low cost and a high resource recycling rate. The obtained film basically meets the national standards for films and can be used in agricultural ground films and agricultural greenhouse films after process improvements. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a simplified process flow diagram of this application. DETAILED DESCRIPTION

[0026] The technical solution of the present application is further limited below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.

[0027] Example 1

[0028] ① Weigh 90g of anhydrous phosphogypsum, 2.25g of DOA and 1.8g of oleic acid and mix them evenly;

[0029] ② Add 90g PE powder, 31g EVA, 270g PE granules and 3g antioxidant to ① and mix well for later use;

[0030] ③ Add the material obtained in ② into a twin-screw extruder for melt blending, air cooling after extrusion, and then granulation for standby use;

[0031] ④ Add the particles in ③ into the film blowing machine to prepare anhydrous phosphogypsum-PP composite film. The film tensile strength is 10.9433MPa; the nominal strain at break is 438.807; the film transmittance is 86.61%; and the haze is 75.71%.

[0032] Example 2

[0033] ① Weigh 90g of anhydrous phosphogypsum, 2g of DOA and 1.5g of oleic acid and mix them evenly;

[0034] ② Add 90g PVC powder, 31.5g EVA, 270g PVC particles and 3g antioxidant to ① and mix well for later use;

[0035] ③ Add the material obtained in ② into a twin-screw extruder for melt blending, air cooling after extrusion, and then granulation for standby use;

[0036] ④ Add the particles in ③ into the film blowing machine to prepare anhydrous phosphogypsum-PVC composite film. The film tensile strength is 12.7128MPa; the nominal strain at break is 479.852; the film transmittance is 84.24%; and the haze is 76.13%.

[0037] Example 3

[0038] ① Weigh 180g of anhydrous phosphogypsum, 3g of DOA and 2g of oleic acid and mix them evenly;

[0039] ② Add 90g PP powder, 31g EVA, 210g PP granules and 3g antioxidant to ① and mix well for later use;

[0040] ③ Add the material obtained in ② into a twin-screw extruder for melt blending, air cooling after extrusion, and then granulation for standby use;

[0041] ④ Add the particles in ③ into the film blowing machine to prepare anhydrous phosphogypsum-PP composite film. The film tensile strength is 9.8312MPa; the nominal strain at break is 425.712; the film transmittance is 84.26%; and the haze is 74.17%.

[0042] Example 4

[0043] ① Weigh 100g of anhydrous phosphogypsum, 2g of DOA and 1.5g of oleic acid and mix them evenly;

[0044] ② Add 90g PE powder, 31g EVA, 250g PE granules and 3g antioxidant to ① and mix well for later use;

[0045] ③ Add the material obtained in ② into a twin-screw extruder for melt blending, air cooling after extrusion, and then granulation for standby use;

[0046] ④ Add the particles in ③ into the film blowing machine to prepare anhydrous phosphogypsum-PE composite film. The film tensile strength is 11.9132MPa; the nominal strain at break is 421.873; the film transmittance is 83.12%; and the haze is 71.71%.

[0047] Finally, it should be pointed out that the above embodiments are only representative examples of the present application. Obviously, the technical solution of the present application is not limited to the above embodiments, and there may be many variations. All variations that can be directly derived or associated with the contents disclosed in the present application by a person of ordinary skill in the art should be considered as the protection scope of the present application.

Claims

1. A method for preparing a phosphogypsum-polymer composite film, characterized in that: The steps include: S1. Weigh anhydrous phosphogypsum, DOA and oleic acid, mix well and set aside; S2. Add polymer powder, polymer particles, CPE, EVA and antioxidant to the sample prepared in S1 and stir evenly for later use; S3. The sample obtained in S2 was added to a twin-screw extruder for melt blending, extrusion, air cooling and pelletizing to obtain anhydrous phosphogypsum - polymer composite particles; S4. Add the anhydrous phosphogypsum-polymer composite material particles obtained in S3 into a film blowing machine for film blowing to obtain an anhydrous phosphogypsum-polymer composite material film.

2. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The mass ratio of the anhydrous phosphogypsum to DOA is 1:0.01-0.

03.

3. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The particle size of the anhydrous phosphogypsum in S1 is ≥800 mesh.

4. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The amount of oleic acid added in S1 is 0.5% to 1% of the weight of the raw materials.

5. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The polymer in S2 is one or more of PE, PP, PVC, PA, PU, ​​PC mixed in any proportion.

6. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The mass ratio of anhydrous phosphogypsum to polymer powder in S2 is 1:0.5-2, and the mass ratio of anhydrous phosphogypsum to polymer particles is 1:1.5-7.

7. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The amount of CPE added in S2 is 1% to 4% of the raw materials.

8. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The amount of EVA added in S2 is 8% to 10% of the raw materials.

9. The method for preparing the phosphogypsum-polymer composite film according to claim 1, characterized in that: The amount of antioxidant added in S2 is 0.4% to 1% of the raw materials.

10. A phosphogypsum-polymer composite film, characterized in that: It is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of polymer-coated ardealite composite master batch

    CN114316632A

  • Processing method of modified anhydrous phosphogypsum plastic pipeline

    CN114536828A