A method and system for removing pollutants and preserving calcium in waste incineration fly ash by flotation

By combining natural carbonation reaction and flotation, heavy metals are selectively captured while retaining Ca-based components, solving the problem of calcium recovery and utilization in fly ash from waste incineration and achieving harmless treatment and resource utilization of fly ash.

CN119951666BActive Publication Date: 2026-11-24QINGDAO UNIV OF TECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510298313.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-13
Publication Date
2026-11-24
Estimated Expiration
2045-03-13

AI Technical Summary

Technical Problem

Existing methods for treating fly ash from waste incineration are insufficient for the efficient recovery of calcium, leading to resource waste. Furthermore, traditional flotation methods are ineffective in separating heavy metals and chloride salts when treating fly ash from waste incineration.

Method used

The process employs a combination of natural carbonation reaction and flotation. Heavy metals are selectively captured by a collector and attached to bubbles to form a foam product. After solid-liquid separation, the Ca-based components remain at the bottom of the flotation cell, forming tailings.

Benefits of technology

It achieves efficient removal of heavy metals and chloride salts while retaining the Ca-based components in fly ash, thereby improving the resource utilization rate of fly ash, reducing the leaching concentration of heavy metals and the chloride content, and meeting the requirements for use in building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119951666B_ABST
    Figure CN119951666B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of solid waste treatment, and relates to a flotation method and system for removing pollutants and preserving calcium in waste incineration fly ash. The waste incineration fly ash is subjected to natural carbonation reaction in a natural environment until the pH value is 7-9, and pretreated fly ash is obtained. The pretreated fly ash is mixed with water, and a collector and a foaming agent are added for flotation separation. Alternatively, the waste fly ash is mixed with an aqueous sulfuric acid solution, and a collector and a foaming agent are added for flotation separation. The collector is one or more of butyl xanthate, butyl ammonium black medicine and ethylthiourea. The present application can not only remove heavy metals and chloride salts in the fly ash, but also preserve Ca-based components in the fly ash, thereby maximizing the resource utilization of waste incineration fly ash.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid waste treatment technology, and specifically to a flotation method and system for decontaminating and preserving calcium in fly ash from waste incineration. Background Technology

[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0003] Fly ash from waste incineration is a fine particulate matter produced during the incineration process. It contains large amounts of heavy metals and chlorides, and is classified as hazardous waste. Currently, the main methods for treating fly ash from waste incineration include cement solidification, melt solidification, and chemical stabilization. However, these methods suffer from high processing costs, low resource utilization rates, and a tendency to cause secondary pollution.

[0004] In recent years, flotation, as a highly efficient physical separation technology, has received widespread attention and application in the treatment of waste incineration fly ash. This technology effectively separates heavy metals and chloride salts from fly ash by utilizing differences in surface chemical properties, achieving not only volume reduction of fly ash but also providing a new avenue for its resource utilization. However, traditional flotation methods still face significant challenges in treating waste incineration fly ash, the most prominent being the recovery and utilization of calcium. Waste incineration fly ash typically contains large amounts of calcium in the form of calcium oxide and calcium hydroxide, which have significant application value in cement manufacturing, building material production, and other fields. However, existing fly ash treatment processes often struggle to achieve efficient calcium recovery, leading to the waste of this valuable resource, which has become one of the key bottlenecks restricting the resource utilization of fly ash. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the purpose of this invention is to provide a flotation method and system for decontamination and calcium retention of waste incineration fly ash. This invention can not only remove heavy metals and chloride salts from fly ash, but also retain the calcium-based components in fly ash, thereby maximizing the resource utilization of waste incineration fly ash.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows:

[0007] In the first aspect, a flotation method for decontamination and calcium retention of waste incineration fly ash involves placing the waste incineration fly ash in a natural environment for natural carbonation reaction until the pH value reaches 7-9, obtaining pretreated fly ash. The pretreated fly ash is then mixed with water, and a collector and a frother are added for flotation separation. The collector is one or more of butyl xanthate, butylammonium black powder, and ethyl thiocyanate.

[0008] In this invention, during the natural carbonation reaction, Ca-based components such as CaO and Ca(OH)2 in fly ash react with CO2 in the air to form CaCO3. Simultaneously, some heavy metal ions in the fly ash also react with CO2 to form carbonate precipitates, thus achieving initial stabilization of heavy metals. During flotation, by selecting the appropriate collector, heavy metals (such as Pb, Zn, Cd, etc.) can be specifically captured and attached to bubbles, rising to the surface to form a foam product. After solid-liquid separation, this becomes scum. Meanwhile, Ca-based components in the fly ash (such as CaCO3) remain at the bottom of the flotation cell, forming tailings. This invention achieves the removal of heavy metals and chloride salts from fly ash, while retaining Ca-based components, through the synergistic effect of the natural carbonation reaction and the collector during flotation.

[0009] Secondly, a flotation system for decontamination and calcium retention of waste incineration fly ash, used to implement the flotation method described in the first aspect of the present invention, includes:

[0010] The pretreatment unit is configured to allow the fly ash from waste incineration to undergo a natural carbonation reaction in the natural environment.

[0011] A flotation device, configured to separate materials from a pretreatment unit by flotation;

[0012] Collector storage tank, configured for adding collector into the flotation unit;

[0013] A conditioning agent storage tank is configured for adding conditioning agents into the flotation unit;

[0014] A frother storage tank is configured for adding frother to the flotation unit.

[0015] Thirdly, a flotation method for decontaminating and preserving calcium from waste incineration fly ash involves mixing the waste fly ash with a sulfuric acid aqueous solution, then adding a collector and a frother for flotation separation; wherein the collector is one or more of butyl xanthate, butylammonium black powder, and ethyl thiocyanate.

[0016] This invention selects an aqueous sulfuric acid solution as the flotation solvent, that is, sulfuric acid is added to water to control the pH during the flotation process, so that some of the sparingly soluble and insoluble chloride salts in the fly ash are removed, while slightly soluble calcium sulfate is generated, thus retaining the Ca-based components. During the flotation process, by selecting a collector, heavy metals (such as Pb, Zn, Cd, etc.) can be specifically captured and attached to bubbles, then captured and floated to the surface, forming a foam product. After solid-liquid separation, the product becomes scum, while the Ca-based components (such as calcium carbonate, calcium sulfate, etc.) in the fly ash remain at the bottom of the flotation cell, forming tailings. This invention achieves the removal of heavy metals and chloride salts from fly ash, as well as the retention of Ca-based components, through the synergistic effect of selecting an aqueous sulfuric acid solution as the flotation solvent and the collector during the flotation process.

[0017] Fourthly, a flotation system for decontamination and calcium retention of waste incineration fly ash, used to implement the flotation method described in the third aspect of the present invention, includes:

[0018] Sulfuric acid storage tank, configured for adding sulfuric acid into the flotation unit;

[0019] A flotation device is configured to separate fly ash from waste incineration by flotation.

[0020] Collector storage tank, configured for adding collector into the flotation unit;

[0021] A conditioning agent storage tank is configured for adding conditioning agents into the flotation unit;

[0022] A frother storage tank is configured for adding frother to the flotation unit.

[0023] Fifthly, a type of fly ash tailings is obtained by the flotation method described in the first aspect of the present invention or the flotation method described in the third aspect of the present invention.

[0024] Sixthly, the application of the fly ash tailings described in the fifth aspect of the present invention in the preparation of building materials.

[0025] The beneficial effects of this invention are as follows:

[0026] 1. This invention firstly involves appropriately acidifying fly ash, which not only converts calcium ions into precipitates or slightly water-soluble components but also releases chloride ions from the fly ash. Specifically, the appropriate acidification treatment includes natural carbonation pretreatment and the selection of sulfuric acid aqueous solution as the flotation solution. Natural carbonation pretreatment utilizes carbon dioxide from the air, requiring no additional chemical reagents, resulting in low cost and no secondary pollution. The selection of sulfuric acid aqueous solution as the flotation solution, by directly adding sulfuric acid to control the pH value at the experimental endpoint, allows for the removal of some sparingly soluble and insoluble chloride salts (Friedel's salts) from the fly ash, improving the removal efficiency of Cl.

[0027] 2. Compared with traditional fly ash flotation, this invention uses mineral processing reagents as collectors to simultaneously and efficiently collect multiple heavy metals such as Pb, Cd, Cu, and Zn from fly ash, increasing the heavy metal content in the slag and effectively reducing the heavy metal leaching concentration in the tailings. At the same time, combined with fly ash acidification treatment, it achieves efficient separation of calcium resources and pollutants in fly ash, obtaining calcium carbonate products with low heavy metal content and improving the utilization rate of fly ash resources.

[0028] 3. This invention can effectively remove heavy metals and chloride salts from waste incineration fly ash while retaining the Ca-based components in the fly ash, thus achieving harmless treatment and resource utilization of fly ash. Attached Figure Description

[0029] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0030] Figure 1 The flowcharts are for the flotation methods for decontamination and calcium retention of waste incineration fly ash in Examples 1-8 of this invention.

[0031] Figure 2 The flowcharts are for the flotation methods for decontamination and calcium retention of waste incineration fly ash in Examples 9-12 of this invention. Detailed Implementation

[0032] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0033] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0034] The flotation described in this invention refers to the process of separating harmful and beneficial components in slurry through flotation reagents and aeration and stirring. The solid obtained after the ash-containing foam scraped off during flotation is dried by filtration is called scum. The solution obtained after filtration of the slurry after flotation is called flotation waste liquid, and the solid obtained is called tailings.

[0035] Given that the heavy metals present in fly ash can leach out and cause secondary pollution when it comes into contact with water during its use in building materials, and that the chlorine present in fly ash can cause corrosion damage to instruments and equipment during co-processing in cement kilns, thus affecting the resource reuse of fly ash, this invention proposes a flotation method and system for decontamination and calcium preservation of waste incineration fly ash.

[0036] A typical embodiment of the present invention provides a flotation method for decontamination and calcium retention of waste incineration fly ash. The fly ash is placed in a natural environment for natural carbonation reaction until the pH value reaches 7-9 to obtain pretreated fly ash. The pretreated fly ash is mixed with water, and a collector and a frother are added for flotation separation. The collector is one or more of butyl xanthate, butylammonium black powder, and ethyl thiocyanate.

[0037] In some embodiments, the natural carbonation reaction takes 5 to 7 days.

[0038] In some embodiments, during the flotation process, the liquid-to-solid ratio of water to pretreated fly ash is 9–11:1, L / kg.

[0039] In some embodiments, during the flotation process, the air flow rate is 200–400 L / h, and the air introduction time is 5–15 min.

[0040] In some embodiments, the mass ratio of pretreated fly ash to collector is 100:0.05 to 1.10. When the collector is ethyl thiocyanate, the mass ratio of pretreated fly ash to collector is 100:0.05 to 0.10. When the collector is butyl xanthate and butylammonium black powder, the mass ratio of pretreated fly ash to collector is 100:0.90 to 1.00. The mass ratio of butyl xanthate and butylammonium black powder is 0.9 to 1.0:1.

[0041] In some embodiments, the foaming agent is sodium dodecyl sulfate.

[0042] In some embodiments, the mass ratio of pretreated fly ash to foaming agent is 100:0.03 to 0.05.

[0043] In some embodiments, a conditioning agent is also added during the flotation separation process. Specifically, the conditioning agent is sodium sulfide. Specifically, the mass ratio of pretreated fly ash to conditioning agent is 100:0.09 to 0.11.

[0044] Another embodiment of the present invention provides a flotation system for decontamination and calcium retention of waste incineration fly ash, used to implement the above-mentioned flotation method, comprising:

[0045] The pretreatment unit is configured to allow the fly ash from waste incineration to undergo a natural carbonation reaction in the natural environment.

[0046] A flotation device, configured to separate materials from a pretreatment unit by flotation;

[0047] Collector storage tank, configured for adding collector into the flotation unit;

[0048] A conditioning agent storage tank is configured for adding conditioning agents into the flotation unit;

[0049] A frother storage tank is configured for adding frother to the flotation unit.

[0050] The third embodiment of the present invention provides a flotation method for decontamination and calcium retention of waste incineration fly ash. The fly ash is mixed with sulfuric acid aqueous solution as flotation liquid, and then a collector and a frother are added for flotation separation. The collector is one or more of butyl xanthate, butylammonium black powder, and ethyl thiocyanate.

[0051] In some embodiments, 20-22 mL of 98% sulfuric acid (by mass) is added per 100 g of fly ash treated. By calculating the acid neutralization capacity of the fly ash, the amount of H₂ required by the fly ash to neutralize the system at pH 7 can be calculated. + The amount of substance is used to calculate the required mass of sulfuric acid. The theoretical formula for calculating the acid neutralization capacity (ANC) of fly ash is as follows:

[0052]

[0053] In the formula, ANC is the numerical value of the acid neutralization capacity of fly ash; The mass fraction (%) of Al2O3 in fly ash; The mass fraction (%) of Fe2O3 in fly ash; ω CaP The mass fraction (%) of CaO in fly ash; ω MgP The mass fraction (%) of MgO in fly ash; The mass fraction (%) of K2O in fly ash; The mass fraction (%) of Na2O in fly ash; The mass fraction (%) of SO3 in fly ash; The mass fraction (%) of H2SO4 in fly ash.

[0054] When calculating the amount of sulfuric acid added, assuming complete electrolysis of sulfuric acid in water, the final pH value of the flotation system is 7. Therefore, the H+ produced by sulfuric acid electrolysis... + The amount of substance must be numerically equal to the ANC of the fly ash. The formula for calculating the mass of sulfuric acid required per gram of fly ash is as follows:

[0055]

[0056] In the formula, m is the mass (g) of sulfuric acid required per gram of fly ash; ANC is the acid neutralization capacity of fly ash.

[0057] Combining the two formulas above and converting the units, we obtain the mass of sulfuric acid required to be added per kilogram of fly ash:

[0058]

[0059] In the formula, ANC is the numerical value of the acid neutralization capacity of fly ash; The mass fraction (%) of Al2O3 in fly ash; The mass fraction (%) of Fe2O3 in fly ash; ω CaP The mass fraction (%) of CaO in fly ash; ω MgO The mass fraction (%) of MgO in fly ash; The mass fraction (%) of K2O in fly ash; The mass fraction (%) of Na2O in fly ash; The mass fraction (%) of SO3 in fly ash; The mass fraction (%) of H2SO4 in fly ash.

[0060] In some embodiments, during the flotation process, the liquid-to-solid ratio of the flotation solution to the pretreated fly ash is 9–11:1, L / kg.

[0061] In some embodiments, during the flotation process, the air flow rate is 200–400 L / h, and the air introduction time is 5–15 min.

[0062] In some embodiments, the mass ratio of pretreated fly ash to collector is 100:0.05 to 1.10. When the collector is ethyl thiocyanate, the mass ratio of pretreated fly ash to collector is 100:0.05 to 0.10. When the collector is butyl xanthate and butylammonium black powder, the mass ratio of pretreated fly ash to collector is 100:0.90 to 1.00. The mass ratio of butyl xanthate and butylammonium black powder is 0.9 to 1.0:1.

[0063] In some embodiments, the foaming agent is sodium dodecyl sulfate.

[0064] In some embodiments, the mass ratio of pretreated fly ash to foaming agent is 100:0.03 to 0.05.

[0065] In some embodiments, a conditioning agent is also added during the flotation separation process. Specifically, the conditioning agent is sodium sulfide. Specifically, the mass ratio of pretreated fly ash to conditioning agent is 100:0.09 to 0.11.

[0066] A fourth embodiment of the present invention provides a flotation system for decontamination and calcium retention of waste incineration fly ash, used to implement the above-mentioned flotation method, comprising:

[0067] Sulfuric acid storage tank, configured for adding sulfuric acid into the flotation unit;

[0068] A flotation device is configured to separate fly ash from waste incineration by flotation.

[0069] Collector storage tank, configured for adding collector into the flotation unit;

[0070] A conditioning agent storage tank is configured for adding conditioning agents into the flotation unit;

[0071] A frother storage tank is configured for adding frother to the flotation unit.

[0072] The fifth embodiment of the present invention provides a fly ash tailings obtained by the above-described flotation method.

[0073] The sixth embodiment of the present invention provides an application of the above-mentioned fly ash tailings in the preparation of building materials.

[0074] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.

[0075] Example 1

[0076] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 1 As shown, the steps are as follows:

[0077] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 5 days to carry out a natural carbonation reaction to achieve mild carbonation treatment.

[0078] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0079] (3) Add 0.46g butyl xanthate and 0.50g butyl ammonium black to the mortar, stir and mix thoroughly, then add 0.04g sodium dodecyl sulfate and stir again to ensure uniform dispersion of the agent.

[0080] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state.

[0081] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0082] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0083] Leachate was prepared from the tailings using the horizontal oscillation method (HJ 557-2010) for leaching toxicity of solid waste. The concentration of heavy metals in the leachate was determined using inductively coupled plasma optical emission spectrometry (ICP-OES). A tailings digest was prepared using the hot plate digestion method (HJ 766-2015) for the determination of metallic elements in solid waste. The Ca content in the tailings digest and the Ca loss in the flotation waste liquor were determined using the EDTA titration method (GB 7476-1987) for the determination of calcium in water. The concentration of heavy metals in the tailings digest was determined according to the silver nitrate titration method (GB 7476-1987) for the determination of chloride in water.

[0084] The standard (11896-1989) is used to test the soluble chlorine content in tailings.

[0085] Example 2

[0086] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 1 As shown, the steps are as follows:

[0087] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 5 days to carry out a natural carbonation reaction to achieve mild carbonation treatment.

[0088] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0089] (3) Add 0.07g of ethyl thiocyanate to the mortar, stir and mix thoroughly, then add 0.04g of sodium dodecyl sulfate and stir again to ensure that the agent is evenly dispersed.

[0090] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state.

[0091] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0092] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0093] Leachate was prepared from the tailings according to the method in HJ 557-2010, and the concentration of heavy metals in the leachate was determined by ICP-OES. Tailings digestate was prepared from the tailings using the hot plate digestion method in HJ 766-2015, and the Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987. The soluble chlorine content in the tailings was determined according to GB 11896-1989.

[0094] Example 3

[0095] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 1 As shown, the steps are as follows:

[0096] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 5 days to carry out a natural carbonation reaction to achieve mild carbonation treatment.

[0097] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0098] (3) Add 0.07g ethyl thiocyanate, 0.46g butyl xanthate and 0.50g butyl ammonium black to the mortar, stir and mix thoroughly, then add 0.04g sodium dodecyl sulfate and stir again to ensure uniform dispersion of the agents.

[0099] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state.

[0100] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0101] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0102] Leachate was prepared from the tailings according to the method in HJ 557-2010, and the concentration of heavy metals in the leachate was determined by ICP-OES. Tailings digestate was prepared from the tailings using the hot plate digestion method in HJ 766-2015, and the Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987. The soluble chlorine content in the tailings was determined according to GB 11896-1989.

[0103] Example 4

[0104] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 1 As shown, the steps are as follows:

[0105] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 5 days to carry out a natural carbonation reaction to achieve mild carbonation treatment.

[0106] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0107] (3) Add 0.10g sodium sulfide to the mortar and stir for 2 minutes. Then add 0.07g ethyl thiocyanate, 0.46g butyl xanthate and 0.50g butyl ammonium black powder. After mixing thoroughly, add 0.04g sodium dodecyl sulfate and stir a second time to ensure that the agent is evenly dispersed.

[0108] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state;

[0109] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0110] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0111] Leachate was prepared from the tailings according to the method in HJ 557-2010, and the concentration of heavy metals in the leachate was determined by ICP-OES. Tailings digestate was prepared from the tailings using the hot plate digestion method in HJ 766-2015, and the Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987. The soluble chlorine content in the tailings was determined according to GB 11896-1989.

[0112] Example 5

[0113] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 1 As shown, the steps are as follows:

[0114] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 7 days to carry out a natural carbonation reaction to achieve heavy carbonation treatment.

[0115] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0116] (3) Add 0.46g butyl xanthate and 0.50g butyl ammonium black to the mortar, stir and mix thoroughly, then add 0.04g sodium dodecyl sulfate and stir again to ensure uniform dispersion of the agent.

[0117] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state;

[0118] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0119] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0120] Leachate was prepared from the tailings according to the method in HJ 557-2010, and the concentration of heavy metals in the leachate was determined by ICP-OES. Tailings digestate was prepared from the tailings using the hot plate digestion method in HJ 766-2015, and the Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987. The soluble chlorine content in the tailings was determined according to GB 11896-1989.

[0121] Example 6

[0122] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 1 As shown, the steps are as follows:

[0123] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 7 days to carry out a natural carbonation reaction to achieve heavy carbonation treatment.

[0124] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0125] (3) Add 0.07g of ethyl thiocyanate to the mortar, stir and mix thoroughly, then add 0.04g of sodium dodecyl sulfate and stir again to ensure that the agent is evenly dispersed.

[0126] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state;

[0127] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0128] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0129] Leachate was prepared from the tailings according to the method in HJ 557-2010, and the concentration of heavy metals in the leachate was determined by ICP-OES. Tailings digestate was prepared from the tailings using the hot plate digestion method in HJ 766-2015, and the Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987. The soluble chlorine content in the tailings was determined according to GB 11896-1989.

[0130] Example 7

[0131] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 1 As shown, the steps are as follows:

[0132] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 7 days to carry out a natural carbonation reaction to achieve heavy carbonation treatment.

[0133] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0134] (3) Add 0.07g ethyl thiocyanate, 0.46g butyl xanthate and 0.50g butyl ammonium black to the mortar, stir and mix thoroughly, then add 0.04g sodium dodecyl sulfate and stir again to ensure uniform dispersion of the agents.

[0135] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state.

[0136] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0137] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0138] Leachate was prepared from the tailings according to the method in HJ 557-2010, and the concentration of heavy metals in the leachate was determined by ICP-OES. Tailings digestate was prepared from the tailings using the hot plate digestion method in HJ 766-2015, and the Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987. The soluble chlorine content in the tailings was determined according to GB 11896-1989.

[0139] Example 8

[0140] A flotation method for decontamination and calcium preservation of waste incineration fly ash, comprising the following steps:

[0141] (1) Place the fly ash from waste incineration in the natural environment and expose it to the air for 7 days to carry out a natural carbonation reaction to achieve heavy carbonation treatment.

[0142] (2) After drying and crushing the fly ash pretreated by natural carbonation, weigh 100g of sample, add deionized water at a liquid-solid ratio of 10:1 (L / kg), place it in a flotation tank and stir at 300r / min for 10min to fully wet the fly ash and obtain a uniform slurry.

[0143] (3) Add 0.10g sodium sulfide to the mortar and stir for 2 minutes. Then add 0.07g ethyl thiocyanate, 0.46g butyl xanthate and 0.50g butyl ammonium black powder. After mixing thoroughly, add 0.04g sodium dodecyl sulfate and stir a second time to ensure that the agent is evenly dispersed.

[0144] (4) Turn on the air supply device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state;

[0145] (5) Immediately after aeration, use a scraper to collect the ash-containing foam. Continue aeration for 10 minutes, then stop aeration and stirring, and collect the two products, ash-containing foam and tailings, respectively.

[0146] (6) A vacuum filtration device is used to separate the two products into solid and liquid components. The solid product obtained after vacuum filtration of the ash-containing foam is called scum, and the solid product obtained after vacuum filtration of the tailings is called tailings. The liquid generated during the vacuum filtration process is collected as flotation waste liquid.

[0147] Leachate was prepared from the tailings according to the method in HJ 557-2010, and the concentration of heavy metals in the leachate was determined by ICP-OES. Tailings digestate was prepared from the tailings using the hot plate digestion method in HJ 766-2015, and the Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987. The soluble chlorine content in the tailings was determined according to GB 11896-1989.

[0148] The data obtained from the testing of Examples 1 to 8 are as follows:

[0149] Table 1. Experimental data of flotation tailings from Examples 1-8

[0150]

[0151] According to the data in Table 1, the heavy metal leaching concentration of the flotation tailings in Examples 1-8 is superior to that of traditionally washed fly ash. Specifically, the heavy metal leaching concentration of the tailings after flotation fully meets the limits required by the "Integrated Wastewater Discharge Standard" (GB 8978-1996). Simultaneously, the soluble chlorine content of the tailings is significantly lower than that of traditionally washed fly ash, and is strictly controlled within the limits specified in the "Technical Specification for Pollution Control of Municipal Solid Waste Incineration Fly Ash" (HJ 1134-2020) (the specification requires that the soluble chlorine content of fly ash after pretreatment not exceed 2%, and preferably not higher than 1%). Furthermore, the Ca loss rate of this method is significantly reduced compared to the traditional washing process, and the Ca content in the tailings is higher than that of traditionally washed fly ash. This result fully demonstrates the significant advantage of this method in reducing the loss of Ca-based components.

[0152] Example 9

[0153] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 2 As shown, the steps are as follows:

[0154] (1) Place the fly ash sample in an oven to dry, and weigh 100g of the dried sample and place it in a flotation cell.

[0155] (2) Add flotation solution (sulfuric acid aqueous solution, prepared by taking 21 mL of sulfuric acid (mass fraction of 98%) and diluting it with water to 1 L) at a liquid-to-solid ratio of 10:1 (L / kg), and stir continuously at a speed of 300 r / min for 10 min to obtain a uniform mortar.

[0156] (3) Add 0.46g of butyl xanthate and 0.50g of butyl ammonium black to the mortar and stir for 2 minutes to mix them thoroughly. Then add 0.04g of sodium dodecyl sulfate as a foaming agent and continue stirring for 30 seconds to disperse the agents evenly.

[0157] (4) Start the aeration device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state to start the flotation operation.

[0158] (5) During the flotation process, a scraper is used to collect the ash-containing foam. After continuous aeration for 10 minutes, the aeration and stirring devices are turned off. The ash-containing foam and the tailings are collected separately and separated by filtration. The ash-containing foam is filtered to obtain scum, the tailings are filtered to obtain tailings, and the filtrate is the flotation waste liquid.

[0159] Leachate was prepared from tailings according to the method in HJ 557-2010, and scum digestate was prepared from scum using the hot plate digestion method in HJ 766-2015. The heavy metal concentration in the tailings leachate and the heavy metal content in the scum digestate were determined using ICP-OES. The Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987 standard. The soluble chlorine content in the tailings was determined according to GB 11896-1989 standard.

[0160] Example 10

[0161] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 2 As shown, the steps are as follows:

[0162] (1) Place the fly ash sample in an oven to dry, and weigh 100g of the dried sample and place it in a flotation cell.

[0163] (2) Add flotation solution (sulfuric acid aqueous solution, prepared by taking 21 mL of sulfuric acid (mass fraction of 98%) and diluting it with water to 1 L) at a liquid-to-solid ratio of 10:1 (L / kg), and stir continuously at a speed of 300 r / min for 10 min to obtain a uniform mortar.

[0164] (3) Add 0.07g of collector ethyl thiocyanate to the mortar and stir for 2 minutes to mix it thoroughly. Then add 0.04g of foaming agent sodium dodecyl sulfate and continue stirring for 30 seconds to disperse the agent evenly.

[0165] (4) Start the aeration device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state to start the flotation operation.

[0166] (5) During the flotation process, a scraper is used to collect the ash-containing foam. After continuous aeration for 10 minutes, the aeration and stirring devices are turned off. The ash-containing foam and the tailings are collected separately and separated by filtration. The ash-containing foam is filtered to obtain scum, the tailings are filtered to obtain tailings, and the filtrate is the flotation waste liquid.

[0167] Leachate was prepared from tailings according to the method in HJ 557-2010, and scum digestate was prepared from scum using the hot plate digestion method in HJ 766-2015. The heavy metal concentration in the tailings leachate and the heavy metal content in the scum digestate were determined using ICP-OES. The Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987 standard. The soluble chlorine content in the tailings was determined according to GB 11896-1989 standard.

[0168] Example 11

[0169] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 2As shown, the steps are as follows:

[0170] (1) Place the fly ash sample in an oven to dry, and weigh 100g of the dried sample and place it in a flotation cell.

[0171] (2) Add flotation solution (sulfuric acid aqueous solution, prepared by taking 21 mL of sulfuric acid (mass fraction of 98%) and diluting it with water to 1 L) at a liquid-to-solid ratio of 10:1 (L / kg), and stir continuously at a speed of 300 r / min for 10 min to obtain a uniform mortar.

[0172] (3) Add 0.46g of butyl xanthate, 0.50g of butyl ammonium black powder and 0.07g of ethyl thiocyanate to the mortar, stir for 2 minutes to mix them thoroughly, then add 0.04g of sodium dodecyl sulfate foaming agent and continue stirring for 30 seconds to disperse the agents evenly.

[0173] (4) Start the aeration device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state to start the flotation operation.

[0174] (5) During the flotation process, a scraper is used to collect the ash-containing foam. After continuous aeration for 10 minutes, the aeration and stirring devices are turned off. The ash-containing foam and the tailings are collected separately and separated by filtration. The ash-containing foam is filtered to obtain scum, the tailings are filtered to obtain tailings, and the filtrate is the flotation waste liquid.

[0175] Leachate was prepared from tailings according to the method in HJ 557-2010, and scum digestate was prepared from scum using the hot plate digestion method in HJ 766-2015. The heavy metal concentration in the tailings leachate and the heavy metal content in the scum digestate were determined using ICP-OES. The Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987 standard. The soluble chlorine content in the tailings was determined according to GB 11896-1989 standard.

[0176] Example 12

[0177] A flotation method for decontamination and calcium retention of fly ash from waste incineration, such as... Figure 2 As shown, the steps are as follows:

[0178] (1) Place the fly ash sample in an oven to dry, and weigh 100g of the dried sample and place it in a flotation cell.

[0179] (2) Add flotation solution (sulfuric acid aqueous solution, prepared by taking 21 mL of sulfuric acid (mass fraction of 98%) and diluting it with water to 1 L) at a liquid-to-solid ratio of 10:1 (L / kg), and stir continuously at a speed of 300 r / min for 10 min to obtain a uniform mortar.

[0180] (3) Add 0.1g of sodium sulfide as a modifier to the mortar and stir for 2 minutes. Then add 0.46g of butyl xanthate, 0.50g of butyl ammonium black powder and 0.07g of ethyl thiocyanate as collectors and stir for 2 minutes to mix them thoroughly. Then add 0.04g of sodium dodecyl sulfate as a foaming agent and continue stirring for 30 seconds to disperse the agents evenly.

[0181] (4) Start the aeration device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state to start the flotation operation.

[0182] (5) During the flotation process, a scraper is used to collect the ash-containing foam. After continuous aeration for 10 minutes, the aeration and stirring devices are turned off. The ash-containing foam and the tailings are collected separately and separated by filtration. The ash-containing foam is filtered to obtain scum, the tailings are filtered to obtain tailings, and the filtrate is the flotation waste liquid.

[0183] Leachate was prepared from tailings according to the method in HJ 557-2010, and scum digestate was prepared from scum using the hot plate digestion method in HJ 766-2015. The heavy metal concentration in the tailings leachate and the heavy metal content in the scum digestate were determined using ICP-OES. The Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987 standard. The soluble chlorine content in the tailings was determined according to GB 11896-1989 standard.

[0184] Example 13

[0185] (1) Place the fly ash sample in an oven to dry, and weigh 100g of the dried sample and place it in a flotation cell.

[0186] (2) Add flotation solution (sulfuric acid aqueous solution, prepared by taking 21 mL of sulfuric acid (mass fraction of 98%) and diluting it with water to 1 L) at a liquid-to-solid ratio of 10:1 (L / kg), and stir continuously at a speed of 300 r / min for 10 min to obtain a uniform mortar.

[0187] (3) Add 1.25 mL of collector kerosene to the mortar and stir for 2 min to mix it thoroughly. Then add 0.15 g of foaming agent sodium dodecyl sulfate and continue stirring for 30 s to disperse the agent evenly.

[0188] (4) Start the aeration device and introduce air at a constant flow rate of 300L / h while maintaining the stirring state to start the flotation operation.

[0189] (5) During the flotation process, a scraper is used to collect the ash-containing foam. After continuous aeration for 10 minutes, the aeration and stirring devices are turned off. The ash-containing foam and the tailings are collected separately and separated by filtration. The ash-containing foam is filtered to obtain scum, the tailings are filtered to obtain tailings, and the filtrate is the flotation waste liquid.

[0190] Leachate was prepared from tailings according to the method in HJ 557-2010, and scum digestate was prepared from scum using the hot plate digestion method in HJ 766-2015. The heavy metal concentration in the tailings leachate and the heavy metal content in the scum digestate were determined using ICP-OES. The Ca content in the tailings digestate and the Ca loss in the flotation waste liquor were determined according to GB 7476-1987 standard. The soluble chlorine content in the tailings was determined according to GB 11896-1989 standard.

[0191] The data obtained from the testing of Examples 9 to 13 are as follows:

[0192] Table 2. Experimental data of flotation tailings from Examples 9-13

[0193]

[0194] Table 3. Experimental data of flotation scum in Examples 9-13

[0195]

[0196] According to the data in Table 2, the heavy metal leaching concentrations of the tailings from Examples 9-12 meet the limits specified in the "Integrated Wastewater Discharge Standard" (GB 8978-1996), and the soluble chlorine content is also lower than the limits specified in the "Technical Specification for Pollution Control of Fly Ash from Municipal Solid Waste Incineration" (HJ1134-2020). Of particular note is the outstanding performance of this method in reducing the Ca loss rate, which is lower than that of conventional flotation and significantly lower than the Ca loss rate of traditional water-washed fly ash processes (approximately 40%). The Ca content in the tailings from Examples 9-12 is higher than that from Example 13 (conventional flotation), indicating that this method can effectively reduce the loss of Ca-based components and retain them adequately in the tailings. Table 2 data further shows that this method has significant advantages in heavy metal enrichment: compared with conventional flotation, the heavy metal content in the scum of Examples 9-12 is significantly increased, with the enrichment effect of Zn increasing by 79.5%, the enrichment effect of Pb increasing by 270.0%, and the enrichment effect of Cd reaching a significant increase of 1472.6%, which fully demonstrates the superiority of this method.

[0197] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A flotation method for decontamination and calcium conservation of waste incineration fly ash, characterized by, The fly ash from waste incineration is placed in a natural environment for natural carbonation reaction for 5 to 7 days until the pH value reaches 7 to 9, resulting in pretreated fly ash. The pretreated fly ash is then mixed with water, and a collector and a frother are added for flotation separation. The collector is one or more of butyl xanthate, butylammonium black powder, and ethyl thiocyanate. The mass ratio of pretreated fly ash to collector is 100:0.05~1.10; when the collector is ethyl thiocyanate, the mass ratio of pretreated fly ash to collector is 100:0.05~0.10; when the collector is butyl xanthate and butyl ammonium black powder, the mass ratio of pretreated fly ash to collector is 100:0.90~1.00, and the mass ratio of butyl xanthate and butyl ammonium black powder is 0.9~1.0:

1. Specifically, the removal of heavy metals and chloride salts from fly ash, as well as the retention of Ca-based components, are achieved through the synergistic effect of the natural carbonation reaction process and the collector during the flotation process. During the flotation process, the liquid-to-solid ratio of the flotation solution to the pretreated fly ash is 9~11:1, L / kg; During the flotation process, the air flow rate is 200~400 L / h, and the air introduction time is 5~15 min.

2. A flotation system for decontamination and calcium retention of fly ash from waste incineration, characterized in that, To implement the flotation method of claim 1, the method comprises: The pretreatment unit is configured to allow the fly ash from waste incineration to undergo a natural carbonation reaction in the natural environment. A flotation device, configured to separate materials from a pretreatment unit by flotation; Collector storage tank, configured for adding collector into the flotation unit; A conditioning agent storage tank is configured for adding conditioning agents into the flotation unit; A frother storage tank is configured for adding frother to the flotation unit.

3. A flotation method for decontamination and calcium retention of fly ash from waste incineration, characterized in that, After mixing the waste fly ash with sulfuric acid aqueous solution, a collector and a frother are added for flotation separation; the collector is one or more of butyl xanthate, butylammonium black powder, and ethyl thiocyanate; 20-22 mL of 98% sulfuric acid is added for every 100 g of fly ash treated. The fly ash from waste incineration is placed in a natural environment for natural carbonation for 5-7 days until the pH value reaches 7-9, resulting in pretreated fly ash. The mass ratio of the pretreated fly ash to the collector is 100:0.05-1.

10. When the collector is ethyl thiocyanate, the mass ratio of the pretreated fly ash to the collector is 100:0.05-0.

10. When the collector is butyl xanthate and butylammonium black powder, the mass ratio of the pretreated fly ash to the collector is 100:0.90-1.00, and the mass ratio of butyl xanthate and butylammonium black powder is 0.9-1.0:

1. Specifically, by selecting sulfuric acid aqueous solution as the flotation solution and working synergistically with the collector during the flotation process, the removal of heavy metals and chloride salts from fly ash and the retention of Ca-based components are achieved. During the flotation process, the liquid-to-solid ratio of the flotation solution to the pretreated fly ash is 9~11:1, L / kg; During the flotation process, the air flow rate is 200~400 L / h, and the air introduction time is 5~15 min.

4. The flotation method as described in claim 1 or 3, characterized in that, The mass ratio of pretreated fly ash to collector is 100:0.05~1.10; Alternatively, the foaming agent is sodium dodecyl sulfate; Alternatively, the mass ratio of pretreated fly ash to foaming agent is 100:0.03~0.05; Alternatively, a modifier may need to be added during the flotation separation process.

5. The flotation method as described in claim 4, characterized in that, The modifier is sodium sulfide.

6. The flotation method as described in claim 4, characterized in that, The mass ratio of pretreated fly ash to modifier is 100:0.09~0.

11.

7. A flotation system for decontamination and calcium retention of fly ash from waste incineration, used to implement the flotation method described in claim 3, comprising: Sulfuric acid storage tank, configured for adding sulfuric acid into the flotation unit; A flotation device is configured to separate fly ash from waste incineration by flotation. Collector storage tank, configured for adding collector into the flotation unit; A conditioning agent storage tank is configured for adding conditioning agents into the flotation unit; A frother storage tank is configured for adding frother to the flotation unit.

8. A type of fly ash tailings, characterized in that, Obtained by the flotation method described in any one of claims 1, 3 to 6.

9. The application of the fly ash tailings as described in claim 8 in the preparation of building materials.

Citation Information

Patent Citations

  • Method for preparing sulphoaluminate cement raw material by using incineration fly ash and formula of sulphoaluminate cement

    CN102923978A

  • Treatment method for two-step flotation of medical waste incineration fly ash

    CN105149101A

  • Resourceful treatment method for waste incineration fly ash

    CN114951236A

  • Fly ash deep dechlorination washing device

    CN221581462U