Preparation method of magnesium-carbon brick for converter bottom quick change

By designing and preparing gradient refractory materials, the problem of damage to magnesia-carbon bricks at the bottom of converters during the later stages of ordinary steelmaking was solved, achieving a stable slag-metal mushroom head structure and improving converter life and steelmaking efficiency.

CN119954498BActive Publication Date: 2026-11-24SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202510058369.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-01-15
Publication Date
2026-11-24
Estimated Expiration
2045-01-15

AI Technical Summary

Technical Problem

The existing magnesia-carbon bricks used for quick-change converter hearths are easily damaged in the later stages of ordinary steelmaking, resulting in a reduced furnace life and an inability to stably form a slag-metal mushroom head structure, which affects steelmaking efficiency and cost.

Method used

A gradient refractory material design is adopted, and magnesia-carbon bricks are prepared by equipment such as jaw crusher, Raymond mill and planetary mixer. Combined with additives such as phenolic resin, a gradient structure of reaction section, middle section and post section is formed to enhance erosion resistance and high temperature strength and promote the stability of slag-metal mushroom head.

Benefits of technology

In the early stages of converter smelting, a stable slag-metal mushroom head structure is formed, which increases the converter life, reduces the damage of magnesia-carbon bricks, improves steelmaking efficiency, and reduces costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a magnesia-carbon brick for quick-change converter hearth and its preparation method. The magnesia-carbon brick is a graded refractory material divided into a reaction section, a middle section, and a rear section. Block fused magnesia, sintered magnesia, forsterite, and calcium-containing magnesia are sequentially passed through a jaw crusher, a double-roll crusher, and a Raymond mill to obtain corresponding aggregate particles and matrix fine powder. The matrix fine powders from the reaction section, middle section, and rear section are pre-mixed uniformly according to the formula. Aggregate particles are then uniformly mixed according to the formula for the reaction section, middle section, and rear section. A phenolic resin binder is then added, and after uniform mixing, graphite is added, followed by the pre-mixed matrix fine powder. After uniform mixing, the mixture is transported to a brick press, where it is sequentially distributed, machine-pressed, and then heat-treated to obtain the magnesia-carbon brick for quick-change converter hearth. This invention overcomes the shortcomings of existing magnesia-carbon bricks for quick-change converter hearths, which require initial smelting of ordinary steel, and the direct damage to the magnesia-carbon bricks during the smelting of special steel. This invention stabilizes and extends the service life of the converter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of refractory materials, and more particularly to a magnesia-carbon brick for quick-change converter bottom and its preparation method. Background Technology

[0002] During steelmaking, the refractory material at the bottom of the converter is easily damaged due to prolonged exposure to high temperatures and corrosion. Traditional replacement methods require shutting down the furnace for cooling, which is not only time-consuming but also affects production efficiency. Therefore, the emergence of converter bottom quick-change technology enables rapid replacement of the refractory material at the bottom while the converter is hot, which is of great significance for improving steelmaking efficiency and reducing costs. To accelerate the turnover rate of its converters used for carbon steel smelting, Shanxi Taigang Stainless Steel Co., Ltd. has adopted the quick-change model, reducing the time from one week to less than three days.

[0003] While quick-change converter hearths shorten the lining time, they also impose strict requirements on the selection of steel grades. For example, in the first 35 heats or so, high-carbon steel grades (Q235B, Q195, etc.) must be smelted to form a slag-metal mushroom head with a stable structure, which covers the magnesia-carbon bricks at the converter hearth, protecting the converter hearth, reducing the impact of molten steel, slag, and smelting temperature fluctuations on the magnesia-carbon bricks at the hearth, avoiding the influence of the magnesia-carbon bricks on the molten steel, and extending the service life of the magnesia-carbon bricks at the converter hearth.

[0004] Shanxi Taiyuan Iron & Steel Co., Ltd. primarily smelts special steels such as stainless steel and silicon steel, with a relatively low proportion of ordinary steel like Q235. Smelting large quantities of ordinary steel like Q235 in the early stages not only wastes resources but also increases costs and extends delivery times. Smelting a small amount of ordinary steel initially followed by special steel leads to extensive damage to the magnesia-carbon bricks at the converter bottom, reducing the furnace life from approximately 8000 heats to just 5 heats. This is because special steel smelting causes damage to the slag-metal mushroom head, with the magnesia-carbon bricks at the bottom in direct contact with the steel / slag, and the high temperature of special steel smelting further exacerbates this damage. To extend furnace life and avoid the impact of special steel smelting on the magnesia-carbon bricks at the converter bottom in the early stages of smelting, a new type of magnesia-carbon brick needs to be developed. This new brick can form a stable slag-metal mushroom head structure in the early stages of smelting, protecting the magnesia-carbon bricks at the converter bottom, extending their lifespan, and maximizing the number of special steel smelting heats.

[0005] Currently, patents related to magnesia-carbon bricks for converters are concentrated in other parts of the converter or the bottom of non-fast-change converters, such as the patent "Preparation process of magnesia-carbon bricks at the converter taphole (CN202311726437.9)" and the patent "A low-carbon magnesia-carbon brick for stainless steel production in a converter and its preparation process (CN202311025636.7)". There are very few patents related to magnesia-carbon bricks for fast-change converter bottoms. For example, the patent "A method for replacing converter bottom blower bricks (CN201910483457)" focuses on the replacement method, not the magnesia-carbon bricks themselves. Furthermore, there are no reports on the use of magnesia-carbon bricks for fast-change converter bottoms in steel smelting.

[0006] The present invention aims to overcome the defects of the prior art and provides a magnesia-carbon brick for quick replacement of converter bottom and its preparation method. This invention overcomes the defects of the prior smelting of magnesia-carbon bricks for quick replacement of converter bottom, which requires ordinary steel and the smelting of special steel will directly damage the magnesia-carbon bricks of the converter bottom, thereby stabilizing and increasing the service life of the converter. Summary of the Invention

[0007] The purpose of this invention is to address the above-mentioned problems by providing a magnesia-carbon brick for quick replacement of converter hearth and its preparation method.

[0008] The objective of this invention is achieved as follows: a magnesia-carbon brick for quick-change converter hearth and its preparation method, comprising the following steps: Step 1: Aggregate preparation: 5-50mm fused magnesia, sintered magnesia, forsterite, and calcium-containing magnesia are sequentially crushed by a jaw crusher and screened into 0.1-1mm, 1-3mm, and 3-5mm particles; to maintain material balance, 10-70% of the 1-3mm or 3-5mm particles are further crushed into 0.1-1mm or 1-3mm particles by a double-roll crusher; the crushed particles are stored in the corresponding silos according to particle size; 0.1-1mm is called small particles, 1-3mm is called medium particles, and 3-5mm is called large particles; Step 2: Preparation of matrix fine powder: storage in silos. After processing 5-12 tons of particles from Step 1, storage is stopped. The particles from the jaw crusher are then directly fed into the Raymond mill. The resulting powder forms matrix fine powder with a particle size below 0.088mm, including fused magnesia fine powder, sintered magnesia fine powder, forsterite fine powder, and calcium-containing magnesia fine powder, which are stored in their respective silos. In actual production, Steps 1 and 2 can be performed simultaneously to shorten the aggregate and matrix preparation time. Step 3: Mixing and Molding: Transport trolleys transport the particles from each silo to the planetary mixer, and the fine powder to the Ericsson mixer. The mixed matrix fine powder is conveyed by belt to the planetary mixer, and the mixture is conveyed by belt to the brick press. The converter hearth quick-change magnesia-carbon bricks are gradient refractory materials with a total length of 860±30 mm. The sample is divided into a reaction section (260±10mm), a middle section (350±10mm), and a final section (350±10mm). In the reaction section, 3-5% of fused magnesia fine powder, 3-8% of sintered magnesia fine powder, 10-15% of calcium-containing magnesia fine powder, and 4-8% of forsterite fine powder are transported to an Ellis mixer and mixed for 3-5 minutes. During this time, 0.1-1% of aluminum powder and 0.2-0.9% of silica powder additives are manually added through the Ellis mixer's feed port. After uniform mixing, the matrix fine powder for the reaction section is obtained. The final section contains 1-3% fused magnesia particles with a large-to-medium-to-small particle ratio of 1:2:1, 4-7% sintered magnesia particles with a large-to-medium-to-small particle ratio of 1.2:2:0.8, and 30-45% of fused magnesia particles with a large-to-medium-to-small particle ratio of... The mixture consists of calcium magnesia sand particles in a ratio of 1.1:2:0.9 and 15-25% forsterite particles with a large, medium, and small particle size ratio of 1.05:2:0.95. These are transported to a planetary mixer and mixed for 3-5 minutes. Then, 3.0-3.6% phenolic resin binder is added and the mixture is stirred for another 3-5 minutes. Next, 14-18% low-carbon graphite fine powder is manually added and mixed for 4-5 minutes. Finally, the matrix fine powder from the reaction section is added and mixed for 3-5 minutes to obtain the reaction section mixture. In the intermediate section, 6-20% fused magnesia fine powder and 3-7% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 3-5 minutes. During this process, 0.5-1.5% aluminum powder and 0.4-1% aluminum powder are manually added through the Ericsson mixer's feed port.3% silica powder additive, after being mixed evenly, yields a mid-section matrix fine powder; 50-60% of fused magnesia particles with a large-to-medium-to-small particle ratio of 1:2:1 and 10-15% of sintered magnesia particles with a large-to-medium-to-small particle ratio of 1.2:2:0.8 are transported to a planetary mixer and mixed for 3-5 minutes, then 3.5-4.0% of phenolic resin binder is added and stirred for another 3-5 minutes, and finally 11-13% of high-purity graphite fine powder and 3% silica powder are manually added. -5% of the flake graphite particles are mixed for 4-5 minutes, and finally the intermediate matrix fine powder is added and mixed for 3-5 minutes to obtain the intermediate mixture; the downstream section: 3-9% of fused magnesia fine powder and 10-18% of sintered magnesia fine powder are transported to the Ericsson mixer and mixed for 3-5 minutes. During this period, 0.1-1.0% of aluminum powder and 0.2-0.9% of silicon powder additive are manually added from the Ericsson mixer feed port. After mixing evenly, the downstream matrix fine powder is obtained. 10-15% of fused magnesia particles with a large, medium, and small particle size ratio of 1:2:1 and 50-60% of sintered magnesia particles with a large, medium, and small particle size ratio of 1.2:2:0.8 are transported to a planetary mixer and mixed for 3-5 minutes. Then, 3.0-3.2% of phenolic resin binder is added and stirred for another 3-5 minutes. Next, 14-18% of high-purity graphite powder is manually added and mixed for 4-5 minutes. Finally, the aforementioned matrix powder is added and mixed for 3-5 minutes. The reaction section, middle section, and rear section mixtures are then transported to a brick press via belt conveyors. The bricks are distributed sequentially at 260±5mm for the reaction section, 350±5mm for the middle section, and 350±5mm for the rear section. After two pressure treatments (30-50MPa for 5-10s and 150-200MPa for 5-10s), the bricks are heat-treated at 200-250℃ for 24-32 hours to obtain the magnesia-carbon bricks for quick-change at the converter hearth.

[0009] The fused magnesia contains ≥97% MgO, ≤0.6% SiO2, ≤1.5% CaO, and ≤0.01% B2O3, with a particle size of 5-50 mm and a bulk density of 3.45-3.53 g / cm³. 3 The sintered magnesia has a true porosity of 0.5-2.5% and a grain size of 270-700 μm; the sintered magnesia contains ≥95% MgO, ≤2.2% SiO2, ≤1.8% CaO, has a particle size of 5-50 mm, and a bulk density of 3.20-3.47 g / cm³. 3 The true porosity is 0.3-3.5%, and the grain size is 10-200 μm; the forsterite has MgO+SiO2≥95%, SiO2≥40%, CaO≤1.0%, Al2O3≤1.0%, a particle size of 5-50 mm, and a bulk density of 3.22-3.33 g / cm³. 3The calcium-magnesium sand contains ≥90% MgO, 5-10% CaO, ∑SiO2+Al2O3+Fe2O3≤3.0%, has a particle size of 5-50mm, and a bulk density of 3.42-3.47g / cm³. 3 .

[0010] The jaw crusher has a production capacity of 250-350 t / h, a finished product size of 0-5 mm, and a maximum feed size of 700 mm; the double roll crusher has a production capacity of 50-100 t / h, a finished product size of 0-3 mm, and a maximum feed size of 60 mm; the Raymond mill has a production capacity of 10-320 t / d, a finished product size of 0.015-0.088 mm, and a maximum feed size of 30 mm; the Ericsson mixer is model RV24, with a speed of 0-1751 r / min; and the planetary mixer has a capacity of 800-1200 kg and is equipped with a heating function.

[0011] The aluminum powder has an Al content of ≥98%, Fe content of ≤0.5%, Si content of ≤0.5%, Cu content of ≤0.1%, and a particle size of 0.015-0.074 mm; the silicon powder has an Si content of ≥98%, and a particle size of 0.015-0.074 mm.

[0012] The phenolic resin is liquid with a viscosity of 0.75-0.95 Pa·s at 25°C, a water content of 1.5-2.5%, a solid content of 75-80%, a residual carbon rate of 43-48%, a free phenol content of 10.0-12.0%, and a pH value of 6.5-7.5.

[0013] The low-carbon graphite powder has 50-80% fixed carbon; the main ash components are SiO2, Al2O3 and Fe2O3, with ∑SiO2+Al2O3+Fe2O3 in the ash being 82.9-88.6%, of which SiO2 accounts for 33-59%, and the particle size is 0.044-0.074 mm.

[0014] The high-purity graphite powder has a fixed carbon content of ≥99.9% and a particle size of 0.074-0.1 mm.

[0015] The flake graphite particles have a fixed carbon content of ≥99.9% and a particle size of 1-3 mm.

[0016] The brick press is a friction brick press.

[0017] The magnesia-carbon bricks for quick-change converter bottoms are prepared according to the above-mentioned preparation method for magnesia-carbon bricks for quick-change converter bottoms.

[0018] The beneficial effects of this invention are as follows: The magnesia-carbon brick for quick-change converter bottom prepared by this invention is a gradient refractory material. The reaction section mainly consists of forsterite, periclase, calcite, and amorphous carbon. Forsterite, due to its high SiO2 content and low refractoriness (1710℃), readily reacts with converter slag. The presence of calcite provides a pathway for further erosion of periclase by the slag, easily forming a slag-metal mushroom head structure. Amorphous carbon, due to its numerous highly active sites, makes it difficult for metal elements such as Fe to oxidize, enhancing the stability of the slag-metal mushroom head. The high ash content of low-carbon graphite also allows for further fusion of the refractory material and slag, promoting faster fusion of the slag-metal mushroom head. Therefore, through the interaction between the reaction section of the magnesia-carbon brick for quick-change converter bottom and the slag, a stable slag-metal mushroom head structure is formed within the first 5 heats of converter smelting.

[0019] The main phases in the intermediate section are large-crystalline periclase and graphite of different particle sizes, exhibiting excellent erosion resistance. Even under extreme conditions, when the reaction section is completely slag-formed in the converter's intense smelting environment, it provides stable attachment sites for the slag-metal mushroom head, maintaining the stability of the slag-metal mushroom head structure; and it is not easily eroded by converter slag. Due to the presence of the reaction section, it is easy to slag-form, effectively buffering most of the thermal stress and mechanical force; therefore, the intermediate section can use a large amount of granular graphite and large-crystalline fused magnesia to maximize erosion resistance while less considering high-temperature strength. Taiyuan Iron & Steel's converter is a top-and-bottom blown converter; sometimes CO2 is used as the bottom-blown gas. Large-crystalline magnesia, flake graphite, and high-purity graphite have low reactivity and do not readily react with CO2.

[0020] The main phases in the latter stage are periclase and graphite. Periaclase has smaller grains, and graphite has a smaller grain size, thus exhibiting good high-temperature strength. Based on practical experience, when there is a low amount of high-carbon steel in the initial smelting, the converter bottom fractures are mostly located in the latter stage. Since the latter stage does not come into contact with slag, the main fracture failure mechanisms are mechanical or thermal spalling. Therefore, small-grained sintered magnesia is used to increase high-temperature strength, and high-purity magnesia is used to increase oxidation resistance, aiming to improve the overall fracture toughness of the latter stage.

[0021] Based on the principle of closest packing of particles, the proportions of large, medium and small particles in each aggregate are determined to reduce or even avoid segregation of the mixture during transportation and pressing, thereby improving the overall performance of magnesia-carbon bricks.

[0022] Therefore, the magnesia-carbon brick for quick-change converter bottom prepared by this invention overcomes the defects of existing magnesia-carbon bricks for quick-change converter bottom that require ordinary steel to be smelted in the early stage, and that smelting special steel will directly damage the magnesia-carbon bricks at the converter bottom. It stably forms slag-metal mushroom head, stabilizes and increases the service life of the converter. Detailed Implementation

[0023] The technical solution adopted in this invention is: the magnesia-carbon brick for quick-change converter bottom and its preparation method, characterized in that the preparation method comprises the following steps: Step 1 (aggregate preparation): 5-50mm fused magnesia, sintered magnesia, forsterite, and calcium-containing magnesia are sequentially crushed and screened into 0.1-1mm, 1-3mm, and 3-5mm particles by a jaw crusher; to ensure material block balance, 10-70% of the 1-3mm or 3-5mm particles can be further crushed into 0.1-1mm or 1-3mm particles by a double-roll crusher. The crushed particles are then stored in the corresponding silos according to particle size.

[0024] 0.1-1mm particles are called small particles, 1-3mm particles are called medium particles, and 3-5mm particles are called large particles.

[0025] Step 2 (Preparation of matrix fine powder): After storing 5-12 tons of the particles in the silo, storage is stopped. Next, the particles obtained from the jaw crusher are directly fed into the Raymond mill, and after pulverization, matrix fine powder (electrominated magnesia fine powder, sintered magnesia fine powder, forsterite fine powder, calcium-containing magnesia fine powder) with a particle size of less than 0.088 mm is formed and stored in the corresponding silo.

[0026] In actual production, steps one and two can be carried out simultaneously to shorten the preparation time of aggregates and matrix.

[0027] Step 3 (mixing and molding): Using computer-controlled trolleys, the above-mentioned granules are transported from each silo to the planetary mixer, the fine powder to the Ericsson mixer, the mixed matrix fine powder is transported by belt to the planetary mixer, and the mixture is transported by belt to the brick press.

[0028] The converter hearth quick-change magnesia-carbon brick is a gradient refractory material with a total length of 860±30mm, divided into a reaction section (260±10mm), a middle section (350±10mm), and a rear section (350±10mm).

[0029] Reaction section: 3-5% of fused magnesia fine powder, 3-8% of sintered magnesia fine powder, 10-15% of calcium-containing magnesia fine powder, and 4-8% of magnesium olivine fine powder are transported to an Ericsson mixer and mixed for 3-5 minutes. During this period, 0.1-1% of aluminum powder and 0.2-0.9% of silicon powder additives are manually added from the Ericsson mixer feed port. After mixing evenly, the matrix fine powder of the reaction section is obtained. 1-3% of fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1), 4-7% of sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8), 30-45% of calcium-containing magnesia particles (large, medium, and small particle mass ratio of 1.1:2:0.9), and 15-25% of forsterite particles (1.05:2:0.95) are transported to a planetary mixer and mixed for 3-5 minutes. Then, 3.0-3.6% of phenolic resin binder is added and stirred for another 3-5 minutes. Next, 14-18% of low-carbon graphite fine powder is manually added and mixed for 4-5 minutes. Finally, the matrix fine powder of the reaction section is added and mixed for 3-5 minutes to obtain the reaction section mixture.

[0030] Mid-section: 6-20% of fused magnesia fine powder and 3-7% of sintered magnesia fine powder are transported to an Erlich mixer and mixed for 3-5 minutes. During this period, 0.5-1.5% of aluminum powder and 0.4-1.3% of silicon powder additive are manually added from the Erlich mixer feed port. After mixing evenly, the mid-section matrix fine powder is obtained. 50-60% of fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1) and 10-15% of sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 3-5 minutes. Then, 3.5-4.0% of phenolic resin binder is added and stirred for another 3-5 minutes. Next, 11-13% of high-purity graphite fine powder and 3-5% of flake graphite particles (medium particles) are manually added and mixed for 4-5 minutes. Finally, the aforementioned intermediate matrix fine powder is added and mixed for 3-5 minutes to obtain the intermediate mixture.

[0031] The downstream section: 3-9% of fused magnesia fine powder and 10-18% of sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 3-5 minutes. During this time, 0.1-1.0% of aluminum powder and 0.2-0.9% of silicon powder additive are manually added through the Ericsson mixer feed port. After uniform mixing, the downstream matrix fine powder is obtained. 10-15% of fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1) and 50-60% of sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 3-5 minutes. Then, 3.0-3.2% of phenolic resin binder is added and the mixture is stirred for another 3-5 minutes. Next, 14-18% of high-purity graphite fine powder is manually added and mixed for 4-5 minutes. Finally, the downstream matrix fine powder is added and mixed for 3-5 minutes to obtain the downstream mixture.

[0032] The mixture from the reaction section, middle section, and rear section is transported to a brick press via belt conveyors. The mixture is then distributed sequentially at 260±5mm for the reaction section, 350±5mm for the middle section, and 350±5mm for the rear section. After being pressurized in two stages (30-50MPa for 5-10s and 150-200MPa for 5-10s), it is heat-treated at 200-250℃ for 24-32 hours to obtain the magnesia-carbon bricks for quick-change at the converter bottom.

[0033] The fused magnesia contains ≥97% MgO, ≤0.6% SiO2, ≤1.5% CaO, and ≤0.01% B2O3; particle size: 5-50mm; bulk density: 3.45-3.53g / cm³. 3 Porosity: 0.5-2.5%; Grain size: 270-700μm.

[0034] The aforementioned magnesia-carbon brick for quick-change converter hearth and its preparation method are characterized in that the sintered magnesia contains MgO ≥ 95%, SiO2 ≤ 2.2%, and CaO ≤ 1.8%; particle size: 5-50 mm; bulk density: 3.20-3.47 g / cm³. 3 Porosity: 0.3-3.5%; Grain size: 10-200μm.

[0035] The forsterite contains MgO+SiO2≥95%, SiO2≥40%, CaO≤1.0%, and Al2O3≤1.0%; the particle size is 5-50mm; and the bulk density is 3.22-3.33g / cm³. 3 .

[0036] The calcium-magnesium sand contains ≥90% MgO, 5-10% CaO, and ∑SiO2+Al2O3+Fe2O3≤3.0%; the particle size is 5-50mm; and the bulk density is 3.42-3.47g / cm³. 3 .

[0037] The jaw crusher has a production capacity of 250-350 t / h, a finished product size of 0-5 mm, and a maximum feed particle size of 700 mm.

[0038] The roller crusher has a production capacity of 50-100t / h, a finished product size of 0-3mm, and a maximum feed particle size of 60mm.

[0039] The Raymond mill has a production capacity of 10-320 t / d, a finished product size of 0.015-0.088 mm, and a maximum feed particle size of 30 mm.

[0040] The Ellis mixer is model RV24, with a rotation speed of 0-1751 r / min.

[0041] The planetary mixer has a capacity of 800-1200 kg and is equipped with a heating function.

[0042] The aluminum powder has an Al ≥ 98%, Fe ≤ 0.5%, Si ≤ 0.5%, and Cu ≤ 0.1%; the particle size is 0.015-0.074 mm.

[0043] The silicon powder has a Si content of ≥98% and a particle size of 0.015-0.074 mm.

[0044] The phenolic resin is liquid with a viscosity of 0.75-0.95 Pa·s at 25°C, a water content of 1.5-2.5%, a solid content of 75-80%, a residual carbon rate of 43-48%, a free phenol content of 10.0-12.0%, and a pH value of 6.5-7.5.

[0045] The low-carbon graphite powder has 50-80% fixed carbon; the main ash components are SiO2, Al2O3 and Fe2O3, and the ∑SiO2+Al2O3+Fe2O3 in the ash is 82.9-88.6%, of which SiO2 accounts for 33-59%; the particle size is 0.044-0.074 mm.

[0046] The high-purity graphite powder has a fixed carbon content of ≥99.9% and a particle size of 0.074-0.1 mm.

[0047] The flake graphite particles have a fixed carbon content of ≥99.9% and a particle size of 1-3 mm.

[0048] The brick press is a friction brick press with a capacity of 2500t.

[0049] The present invention will be further described below with reference to specific embodiments, but this is not intended to limit the scope of protection thereof.

[0050] To avoid repetition, the equipment and materials involved in the specific implementation methods are described uniformly as follows, and will not be repeated in the examples: The fused magnesia contains MgO≥97%, SiO2≤0.6%, CaO≤1.5%, B2O3≤0.01%; particle size: 5-50mm; bulk density: 3.45-3.53g / cm³. 3 Porosity: 0.5-2.5%; Grain size: 270-700μm.

[0051] The aforementioned magnesia-carbon brick for quick-change converter hearth and its preparation method are characterized in that the sintered magnesia contains MgO ≥ 95%, SiO2 ≤ 2.2%, and CaO ≤ 1.8%; particle size: 5-50 mm; bulk density: 3.20-3.47 g / cm³. 3 Porosity: 0.3-3.5%; Grain size: 10-200μm.

[0052] The forsterite contains MgO+SiO2≥95%, SiO2≥40%, CaO≤1.0%, and Al2O3≤1.0%; the particle size is 5-50mm; and the bulk density is 3.22-3.33g / cm³. 3 .

[0053] The aforementioned magnesia-carbon brick for quick-change converter hearth and its preparation method are characterized in that the calcium-magnesia sand contains ≥90% MgO, 5-10% CaO, and ∑SiO2+Al2O3+Fe2O3≤3.0%; the particle size is 5-50mm; and the bulk density is 3.42-3.47g / cm³. 3 .

[0054] The jaw crusher has a production capacity of 250-350 t / h, a finished product size of 0-5 mm, and a maximum feed particle size of 700 mm.

[0055] The roller crusher has a production capacity of 50-100t / h, a finished product size of 0-3mm, and a maximum feed particle size of 60mm.

[0056] The Raymond mill has a production capacity of 10-320 t / d, a finished product size of 0.015-0.088 mm, and a maximum feed particle size of 30 mm.

[0057] The Ellis mixer is model RV24, with a rotation speed of 0-1751 r / min.

[0058] The planetary mixer has a capacity of 800-1200 kg and is equipped with a heating function.

[0059] The aluminum powder has an Al ≥ 98%, Fe ≤ 0.5%, Si ≤ 0.5%, and Cu ≤ 0.1%; the particle size is 0.015-0.074 mm.

[0060] The silicon powder has a Si content of ≥98% and a particle size of 0.015-0.074 mm.

[0061] The phenolic resin is liquid with a viscosity of 0.75-0.95 Pa·s at 25°C, a water content of 1.5-2.5%, a solid content of 75-80%, a residual carbon rate of 43-48%, a free phenol content of 10.0-12.0%, and a pH value of 6.5-7.5.

[0062] The low-carbon graphite powder has 50-80% fixed carbon; the main ash components are SiO2, Al2O3 and Fe2O3, and the ∑SiO2+Al2O3+Fe2O3 in the ash is 82.9-88.6%, of which SiO2 accounts for 33-59%; the particle size is 0.044-0.074 mm.

[0063] The high-purity graphite powder has a fixed carbon content of ≥99.9% and a particle size of 0.074-0.1 mm.

[0064] The flake graphite particles have a fixed carbon content of ≥99.9% and a particle size of 1-3 mm.

[0065] The brick press is a friction brick press with a capacity of 2500t.

[0066] Example 1 (Complete Replacement)

[0067] A magnesia-carbon brick for quick replacement of converter hearth and its preparation method. This embodiment will completely replace the original bricks of the converter hearth. The preparation method includes the following steps: Step 1 (Aggregate Preparation): Fused magnesia (5-50mm), sintered magnesia, forsterite, and calcium-containing magnesia are sequentially crushed and screened into 0.1-1mm, 1-3mm, and 3-5mm particles using a jaw crusher. To ensure material particle size distribution, some of the 1-3mm or 3-5mm particles can be further crushed into 0.1-1mm or 1-3mm particles using a double-roll crusher. The crushed particles are then stored in the corresponding silos according to their particle size.

[0068] 0.1-1mm particles are called small particles, 1-3mm particles are called medium particles, and 3-5mm particles are called large particles.

[0069] Step 2 (Preparation of matrix fine powder): After storing a sufficient amount of the particles in the silo, storage is stopped. Next, the particles obtained from the jaw crusher are directly fed into the Raymond mill, and after pulverization, matrix fine powder (electrominated magnesia fine powder, sintered magnesia fine powder, forsterite fine powder, calcium-containing magnesia fine powder) with a particle size of less than 0.088 mm is formed and stored in the corresponding silo.

[0070] In actual production, steps one and two can be carried out simultaneously to shorten the preparation time of aggregates and matrix.

[0071] Step 3 (mixing and molding): Using computer-controlled trolleys, the above-mentioned granules are transported from each silo to the planetary mixer, the fine powder to the Ericsson mixer, the mixed matrix fine powder is transported by belt to the planetary mixer, and the mixture is transported by belt to the brick press.

[0072] The converter bottom quick-change magnesia-carbon brick is a gradient refractory material with a total length of 860mm, divided into a reaction section (260±10mm), a middle section (350±10mm), and a rear section (350±10mm).

[0073] Reaction section: 5% fused magnesia fine powder, 8% sintered magnesia fine powder, 10% calcium-containing magnesia fine powder, and 4% magnesium olivine fine powder are transported to an Ericsson mixer and mixed for 3 minutes. During this period, 0.1% aluminum powder and 0.2% silicon powder additives are manually added from the Ericsson mixer feed port. After mixing evenly, the matrix fine powder of the reaction section is obtained. 3% of fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1), 7% of sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8), 30% of calcium-containing magnesia particles (large, medium, and small particle mass ratio of 1.1:2:0.9), and 15% of forsterite particles (1.05:2:0.95) were transported to a planetary mixer and mixed for 3 minutes. Then, 3.6% of phenolic resin binder was added and stirred for another 3 minutes. Next, 18% of low-carbon graphite fine powder was manually added and mixed for 4 minutes. Finally, the matrix fine powder of the reaction section was added and mixed for 3 minutes to obtain the reaction section mixture.

[0074] Intermediate Section: 16% fused magnesia fine powder and 3% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 3 minutes. During this time, 0.5% aluminum powder and 0.4% silicon powder additives are manually added through the Ericsson mixer feed port. After uniform mixing, the intermediate section matrix fine powder is obtained. 55% fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1) and 10% sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 3 minutes. Then, 4.0% phenolic resin binder is added and the mixture is stirred for another 3 minutes. Next, 11% high-purity graphite fine powder and 5% flake graphite particles (medium particles) are manually added and mixed for 4 minutes. Finally, the intermediate section matrix fine powder is added and mixed for 3 minutes to obtain the intermediate section mixture.

[0075] The downstream section: 5% fused magnesia fine powder and 10% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 3 minutes. During this time, 0.1% aluminum powder and 0.9% silicon powder additives are manually added through the Ericsson mixer feed port. After uniform mixing, the downstream matrix fine powder is obtained. 11% fused magnesia particles (large, medium and small particle mass ratio of 1:2:1) and 59% sintered magnesia particles (large, medium and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 3 minutes. Then, 3.0% phenolic resin binder is added and mixed for another 3 minutes. Next, 15% high-purity graphite fine powder is manually added and mixed for 4 minutes. Finally, the downstream matrix fine powder is added and mixed for 3 minutes to obtain the downstream mixture.

[0076] The mixture from the reaction section, middle section, and rear section is transported to the brick press via belt conveyors. The mixture is then laid out sequentially at 260mm for the reaction section, 350mm for the middle section, and 350mm for the rear section. After being pressurized in two stages (30MPa for 7s and 150MPa for 10s), the mixture is heat-treated at 200℃ for 32 hours to obtain the magnesia-carbon bricks for quick-change at the converter bottom.

[0077] The magnesia-carbon bricks for quick-change converter bottoms prepared in this embodiment were tested and found that: after 5 heats, special steel smelting began; after 1000 heats, the bottom thickness increased significantly, affecting the converter bottom blowing effect.

[0078] Example 2 (Replacing the breathable brick)

[0079] A magnesia-carbon brick for quick replacement of converter hearth and its preparation method. This embodiment only replaces the permeable bricks of the converter hearth. The preparation method includes the following steps: Step 1 (Aggregate Preparation): Fused magnesia (5-50mm), sintered magnesia, forsterite, and calcium-containing magnesia are sequentially crushed and screened into 0.1-1mm, 1-3mm, and 3-5mm particles using a jaw crusher. To ensure material particle size distribution, some of the 1-3mm or 3-5mm particles can be further crushed into 0.1-1mm or 1-3mm particles using a double-roll crusher. The crushed particles are then stored in the corresponding silos according to their particle size.

[0080] 0.1-1mm particles are called small particles, 1-3mm particles are called medium particles, and 3-5mm particles are called large particles.

[0081] Step 2 (Preparation of matrix fine powder): After storing a sufficient amount of the particles in the silo, storage is stopped. Next, the particles obtained from the jaw crusher are directly fed into the Raymond mill, and after pulverization, matrix fine powder (electrominated magnesia fine powder, sintered magnesia fine powder, forsterite fine powder, calcium-containing magnesia fine powder) with a particle size of less than 0.088 mm is formed and stored in the corresponding silo.

[0082] In actual production, steps one and two can be carried out simultaneously to shorten the preparation time of aggregates and matrix.

[0083] Step 3 (mixing and molding): Using computer-controlled trolleys, the above-mentioned granules are transported from each silo to the planetary mixer, the fine powder to the Ericsson mixer, the mixed matrix fine powder is transported by belt to the planetary mixer, and the mixture is transported by belt to the brick press.

[0084] The converter bottom quick-change magnesia-carbon brick is a gradient refractory material with a total length of 860mm, divided into a reaction section (260±10mm), a middle section (350±10mm), and a rear section (350±10mm).

[0085] Reaction section: 3% fused magnesia fine powder, 3% sintered magnesia fine powder, 12% calcium-containing magnesia fine powder, and 8% magnesium olivine fine powder are transported to an Ericsson mixer and mixed for 3 minutes. During this period, 1% aluminum powder and 0.9% silicon powder additive are manually added from the Ericsson mixer feed port. After mixing evenly, the matrix fine powder of the reaction section is obtained. 1% of fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1), 4% of sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8), 30% of calcium-containing magnesia particles (large, medium, and small particle mass ratio of 1.1:2:0.9), and 25% of forsterite particles (1.05:2:0.95) were transported to a planetary mixer and mixed for 3 minutes. Then, 3.0% of phenolic resin binder was added and stirred for another 3 minutes. Next, 14% of low-carbon graphite fine powder was manually added and mixed for 4 minutes. Finally, the matrix fine powder of the reaction section was added and mixed for 3 minutes to obtain the reaction section mixture.

[0086] Intermediate Section: 14% fused magnesia fine powder and 7% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 4 minutes. During this time, 1.5% aluminum powder and 1.3% silicon powder additives are manually added through the Ericsson mixer feed port. After uniform mixing, the intermediate section matrix fine powder is obtained. 50% fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1) and 15% sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 4 minutes. Then, 3.5% phenolic resin binder is added and the mixture is stirred for another 4 minutes. Next, 11% high-purity graphite fine powder and 3% flake graphite particles (medium particles) are manually added and mixed for 4 minutes. Finally, the intermediate section matrix fine powder is added and mixed for 4 minutes to obtain the intermediate section mixture.

[0087] The downstream section: 6% fused magnesia fine powder and 10% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 3 minutes. During this time, 1.0% aluminum powder and 0.2% silicon powder additive are manually added through the Ericsson mixer feed port. After uniform mixing, the downstream matrix fine powder is obtained. 14% fused magnesia particles (large, medium and small particle mass ratio of 1:2:1) and 56% sintered magnesia particles (large, medium and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 3 minutes. Then, 3.1% phenolic resin binder is added and the mixture is stirred for 4 minutes. Next, 14% high-purity graphite fine powder is manually added and mixed for 4 minutes. Finally, the downstream matrix fine powder is added and mixed for 3 minutes to obtain the downstream mixture.

[0088] The mixture from the reaction section, middle section, and rear section is transported to the brick press via belt conveyors. The mixture is then laid out sequentially at 260mm for the reaction section, 350mm for the middle section, and 350mm for the rear section. After being pressurized in two stages (40MPa for 6 seconds and 150MPa for 5 seconds), it is heat-treated at 220℃ for 30 hours to obtain the magnesia-carbon bricks for quick-change at the converter bottom.

[0089] The magnesia-carbon bricks for quick-change converter bottoms prepared in this embodiment were tested and found to be suitable for smelting special steel after 5 heats; however, the permeable tube bricks were damaged and the surrounding refractory bricks were also damaged after 26 heats.

[0090] Example 3 (Replacing the permeable bricks and the surrounding 5 layers of refractory bricks)

[0091] A magnesia-carbon brick for quick replacement of converter hearth and its preparation method. This embodiment replaces the permeable bricks at the converter hearth and the surrounding five layers of refractory bricks. The preparation method includes the following steps: Step 1 (Aggregate Preparation): Fused magnesia (5-50mm), sintered magnesia, forsterite, and calcium-containing magnesia are sequentially crushed and screened into 0.1-1mm, 1-3mm, and 3-5mm particles using a jaw crusher. To ensure material particle size distribution, some of the 1-3mm or 3-5mm particles can be further crushed into 0.1-1mm or 1-3mm particles using a double-roll crusher. The crushed particles are then stored in the corresponding silos according to their particle size.

[0092] 0.1-1mm particles are called small particles, 1-3mm particles are called medium particles, and 3-5mm particles are called large particles.

[0093] Step 2 (Preparation of matrix fine powder): After storing a sufficient amount of the particles in the silo, storage is stopped. Next, the particles obtained from the jaw crusher are directly fed into the Raymond mill, and after pulverization, matrix fine powder (electrominated magnesia fine powder, sintered magnesia fine powder, forsterite fine powder, calcium-containing magnesia fine powder) with a particle size of less than 0.088 mm is formed and stored in the corresponding silo.

[0094] In actual production, steps one and two can be carried out simultaneously to shorten the preparation time of aggregates and matrix.

[0095] Step 3 (mixing and molding): Using computer-controlled trolleys, the above-mentioned granules are transported from each silo to the planetary mixer, the fine powder to the Ericsson mixer, the mixed matrix fine powder is transported by belt to the planetary mixer, and the mixture is transported by belt to the brick press.

[0096] The converter bottom quick-change magnesia-carbon brick is a gradient refractory material with a total length of 860mm, divided into a reaction section (260±10mm), a middle section (350±10mm), and a rear section (350±10mm).

[0097] Reaction section: 4% fused magnesia fine powder, 5% sintered magnesia fine powder, 12% calcium-containing magnesia fine powder, and 6% magnesium olivine fine powder are transported to an Ericsson mixer and mixed for 3 minutes. During this period, 0.5% aluminum powder and 0.5% silicon powder additives are manually added from the Ericsson mixer feed port. After mixing evenly, the matrix fine powder of the reaction section is obtained. 2% fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1), 5% sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8), 35% calcium-containing magnesia particles (large, medium, and small particle mass ratio of 1.1:2:0.9), and 15% forsterite particles (1.05:2:0.95) were transported to a planetary mixer and mixed for 3 minutes. Then, 3.4% phenolic resin binder was added and stirred for 4 minutes. Next, 16% low-carbon graphite fine powder was manually added and mixed for 5 minutes. Finally, the matrix fine powder of the reaction section was added and mixed for 4 minutes to obtain the reaction section mixture.

[0098] Intermediate Section: 9% fused magnesia fine powder and 7% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 5 minutes. During this time, 1.0% aluminum powder and 1.0% silicon powder additive are manually added through the Ericsson mixer feed port. After uniform mixing, the intermediate section matrix fine powder is obtained. 60% fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1) and 10% sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 5 minutes. Then, 4.0% phenolic resin binder is added and the mixture is stirred for another 5 minutes. Next, 11% high-purity graphite fine powder and 3% flake graphite particles (medium particles) are manually added and mixed for 5 minutes. Finally, the intermediate section matrix fine powder is added and mixed for 5 minutes to obtain the intermediate section mixture.

[0099] The downstream section: 4% fused magnesia fine powder and 18% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 4 minutes. During this time, 0.5% aluminum powder and 0.8% silicon powder additives are manually added through the Ericsson mixer feed port. After uniform mixing, the downstream matrix fine powder is obtained. 10% fused magnesia particles (large, medium and small particle mass ratio of 1:2:1) and 50% sintered magnesia particles (large, medium and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 4 minutes. Then, 3.1% phenolic resin binder is added and the mixture is stirred for 5 minutes. Next, 18% high-purity graphite fine powder is manually added and mixed for 5 minutes. Finally, the downstream matrix fine powder is added and mixed for 4 minutes to obtain the downstream mixture.

[0100] The mixture from the reaction section, middle section, and rear section is transported to the brick press via belt conveyors. The mixture is then laid out sequentially at 260mm for the reaction section, 350mm for the middle section, and 350mm for the rear section. After being pressurized by two pressure treatments of 50MPa for 5s and 200MPa for 5s, the mixture is heat-treated at 230℃ for 26 hours to obtain the magnesia-carbon bricks for quick replacement of the converter bottom.

[0101] The magnesia-carbon bricks for quick-change converter bottoms prepared in this embodiment were tested and found to be suitable for smelting special steel after 5 heats; the furnace lifespans were 8541 heats, 8695 heats, and 9021 heats. In the early stages, a slag-metal mushroom head structure could be formed, but occasional bottom-blowing blockage and reduced bottom-blowing gas flow occurred in the early stages.

[0102] Example 4 (Replace the 5 layers of refractory bricks around the permeable brick, but do not replace the permeable brick)

[0103] A magnesia-carbon brick for quick replacement of converter bottom and its preparation method. This embodiment replaces the five layers of refractory bricks surrounding the permeable bricks at the converter bottom, without replacing the permeable bricks themselves. The preparation method includes the following steps: Step 1 (Aggregate Preparation): Fused magnesia (5-50mm), sintered magnesia, forsterite, and calcium-containing magnesia are sequentially crushed and screened into 0.1-1mm, 1-3mm, and 3-5mm particles using a jaw crusher. To ensure material particle size distribution, some of the 1-3mm or 3-5mm particles can be further crushed into 0.1-1mm or 1-3mm particles using a double-roll crusher. The crushed particles are then stored in the corresponding silos according to their particle size.

[0104] 0.1-1mm particles are called small particles, 1-3mm particles are called medium particles, and 3-5mm particles are called large particles.

[0105] Step 2 (Preparation of matrix fine powder): After storing a sufficient amount of the particles in the silo, storage is stopped. Next, the particles obtained from the jaw crusher are directly fed into the Raymond mill, and after pulverization, matrix fine powder (electrominated magnesia fine powder, sintered magnesia fine powder, forsterite fine powder, calcium-containing magnesia fine powder) with a particle size of less than 0.088 mm is formed and stored in the corresponding silo.

[0106] In actual production, steps one and two can be carried out simultaneously to shorten the preparation time of aggregates and matrix.

[0107] Step 3 (mixing and molding): Using computer-controlled trolleys, the above-mentioned granules are transported from each silo to the planetary mixer, the fine powder to the Ericsson mixer, the mixed matrix fine powder is transported by belt to the planetary mixer, and the mixture is transported by belt to the brick press.

[0108] The converter bottom quick-change magnesia-carbon brick is a gradient refractory material with a total length of 860mm, divided into a reaction section (260±10mm), a middle section (350±10mm), and a rear section (350±10mm).

[0109] Reaction section: 3% fused magnesia fine powder, 4% sintered magnesia fine powder, 15% calcium-containing magnesia fine powder, and 8% magnesium olivine fine powder are transported to an Ericsson mixer and mixed for 5 minutes. During this period, 0.5% aluminum powder and 0.6% silicon powder additives are manually added from the Ericsson mixer feed port. After mixing evenly, the matrix fine powder of the reaction section is obtained. 1% of fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1), 4% of sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8), 30% of calcium-containing magnesia particles (large, medium, and small particle mass ratio of 1.1:2:0.9), and 20% of forsterite particles (1.05:2:0.95) were transported to a planetary mixer and mixed for 5 minutes. Then, 3.2% of phenolic resin binder was added and stirred for another 5 minutes. Next, 15% of low-carbon graphite fine powder was manually added and mixed for 5 minutes. Finally, the matrix fine powder of the reaction section was added and mixed for 5 minutes to obtain the reaction section mixture.

[0110] Intermediate Section: 20% of fused magnesia fine powder and 3% of sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 5 minutes. During this time, 1.2% of aluminum powder and 1.0% of silicon powder additives are manually added through the Ericsson mixer feed port. After uniform mixing, the intermediate section matrix fine powder is obtained. 50% of fused magnesia particles (large, medium, and small particle mass ratio of 1:2:1) and 11% of sintered magnesia particles (large, medium, and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 5 minutes. Then, 3.5% of phenolic resin binder is added and the mixture is stirred for another 5 minutes. Next, 13% of high-purity graphite fine powder and 3% of flake graphite particles (medium particles) are manually added and mixed for 5 minutes. Finally, the intermediate section matrix fine powder is added and mixed for 5 minutes to obtain the intermediate section mixture.

[0111] The downstream section: 5% fused magnesia fine powder and 18% sintered magnesia fine powder are transported to an Ericsson mixer and mixed for 5 minutes. During this time, 1.0% aluminum powder and 0.9% silicon powder additive are manually added through the Ericsson mixer feed port. After uniform mixing, the downstream matrix fine powder is obtained. 10% fused magnesia particles (large, medium and small particle mass ratio of 1:2:1) and 53% sintered magnesia particles (large, medium and small particle mass ratio of 1.2:2:0.8) are transported to a planetary mixer and mixed for 5 minutes. Then, 3.2% phenolic resin binder is added and mixed for another 5 minutes. Next, 14% high-purity graphite fine powder is manually added and mixed for 5 minutes. Finally, the downstream matrix fine powder is added and mixed for 5 minutes to obtain the downstream mixture.

[0112] The mixture from the reaction section, middle section, and rear section is transported to the brick press via belt conveyors. The mixture is then laid out sequentially at 260mm for the reaction section, 350mm for the middle section, and 350mm for the rear section. After being pressurized by two pressure tests at 50MPa for 10s and 200MPa for 10s, the mixture is heat-treated at 250℃ for 24 hours to obtain the magnesia-carbon bricks for quick-change at the converter bottom.

[0113] The magnesia-carbon bricks for quick-change converter bottom prepared in this embodiment were tested and found to be suitable for smelting special steel after 5 heats; the furnace life was 8368-9568 heats; no bottom thickening phenomenon was observed around 1000 heats; the slag-metal mushroom head structure was stable in the early stage; and the bottom blowing gas flow rate was stable.

[0114] The above description is only a specific embodiment of the present invention, but the structural features protected by the present invention are not limited thereto. Any changes or modifications made by those skilled in the art within the scope of the present invention are covered by the patent scope of the present invention.

Claims

1. A method for preparing magnesia-carbon bricks for quick-change converter hearths, characterized in that: Includes the following steps: Step 1: Aggregate Preparation: 5-50mm fused magnesia, sintered magnesia, forsterite, and calcium-containing magnesia are sequentially crushed and screened into 0.1-1mm, 1-3mm, and 3-5mm particles using a jaw crusher. To maintain material balance, 10-70% of the 1-3mm or 3-5mm particles are further crushed into 0.1-1mm or 1-3mm particles using a double-roll crusher. The crushed particles are then stored in the corresponding silos according to their particle size; 0.1-1mm particles are called small particles, 1-3mm particles are called medium particles, and 3-5mm particles are called large particles. Step 2: Preparation of matrix fine powder: After storing 5-12 tons of particles from Step 1 in the silo, storage is stopped. Then, the particles from the jaw crusher are directly fed into the Raymond mill. After pulverization, matrix fine powder with a particle size of less than 0.088mm is formed, namely fused magnesia fine powder, sintered magnesia fine powder, forsterite fine powder, and calcium-containing magnesia fine powder, and stored in the corresponding silos. In actual production, Step 1 and Step 2 are carried out simultaneously to shorten the aggregate and matrix preparation time. Step 3: Mixing and Molding: The transport trolleys transport the above-mentioned granules from each silo to the planetary mixer, the fine powder to the Ericsson mixer, the mixed matrix fine powder is transported by belt to the planetary mixer, and the mixture is transported by belt to the brick press; the magnesia-carbon bricks used for quick-change at the converter bottom are gradient refractory materials with a total length of 860±30mm, divided into a reaction section of 260±10mm, a middle section of 350±10mm and a rear section of 350±10mm; Reaction Section: 3-5% fused magnesia fine powder, 3-8% sintered magnesia fine powder, 10-15% calcium-containing magnesia fine powder, and 4-8% forsterite fine powder are transported to an Ericsson mixer and mixed for 3-5 minutes. During this time, 0.1-1% aluminum powder and 0.2-0.9% silica powder additives are manually added through the Ericsson mixer feed port. After uniform mixing, the matrix fine powder for the reaction section is obtained. 1-3% fused magnesia particles with a large, medium, and small particle size ratio of 1:2:1 and 4-7% large, medium, and small particle size ratio of 1.2:2:0.8 are then added. Sintered magnesia particles, 30-45% calcium-containing magnesia particles with a large, medium, and small particle mass ratio of 1.1:2:0.9, and 15-25% forsterite particles with a large, medium, and small particle mass ratio of 1.05:2:0.95 are transported to a planetary mixer and mixed for 3-5 minutes. Then, 3.0-3.6% phenolic resin binder is added and stirred for another 3-5 minutes. Next, 14-18% low-carbon graphite fine powder is manually added and mixed for 4-5 minutes. Finally, the matrix fine powder of the reaction section is added and mixed for 3-5 minutes to obtain the reaction section mixture. Mid-section: 6-20% of fused magnesia fine powder and 3-7% of sintered magnesia fine powder are transported to an Ellis mixer and mixed for 3-5 minutes. During this time, 0.5-1.5% of aluminum powder and 0.4-1.3% of silicon powder additive are manually added through the Ellis mixer feed port. After uniform mixing, the mid-section matrix fine powder is obtained. 50-60% of fused magnesia particles with a large, medium, and small particle size ratio of 1:2:1 and 10-15% of sintered magnesia particles with a large, medium, and small particle size ratio of 1.2:2:0.8 are transported to a planetary mixer. Mix for 3-5 minutes, then add 3.5-4.0% phenolic resin binder and stir for another 3-5 minutes. Next, manually add 11-13% high-purity graphite fine powder and 3-5% flake graphite particles and mix for 4-5 minutes. Finally, add the aforementioned intermediate matrix fine powder and mix for 3-5 minutes to obtain the intermediate mixture. For the final stage: transport 3-9% fused magnesia fine powder and 10-18% sintered magnesia fine powder to an Ericsson mixer and mix for 3-5 minutes. During this time, manually add 0% phenolic resin binder through the Ericsson mixer's feed port. 0.1-1.0% aluminum powder and 0.2-0.9% silicon powder additive are mixed evenly to obtain the downstream matrix fine powder; 10-15% of fused magnesia particles with a large, medium, and small particle size ratio of 1:2:1 and 50-60% of sintered magnesia particles with a large, medium, and small particle size ratio of 1.2:2:0.8 are transported to a planetary mixer and mixed for 3-5 minutes, then 3.0-3.2% phenolic resin binder is added and stirred for another 3-5 minutes, and finally 14-18% high-purity graphite fine powder is manually added and mixed for 4-5 minutes. Finally, the fine powder of the downstream matrix is ​​added and mixed for 3-5 minutes to obtain the downstream mixture. The mixtures of the reaction section, the middle section, and the rear section are transported to the brick press by belt conveyor. The bricks are distributed in sequence according to the following thicknesses: reaction section 260±5mm, middle section 350±5mm, and rear section 350±5mm. After being pressurized by two stages of pressure treatment (30-50MPa for 5-10s and 150-200MPa for 5-10s), the bricks are heat-treated at 200-250℃ for 24-32 hours to obtain the magnesia-carbon bricks for quick replacement of the converter bottom. The fused magnesia contains ≥97% MgO, ≤0.6% SiO2, ≤1.5% CaO, and ≤0.01% B2O3, with a particle size of 5-50 mm and a bulk density of 3.45-3.53 g / cm³. 3 The sintered magnesia has a true porosity of 0.5-2.5% and a grain size of 270-700 μm; the sintered magnesia contains ≥95% MgO, ≤2.2% SiO2, ≤1.8% CaO, has a particle size of 5-50 mm, and a bulk density of 3.20-3.47 g / cm³. 3 The true porosity is 0.3-3.5%, and the grain size is 10-200 μm; the forsterite has MgO+SiO2≥95%, SiO2≥40%, CaO≤1.0%, Al2O3≤1.0%, a particle size of 5-50 mm, and a bulk density of 3.22-3.33 g / cm³. 3 The calcium-magnesium sand contains ≥90% MgO, 5-10% CaO, ∑SiO2+Al2O3+Fe2O3≤3.0%, has a particle size of 5-50mm, and a bulk density of 3.42-3.47g / cm³. 3 .

2. The method for preparing magnesia-carbon bricks for quick-change converter hearths according to claim 1, characterized in that: The jaw crusher has a production capacity of 250-350 t / h, a finished product size of 0-5 mm, and a maximum feed size of 700 mm; the double roll crusher has a production capacity of 50-100 t / h, a finished product size of 0-3 mm, and a maximum feed size of 60 mm; the Raymond mill has a production capacity of 10-320 t / d, a finished product size of 0.015-0.088 mm, and a maximum feed size of 30 mm; the Ericsson mixer is model RV24, with a speed of 0-1751 r / min; and the planetary mixer has a capacity of 800-1200 kg and is equipped with a heating function.

3. The method for preparing magnesia-carbon bricks for quick-change converter hearths according to claim 1, characterized in that: The aluminum powder contains Al≥98%, Fe≤0.5%, Si≤0.5%, Cu≤0.1%, and has a particle size of 0.015-0.074mm; the silicon powder contains Si≥98% and has a particle size of 0.015-0.074mm.

4. The method for preparing magnesia-carbon bricks for quick-change converter hearths according to claim 1, characterized in that: The phenolic resin is liquid with a viscosity of 0.75-0.95 Pa·s at 25°C, a water content of 1.5-2.5%, a solid content of 75-80%, a residual carbon rate of 43-48%, a free phenol content of 10.0-12.0%, and a pH value of 6.5-7.

5.

5. The method for preparing magnesia-carbon bricks for quick-change converter hearths according to claim 1, characterized in that: The low-carbon graphite powder has 50-80% fixed carbon; the main ash components are SiO2, Al2O3 and Fe2O3, with ∑SiO2+Al2O3+Fe2O3 in the ash being 82.9-88.6%, of which SiO2 accounts for 33-59%, and the particle size is 0.044-0.074 mm.

6. The method for preparing magnesia-carbon bricks for quick-change converter hearths according to claim 1, characterized in that: The high-purity graphite powder has a fixed carbon content of ≥99.9% and a particle size of 0.074-0.1 mm.

7. The method for preparing magnesia-carbon bricks for quick-change converter hearths according to claim 1, characterized in that: The flake graphite contains ≥99.9% fixed carbon particles with a particle size of 1-3 mm.

8. The method for preparing magnesia-carbon bricks for quick-change converter hearths according to claim 1, characterized in that: The brick press is a friction brick press.

9. A magnesia-carbon brick for quick-replacement of converter hearth, characterized in that: The magnesia-carbon brick for quick-change of converter bottom is prepared by the method for preparing magnesia-carbon brick for quick-change of converter bottom according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for replacing converter bottom blowing seat brick

    CN110184412A

  • Low-carbon magnesia carbon brick for producing stainless steel by converter and preparation process of low-carbon magnesia carbon brick

    CN117069480A

  • Preparation process of magnesia carbon brick for tapping hole of converter

    CN117430407A

  • Dry type magnesium-calcium gravity flow fire-resistant material and preparation thereof

    CN101462887A

  • Composite converter magnesia-carbon brick and preparation method thereof

    CN110423125A