Ammonia oxidation catalyst, method for preparing the same, and use thereof, and method for preparing acrylonitrile

CN119972107BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311509064.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-13
Publication Date
2026-11-24
Estimated Expiration
2043-11-13

AI Technical Summary

Technical Problem

[0008]本发明的目的是为了克服现有技术存在的用于氨氧化反应的催化剂在高负荷条件下,目标产物收率低的问题,提供一种氨氧化催化剂及其制备方法与应用以及丙烯腈的制备方法

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119972107B_ABST
    Figure CN119972107B_ABST
Patent Text Reader

Abstract

This invention relates to the field of catalysts, and discloses an ammonia oxidation catalyst, its preparation method and application, as well as a method for preparing acrylonitrile. The catalyst comprises an active component and a support, and the active component has the following general formula: Fe d Bi e Mo f A a B b C c O x The values ​​of a range from 0 to 1, b from 0 to 12.5, c from 0 to 3, d from 0.1 to 4, e from 0.01 to 3, and f from 9 to 16. x represents the total number of oxygen atoms required to satisfy the oxidation states of each element in the above active components. The catalyst comprises microspheres with a partially hollow structure, and the hollowness of the catalyst is 10-30%. This catalyst not only exhibits high propylene ammoxidation activity and acrylonitrile selectivity in the propylene ammoxidation reaction, but also achieves a high single-pass yield of acrylonitrile under high loading conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalysts, specifically to an ammonia oxidation catalyst with a hollow structure, its preparation method and application, and a method for preparing acrylonitrile. Background Technology

[0002] Acrylonitrile, an important organic chemical raw material, is a crucial monomer for synthesizing synthetic materials such as acrylic fibers, ABS, SAN, and carbon fibers. It can also be used as an intermediate in the preparation of chemicals such as adiponitrile and acrylamide. Currently, fluidized bed ammoxidation is the most common production process, with catalysts being one of the core technologies of this process, and research and improvement of these catalysts have been ongoing. Developing acrylonitrile synthesis catalysts capable of handling high catalyst loadings, i.e., increasing the number of tons of propylene processed per ton of catalyst per hour, is a significant trend in acrylonitrile catalyst development. However, with increased catalyst loading, the reactor feed rate increases, and the corresponding contact time between the catalyst and the raw material shortens, placing higher demands on the catalytic performance of the catalyst itself. Existing catalysts, due to their limited utilization of their active components, cannot fully adapt to the requirements of high loading conditions, and are prone to problems such as low acrylonitrile yield and poor stability when used under high loading conditions.

[0003] To ensure good fluidization performance, acrylonitrile catalysts used in fluidized bed processes are typically spherical with a specific size distribution, averaging around 50 μm in diameter. Under high load conditions, due to the short contact time between the catalyst and the feedstock, the internal regions of the catalyst particles are affected by the mass transfer and diffusion rate, making effective contact with the feedstock difficult. The most readily available active components are concentrated in the outer regions of the catalyst particles, resulting in a lower utilization rate of the active components at lower loads. Consequently, the catalyst activity decreases significantly under high load conditions.

[0004] CN111744493A discloses an acrylonitrile catalyst that can improve the stability of the catalyst during long-term operation by controlling the relative magnitudes of the Mo / Bi molar ratio on the catalyst particle surface and the bulk Mo / Bi molar ratio. However, the loading used in the catalyst evaluation is relatively low.

[0005] CN107282063B, CN107282060B, CN107282065B, and CN107282094B disclose that adding a certain amount of zirconium oxide, titanium oxide, diatomaceous earth, and ZSM-5 molecular sieve as a support modifier during catalyst preparation can improve the selectivity and stability of the catalyst in the propylene ammoxidation reaction. However, the catalyst evaluation was also carried out under low loading conditions.

[0006] The above methods show that although controlling the spatial distribution of elements in the catalyst or adding appropriate support modifiers can improve the performance of the catalyst to a certain extent, they still cannot solve the problems of low acrylonitrile yield and poor stability of current propylene ammoxidation catalysts under high load conditions.

[0007] Obtaining catalysts that simultaneously possess good selectivity, high conversion rate, high single-pass yield, and good stability under high loads has always been an important research direction in the field of ammonia oxidation catalysts. Summary of the Invention

[0008] The purpose of this invention is to overcome the problem of low yield of target product in existing catalysts for ammonia oxidation under high loading conditions, and to provide an ammonia oxidation catalyst, its preparation method and application, as well as a method for preparing acrylonitrile. This catalyst not only exhibits high ammonia oxidation activity and acrylonitrile selectivity in the propylene ammonia oxidation reaction, but also achieves a high single-pass yield of acrylonitrile under high loading conditions.

[0009] A first aspect of the present invention provides an ammonia oxidation catalyst, wherein the catalyst comprises an active component and a support, the active component having the following general formula Fe d Bi e Mo f A a B b C c O x ;

[0010] Wherein, A is at least one of the alkali metal elements, B is at least one of the alkaline earth metal elements, transition metal elements, group IIIA metal elements, antimony and tellurium, and C is a rare earth element.

[0011] The value of a ranges from 0 to 1, the value of b ranges from 0 to 12.5, the value of c ranges from 0 to 3, the value of d ranges from 0.1 to 4, the value of e ranges from 0.01 to 3, the value of f ranges from 9 to 16, and x is the total number of oxygen atoms required to satisfy the oxidation states of each element in the above active components.

[0012] The catalyst includes microspheres with partially hollow structures, and the hollowness of the catalyst is 10-30%. The hollowness refers to the percentage of microspheres with hollow structures in the catalyst microspheres out of the total number of catalyst microspheres. Microspheres with hollow structures refer to catalyst particles whose maximum diameter of the hollow structure exceeds 25% of the maximum diameter of the catalyst particles.

[0013] A second aspect of this invention provides a method for preparing an ammonia oxidation catalyst, the method comprising the following steps:

[0014] (a) Provide a solution I containing the Mo precursor;

[0015] (b) Provide a solution containing Fe precursor, Bi precursor, optional A precursor, optional B precursor, optional C precursor and polycarboxylic acid, and then age it to obtain solution II;

[0016] (c) Mix the solution I obtained in step (a), fumed silica and optionally a solvent to obtain slurry I;

[0017] (d) Mix the slurry I obtained in step (c) with the silica precursor to obtain slurry II;

[0018] (e) Mix the slurry II obtained in step (d) and the solution II obtained in step (b) to obtain slurry III;

[0019] (f) Boil the slurry III obtained in step (e);

[0020] (g) The slurry obtained in step (f) is dried and calcined;

[0021] Wherein, A is at least one of the alkali metal elements, B is at least one of the alkaline earth metal elements, transition metal elements, Group IIIA metal elements, antimony and tellurium, and C is a rare earth element.

[0022] A third aspect of the present invention provides a catalyst prepared by the method described in the second aspect.

[0023] The fourth aspect of the present invention provides the application of the catalyst described in the first or third aspect in an ammonia oxidation reaction, preferably in an olefin ammonia oxidation reaction, and more preferably in the ammonia oxidation of propylene to prepare acrylonitrile.

[0024] The fifth aspect of the present invention provides a method for preparing acrylonitrile, the method comprising: reacting propylene, an ammonia source and an oxygen source in the presence of the catalyst described in the first or third aspect.

[0025] The inventors of this invention discovered during their research that by optimizing the catalyst composition, adding polycarboxylic acids as pore-forming agents, and using fumed silica and silica precursors in the preparation process, the resulting catalyst exhibits a partially hollow spherical structure with a spherical hollow structure. The active components in the catalyst are more concentrated in the outer region of the catalyst particles, which improves the effective utilization rate of the active components. When the hollowness is 10-30%, the catalytic performance under high-load conditions can be effectively improved, and the catalyst has good stability, maintaining a high single-pass yield of acrylonitrile for a long time, thereby significantly improving the efficiency and economy of acrylonitrile production. Specifically, compared with the prior art, this invention has the following advantages:

[0026] (1) The catalyst of the present invention includes microspheres with a partially hollow sphere structure and a hollowness of 10-30%. The active components in the catalyst are more concentrated in the outer region of the catalyst particles, which can improve the effective utilization rate of the active components of the catalyst.

[0027] (2) The catalyst has good stability and can maintain a high single-pass yield of acrylonitrile for a long time, thereby greatly improving the efficiency and economy of acrylonitrile production.

[0028] (3) The propylene conversion rate can reach more than 99%, and the acrylonitrile single-pass yield can reach more than 84%. Attached Figure Description

[0029] Figure 1 It is a 2D planar image of the catalyst along the Z-axis. Detailed Implementation

[0030] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0031] A first aspect of the present invention provides an ammonia oxidation catalyst, wherein the catalyst comprises an active component and a support, the active component having the following general formula Fe d Bi e Mo f A a B b C c O x ;

[0032] Wherein, A is at least one of the alkali metal elements, B is at least one of the alkaline earth metal elements, transition metal elements, group IIIA metal elements, antimony and tellurium, and C is a rare earth element.

[0033] The value of a ranges from 0 to 1, the value of b ranges from 0 to 12.5, the value of c ranges from 0 to 3, the value of d ranges from 0.1 to 4, the value of e ranges from 0.01 to 3, the value of f ranges from 9 to 16, and x is the total number of oxygen atoms required to satisfy the oxidation states of each element in the above active components.

[0034] The catalyst includes microspheres with partially hollow structures, and the hollowness of the catalyst is 10-30%. The hollowness refers to the percentage of microspheres with hollow structures in the catalyst microspheres out of the total number of catalyst microspheres. Microspheres with hollow structures refer to catalyst particles whose maximum diameter of the hollow structure exceeds 25% of the maximum diameter of the catalyst particles.

[0035] In this invention, the hollow structure is spherical or near-spherical.

[0036] In this invention, the hollowness rate refers to the percentage of catalyst microspheres with hollow structures out of the total number of catalyst microspheres. Specifically, the hollowness rate (%) = number of catalyst particles with hollow structures / total number of catalyst particles counted × 100%. In this invention, the hollowness rate is obtained by counting more than 200 (preferably not less than 250) intact catalyst particles.

[0037] In this invention, the maximum diameter of the hollow structure of the catalyst particles exceeds 25% of the maximum diameter of the catalyst particles, and is defined as a microsphere with a hollow structure. The hollowness of the catalyst can be determined by micron-level X-ray computed tomography using a Zeiss Xraida 400Versa 3D X-ray microscope. The catalyst sample is packed into a sample tube with a diameter of 1 mm and a length of approximately 1 cm, and vertically placed in the micron-level CT scanner. The single-image exposure time is set to 5 s, the scanning voltage to 60 kV, and the test temperature to 20 °C. 2D planar images (approximately 2048 images) along the Z-axis are obtained and used to statistically analyze the hollowness of the catalyst. A typical 2D planar image is shown below. Figure 1 As shown, the high-contrast region represents the active components and support contained in the catalyst, while the low-contrast region represents the gaps between catalyst particles or cavities in the catalyst particles.

[0038] According to a preferred embodiment of the invention, the hollowness of the catalyst is 10-22.5%, for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21% or 22.5%.

[0039] The catalyst has a partially hollow spherical structure, which allows the active components to be concentrated in the outer region of the catalyst particles, thus improving the effective utilization rate of the active components and significantly increasing the efficiency and economy of acrylonitrile production.

[0040] It should be noted that in this invention, "Fe" d Bi e Mo f A a B b C c Ox The general formula "" only represents the individual elements and their molar content of the active component in the catalyst, and does not mean that the active component of the catalyst in this invention exists as a molecule of this general formula.

[0041] According to a preferred embodiment of the present invention, the alkali metal element is selected from at least one of Na, K, Rb and Cs.

[0042] According to a preferred embodiment of the present invention, the alkaline earth metal element is selected from at least one of Mg, Ca, Ba and Sr.

[0043] According to a preferred embodiment of the present invention, the transition metal element is selected from at least one of Mn, Co, Ni, Zn, Cr, Zr, Ti, Nb, and W, preferably at least one of Ni, Co, and Mn, more preferably at least two of Ni, Co, and Mn, and most preferably Ni, Co, and Mn. When two or three of Ni, Co, and Mn are combined, the present invention does not particularly limit their proportions. For example, the molar ratio of Ni, Co, and Mn is 1:0.1-2.5:0.1-2.5.

[0044] According to a preferred embodiment of the present invention, the Group IIIA metal element is selected from at least one of Al, Ga and In.

[0045] According to a preferred embodiment of the present invention, the rare earth element is selected from at least one of Ce, Pr, Nd and Sm.

[0046] Using the above-mentioned active components in combination is more conducive to further improving the ammonia oxidation reaction performance of the catalyst.

[0047] In this invention, components A, B, and C may be included or excluded, but inclusion is preferred. When included, the range of their content can be wide.

[0048] According to a preferred embodiment of the present invention, the value of 'a' ranges from 0.05 to 0.5 (e.g., 0.05, 0.1, 0.3, 0.4, or 0.5), the value of 'b' ranges from 1 to 10 (e.g., 1, 2, 4, 5, 7, 8, 9, or 10), and the value of 'c' ranges from 0.01 to 2 (e.g., 0.01, 0.03, 0.05, 0.06, 0.07, 0.1, 0.2, 0.5). 1, 1.5, or 2), where d ranges from 0.5 to 4 (e.g., 0.5, 1, 1.5, 2, 2.5, 3, 4), e ranges from 0.01 to 1.5 (e.g., 0.01, 0.03, 0.05, 0.06, 0.07, 0.1, 0.2, 0.5, 1, or 1.5), and f ranges from 10 to 15 (e.g., 10, 11, 12, 13, 14, or 15). Using the aforementioned embodiments, the catalytic performance of the catalyst in the ammonia oxidation reaction can be better increased.

[0049] Preferably, e / f is 0.005-0.5, more preferably 0.01-0.25 (e.g. 0.01, 0.03, 0.05, 0.06, 0.07, 0.1, 0.2 or 0.25).

[0050] Preferably, d / f is 0.02-1.25, more preferably 0.1-1 (e.g. 0.1, 0.3, 0.5, 0.6, 0.7, 0.8, 0.9 or 1).

[0051] Using a specific e / f or d / f ratio is more conducive to improving the catalytic performance of the catalyst in the ammonia oxidation reaction.

[0052] According to a preferred embodiment of the present invention, the carrier is silicon dioxide.

[0053] According to the present invention, preferably, the content of the support is 30-70 wt% based on the total amount of catalyst, and the content of the active component, calculated as oxide, is 30-70 wt%; more preferably, the content of the support is 40-60 wt% based on the total amount of catalyst, and the content of the active component, calculated as oxide, is 40-60 wt%. Using the foregoing embodiments, the activity of the catalyst can be better improved.

[0054] According to the present invention, preferably, the specific surface area of ​​the catalyst is 30-45 m². 2 / g, preferably 35-45m 2 / g, further preferably 38-45m 2 / g, with an average pore size of 6-15nm, preferably 9-15nm.

[0055] A second aspect of this invention provides a method for preparing an ammonia oxidation catalyst, the method comprising the following steps:

[0056] (a) Provide a solution I containing the Mo precursor;

[0057] (b) Provide a solution containing Fe precursor, Bi precursor, optional A precursor, optional B precursor, optional C precursor and polycarboxylic acid, and then age it to obtain solution II;

[0058] (c) Mix the solution I obtained in step (a), fumed silica and optionally a solvent to obtain slurry I;

[0059] (d) Mix the slurry I obtained in step (c) with the silica precursor to obtain slurry II;

[0060] (e) Mix the slurry II obtained in step (d) and the solution II obtained in step (b) to obtain slurry III;

[0061] (f) Boil the slurry III obtained in step (e);

[0062] (g) The slurry obtained in step (f) is dried and calcined;

[0063] Wherein, A is at least one of the alkali metal elements, B is at least one of the alkaline earth metal elements, transition metal elements, Group IIIA metal elements, antimony and tellurium, and C is a rare earth element.

[0064] According to a preferred embodiment of the present invention, the average particle size of the fumed silica is 5-30 nm, preferably 5-15 nm, and the specific surface area is 200-500 m². 2 / g, preferably 300-450m 2 / g. Using fumed silica with the above characteristics is more conducive to improving the ammonia oxidation reaction performance of the prepared catalyst. The average particle size of the fumed silica can be obtained by measuring a nano-potential analyzer, and the specific surface area can be obtained by measuring the BET method.

[0065] The present invention does not have any particular limitation on the source of the fumed silica, which can be prepared by existing methods or obtained commercially.

[0066] Preferably, the silica precursor is selected from at least one of silica sol, water glass, inorganic silica gel and silicate ester, and more preferably silica sol.

[0067] According to the present invention, preferably, the solid content of the silica sol is 20-50 wt% based on silicon dioxide.

[0068] According to the present invention, preferably, the mass ratio of the fumed silica to the silica precursor, based on silica, is 1:1-1:20, more preferably 1:2-20, for example 1:2, 1:3, 1:2, 1:3, 1:4, 1:6, 1:8, 1:10, 1:10, 1:12, 1:14, 1:16, 1:18 or 1:20, more preferably 1:2-5.

[0069] The catalyst of this invention is prepared by using fumed silica and a silica precursor, resulting in a partially hollow spherical structure. When the mass ratio of silicon in the fumed silica to that in the silica precursor is 1:1-1:20, preferably 1:2-20, it facilitates the formation of a uniformly dispersed slurry. The fumed silica has a smaller average particle size and a higher specific surface area, which can increase the specific surface area of ​​the catalyst to a certain extent. Furthermore, the thixotropic and reinforcing properties of fumed silica contribute to the stable formation of the hollow structure of the catalyst, thereby improving the catalytic performance and stability of the catalyst under high-load conditions.

[0070] According to the method provided by the present invention, the selection range of each metal active component can be the same as the selection range described in the first aspect above, and the present invention will not repeat it here.

[0071] According to one specific embodiment of the present invention, the precursors of Fe, Bi, Mo, A, B, and C can be soluble compounds of the corresponding elements. The specific types of precursors are not particularly limited, as long as they can be converted into oxides of the corresponding components through subsequent calcination.

[0072] According to a preferred embodiment of the present invention, the molar ratio of Fe, Bi, Mo, A, B, and C is 0.1-4:0.01-3:9-16:0-1:0-12.5:0-3, preferably 0.5-3:0.01-1.5:10-15:0.05-0.5:1-10:0.01-2.

[0073] According to the present invention, preferably, the molar ratio of Bi to Mo is 0.005-0.5, more preferably 0.01-0.25.

[0074] According to the present invention, preferably, the molar ratio of Fe to Mo is 0.02-1.25, more preferably 0.1-1.

[0075] According to a preferred embodiment of the present invention, the amounts of Fe precursor, Bi precursor, optional A element precursor, optional B element precursor, optional C element precursor, fumed silica, and silica precursor are such that, based on the total amount of catalyst, the content of Fe, Bi, Mo, A, B, and C, calculated as oxides, is 30-70 wt%, preferably 40-60 wt%, and the content of silica is 30-70 wt%, preferably 40-60 wt%.

[0076] The present invention does not impose any particular limitation on the way the solution is provided in the method provided, and has a wide range of choices for the type of solvent and the concentration of the solution, as long as a mixing environment can be provided. The preferred solvent is water.

[0077] The present invention does not particularly limit the method of providing solution II in step (b). The Fe precursor, Bi precursor, optionally an A element precursor, optionally an B element precursor, optionally an C element precursor, and the polycarboxylic acid can be added to the solvent sequentially or simultaneously for mixing and contact. Alternatively, a portion of the precursor or polycarboxylic acid can be mixed uniformly with the solvent first, and then mixed with the remaining precursor. Preferably, the polycarboxylic acid is added after the Fe precursor, Bi precursor, optionally an A element precursor, optionally an B element precursor, and optionally an C element precursor are mixed. To achieve more uniform mixing, mixing can be carried out under heating and / or stirring conditions, for example, heating and stirring at a temperature of 40-120°C and a stirring speed of 100-500 rpm for 10-30 minutes.

[0078] According to a preferred embodiment of the present invention, in step (b), the polycarboxylic acid is selected from at least one of citric acid, oxalic acid, tartaric acid, and ethylenediaminetetraacetic acid, preferably citric acid.

[0079] According to a preferred embodiment of the present invention, the molar ratio of the amount of the added polycarboxylic acid to the total molar number of Fe, Bi, and Mo is 0.01-0.5:1, for example, 0.01, 0.03, 0.05, 0.06, 0.07, 0.1, 0.2, or 0.5, preferably 0.1-0.3:1.

[0080] According to a preferred embodiment of the present invention, the aging conditions include: a temperature of 40-80°C and a time of 0.1-0.5 h. Preferably, the aging is carried out under stirring conditions, and preferably the stirring speed is 200-1000 rpm.

[0081] In this invention, polycarboxylic acids are used as pore-forming agents, which can generate gas during the calcination process, making it easier for the catalyst to form a hollow structure. Furthermore, the porosity of the catalyst can be further adjusted by selecting appropriate types and amounts of polycarboxylic acids.

[0082] The mixing in step (c) of this invention may or may not involve the addition of a solvent. This invention does not have any particular limitation on this, but water is preferred as the solvent.

[0083] According to a preferred embodiment of the present invention, the mixing in step (d) is carried out under stirring conditions. The present invention does not particularly limit the stirring speed, but rather aims to achieve a more uniform mixing speed.

[0084] According to a preferred embodiment of the present invention, in step (f), the conditions for boiling the slurry include: a temperature of 80-175°C, a time of 0.1-3 hours, and a stirring speed of 200-1000 rpm. This preferred embodiment is more conducive to achieving uniform dispersion of fumed silica in the slurry and makes it easier to form a uniform hollow structure.

[0085] Preferably, in step (g), the drying method is spray drying. This invention offers a wide range of spray drying conditions. Preferably, the spray drying conditions include: a drying temperature of 250-400℃, a drying time of 0.5-3 hours, and an average droplet diameter of 40-200 μm.

[0086] Preferably, in step (g), the calcination conditions include: calcination temperature of 200-750℃ and calcination time of 1-8h under an oxygen-containing atmosphere; more preferably, the calcination temperature is 400-650℃ and the calcination time is 1-6h.

[0087] A third aspect of the present invention provides a catalyst prepared by the method described in the second aspect.

[0088] A fourth aspect of this invention provides the application of the catalyst described in the first or third aspect in an ammoxidation reaction, preferably in the ammoxidation reaction of olefins, and more preferably in the ammoxidation of propylene to acrylonitrile. Using the catalyst of this invention in the ammoxidation reaction of olefins, not only does it exhibit good catalytic activity, but it also maintains a high single-pass yield of nitrile compounds even after prolonged operation.

[0089] The fifth aspect of the present invention provides a method for preparing acrylonitrile, the method comprising: reacting propylene, an ammonia source and an oxygen source in the presence of the catalyst described in the first or third aspect.

[0090] Preferably, the conditions for the contact reaction include: a molar ratio of propylene:ammonia source:oxygen source of 1:1-1.5:8-10.5, preferably 1:1-1.3:8.8-10; and / or a reaction temperature of 400-470℃, preferably 410-450℃; and / or a reaction pressure (gauge pressure) of 0.03-0.15 MPa, preferably 0.06-0.14 MPa; and / or a reaction load (WWH) of 0.045-0.15 h. -1 The preferred concentration is 0.06-0.12h. -1 .

[0091] The present invention will be described in detail below through embodiments. In the following embodiments and comparative examples:

[0092] Specific surface area and pore size were measured using a TriStar II physical adsorption instrument. Before testing, samples underwent heating and vacuum degassing. Porosity was determined at 77 K, and specific surface area was calculated using the Brunauer-Emmett-Teller (BET) method. The pore size distribution and pore volume were calculated from the isothermal adsorption branch using the Barrettner-Joyner-Halenda (BJH) model.

[0093] The definition and testing method of hollowness rate have been described above and will not be repeated here.

[0094] The catalyst activity was evaluated in a fluidized bed reactor with an inner diameter of 38 mm. The catalyst loading was 400 g, the reaction temperature was 430 °C, the molar ratio of propylene:ammonia:air was 1:1.25:9.7, the reaction pressure (gauge pressure) was 0.085 MPa, and the reaction load (WWH) was 0.095 h⁻¹. -1 .

[0095] The conversion rate of propylene, the selectivity of acrylonitrile, and the single-pass yield are used as indicators to evaluate catalyst performance, and their definitions are as follows:

[0096] Propylene conversion rate (%) = (moles of propylene consumed in the reaction / moles of propylene fed) × 100%

[0097] Acrylonitrile selectivity (%) = (moles of acrylonitrile produced / moles of propylene consumed in the reaction) × 100%

[0098] Acrylonitrile single-pass yield (%) = (moles of acrylonitrile produced / moles of propylene fed) × 100%

[0099] Example 1

[0100] 860.7 grams of (NH4)6Mo7O 24Dissolve 4H₂O in 1000 mL of water to obtain mixed solution I. Dissolve 173.9 g of Bi(NO₃)₃·5H₂O, 469.1 g of Ni(NO₃)₂·6H₂O, 104.3 g of Co(NO₃)₂·6H₂O, 434.4 g of Fe(NO₃)₃·9H₂O, 42.3 g of Ca(NO₃)₂·4H₂O, 6.0 g of KOH, 93.4 g of Ce(NO₃)₃·6H₂O, and 128.29 g of 50% Mn(NO₃)₂ aqueous solution in 200 mL of water, and add 81.9 g of citric acid. The molar ratio of citric acid to the total moles of Mo, Bi, and Fe is 0.2:1. Age the solution at 60 °C and 400 rpm for 0.25 h to obtain mixed solution II. Then, 270 g of particles with an average particle size of 7 nm and a specific surface area of ​​380 m² / g are used. 2 / g of fumed silica and 800g of water are added to mixed solution I to obtain slurry I.

[0101] 1575 g of silica sol with a mass concentration of 40 wt% was added to slurry I under stirring conditions to obtain slurry II. Slurry II and mixed solution II were then mixed to obtain slurry III, which was stirred and boiled at 300 rpm for 0.75 h at 160 °C. Following this, spray drying was performed at 325 °C for 1 h, resulting in an average droplet diameter of 120 μm, yielding particulate matter. Finally, the obtained particulate matter was calcined at 580 °C for 1 h in an oxygen-containing atmosphere (oxygen volume fraction 21%) to obtain the catalyst.

[0102] Example 2

[0103] The catalyst preparation steps are the same as in Example 1, except that...

[0104] The raw material is 957.3 grams of (NH4)6Mo7O 24 ·4H2O, 193.4 g Bi(NO3)3·5H2O, 521.8 g Ni(NO3)2·6H2O, 94.2 g Ca(NO3)2·4H2O, 116.0 g Co(NO3)2·6H2O, 483.2 g Fe(NO3)3·9H2O, 6.7 g KOH, 103.9 g Ce(NO3)3·6H2O;

[0105] The molar ratio of citric acid to the total moles of Mo, Bi, and Fe was changed to 0.15:1;

[0106] Add 240 grams of particles with an average particle size of 7 nm and a specific surface area of ​​380 m². 2 / g of fumed silica and 700g of water are added to mixed solution I to obtain slurry I;

[0107] Add 1400g of silica sol with a mass concentration of 40wt% to slurry I to obtain slurry II.

[0108] Example 3

[0109] The catalyst preparation steps are the same as in Example 1, except that...

[0110] The added fumed silica has an average particle size of 15 nm and a specific surface area of ​​340 m². 2 / g.

[0111] Example 4

[0112] The catalyst preparation steps are the same as in Example 1, except that...

[0113] The raw material is 762.2 grams of (NH4)6Mo7O 24 ·4H2O, 231.0 g Bi(NO3)3·5H2O, 419.7 g Ni(NO3)2·6H2O, 138.6 g Co(NO3)2·6H2O, 259.1 g Fe(NO3)3·9H2O, 122.1 g Mg(NO3)2·6H2O, 9.23 g CsNO3, 103.4 g Ce(NO3)3·6H2O.

[0114] Example 5

[0115] The catalyst preparation steps are the same as in Example 1, except that...

[0116] The raw material is 867.6 grams of (NH4)6Mo7O 24 ·4H2O, 131.4 g Bi(NO3)3·5H2O, 530.8 g Ni(NO3)2·6H2O, 128.0 g Ca(NO3)2·4H2O, 589.9 g Fe(NO3)3·9H2O, 92.7 g Mg(NO3)2·6H2O, 13.3 g Rb(NO3)2, 93.8 g Pr(NO3)3·6H2O.

[0117] Example 6

[0118] The catalyst preparation steps are the same as in Example 1, except that citric acid is replaced with oxalic acid, and the molar ratio of the amount of oxalic acid added to the total number of moles of Mo, Bi, and Fe elements is 0.2:1.

[0119] Example 7

[0120] The catalyst preparation steps are the same as in Example 1, except that...

[0121] The spray drying conditions were a drying temperature of 350℃, a drying time of 1 hour, and an average droplet diameter of 100μm.

[0122] Example 8

[0123] The catalyst preparation steps are the same as in Example 1, except that...

[0124] The calcination conditions were as follows: calcination at 640°C for 0.5 h in an oxygen-containing atmosphere (oxygen volume fraction 21%).

[0125] Example 9

[0126] The catalyst preparation steps are the same as in Example 1, except that...

[0127] Add 150 grams of particles with an average particle size of 7 nm and a specific surface area of ​​380 m². 2 / g of fumed silica and 400g of water are added to mixed solution I to obtain slurry I;

[0128] Add 1875 grams of silica sol with a mass concentration of 40 wt% to slurry I to obtain slurry II.

[0129] Comparative Example 1

[0130] The catalyst preparation steps are the same as in Example 1, except that...

[0131] No fumed silica was added; only silica sol with a weight concentration of 40 wt% was used as the carrier precursor.

[0132] Comparative Example 2

[0133] The catalyst preparation steps are the same as in Example 1, except that...

[0134] No silica sol with a weight concentration of 40 wt% was added; only fumed silica was used as the carrier.

[0135] Comparative Example 3

[0136] The catalyst preparation steps are the same as in Example 1, except that...

[0137] Citric acid was replaced with acetic acid, and the molar ratio of the amount of acetic acid added to the total number of moles of Mo, Bi, and Fe elements was 0.2:1.

[0138] The catalyst-related data and evaluation data of the above embodiments and comparative examples are shown in Table 1 and Table 2, respectively.

[0139] Table 1

[0140]

[0141]

[0142] Table 2

[0143]

[0144] As can be seen from Tables 1 and 2, the ammonia oxidation catalyst prepared by the method of the present invention has a void ratio of 10%-30%, and has high propylene ammonia oxidation activity and acrylonitrile selectivity. It can also maintain a high acrylonitrile single-pass yield for a long time under high load conditions.

[0145] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. An ammonia oxidation catalyst, characterized in that, The catalyst comprises an active component and a support, wherein the active component has the following general formula Fe d Bi e Mo f A a B b C c O x ; Wherein, A is at least one of the alkali metal elements, B is at least one of the alkaline earth metal elements, transition metal elements, group IIIA metal elements, antimony and tellurium, and C is a rare earth element. The values ​​of a range from 0 to 1, b range from 0 to 12.5, c range from 0 to 3, d range from 0.1 to 4, e range from 0.01 to 3, f range from 9 to 16, and x is the total number of oxygen atoms required to satisfy the oxidation states of each element in the above active components; where e / f is 0.05-0.25 and d / f is 0.147-1. The catalyst includes microspheres with partially hollow spherical structures, and the hollowness of the catalyst is 12-21%. The hollowness refers to the percentage of microspheres with hollow structures in the catalyst microspheres out of the total number of catalyst microspheres. Microspheres with hollow structures refer to catalyst particles whose maximum diameter of the hollow structure exceeds 25% of the maximum diameter of the catalyst particles. The catalyst has a specific surface area of ​​30-45 m². 2 / g, with an average pore size of 6-15nm; The catalyst is prepared by the following method, including the following steps: (a) Provide a solution I containing the Mo precursor; (b) Provide a solution containing Fe precursor, Bi precursor, optional A precursor, optional B precursor, optional C precursor and polycarboxylic acid, and then age it to obtain solution II; (c) Mix solution I obtained in step (a), fumed silica, and optionally a solvent to obtain slurry I; (d) Mix the slurry I obtained in step (c) with the silica precursor to obtain slurry II; (e) Mix the slurry II obtained in step (d) and the solution II obtained in step (b) to obtain slurry III; (f) Boil the slurry III obtained in step (e); (g) The slurry obtained in step (f) is dried and calcined.

2. The catalyst according to claim 1, wherein, The alkali metal element is selected from at least one of Na, K, Rb, and Cs; And / or, the alkaline earth metal element is selected from at least one of Mg, Ca, Ba and Sr; And / or, the transition metal element is selected from at least one of Mn, Co, Ni, Zn, Cr, Zr, Ti, Nb and W; And / or, the Group IIIA metal element is selected from at least one of Al, Ga and In; And / or, the rare earth element is selected from at least one of Ce, Pr, Nd and Sm.

3. The catalyst according to claim 2, wherein, The transition metal element is selected from at least one of Ni, Co, and Mn.

4. The catalyst according to claim 1, wherein, The value of a ranges from 0.05 to 0.5, the value of b ranges from 1 to 10, the value of c ranges from 0.01 to 2, the value of d ranges from 0.5 to 4, the value of e ranges from 0.01 to 1.5, and the value of f ranges from 10 to 15.

5. The catalyst according to claim 1, wherein, The carrier is silicon dioxide.

6. The catalyst according to claim 1, wherein, Based on the total amount of catalyst, the content of the support is 30-70 wt%, and the content of the active component, calculated as oxide, is 30-70 wt%.

7. The catalyst according to claim 6, wherein, Based on the total amount of catalyst, the content of the support is 40-60 wt%, and the content of the active component, calculated as oxide, is 40-60 wt%.

8. A method for preparing the ammonia oxidation catalyst according to any one of claims 1-7, characterized in that, The method includes the following steps: (a) Provide a solution I containing the Mo precursor; (b) Provide a solution containing Fe precursor, Bi precursor, optional A precursor, optional B precursor, optional C precursor and polycarboxylic acid, and then age it to obtain solution II; (c) Mix solution I obtained in step (a), fumed silica, and optionally a solvent to obtain slurry I; (d) Mix the slurry I obtained in step (c) with the silica precursor to obtain slurry II; (e) Mix the slurry II obtained in step (d) and the solution II obtained in step (b) to obtain slurry III; (f) Boil the slurry III obtained in step (e); (g) The slurry obtained in step (f) is dried and calcined; Wherein, A is at least one of the alkali metal elements, B is at least one of the alkaline earth metal elements, transition metal elements, Group IIIA metal elements, antimony and tellurium, and C is a rare earth element.

9. The preparation method according to claim 8, wherein, The fumed silica particles have an average particle size of 5-30 nm and a specific surface area of ​​200-500 m². 2 / g.

10. The preparation method according to claim 9, wherein, The fumed silica has an average particle size of 5-15 nm and a specific surface area of ​​300-450 m². 2 / g.

11. The preparation method according to claim 8, wherein, The silica precursor is selected from at least one of silica sol, water glass, inorganic silica gel, and silicate ester.

12. The preparation method according to claim 11, wherein, The silica precursor is silica sol.

13. The preparation method according to claim 12, wherein, The solid content of the silica sol is 20-50 wt% based on silicon dioxide.

14. The preparation method according to claim 8, wherein, The mass ratio of the fumed silica to the silica precursor is 1:1-20, based on silica.

15. The preparation method according to claim 14, wherein, The mass ratio of the fumed silica to the silica precursor is 1:2-20, based on silica.

16. The preparation method according to claim 8, wherein, The alkali metal element is selected from at least one of Na, K, Rb, and Cs; And / or, the alkaline earth metal element is selected from at least one of Mg, Ca, Ba and Sr; And / or, the transition metal element is selected from at least one of Mn, Co, Ni, Zn, Cr, Zr, Ti, Nb and W; And / or, the Group IIIA metal element is selected from at least one of Al, Ga and In; And / or, the rare earth element is selected from at least one of Ce, Pr, Nd and Sm.

17. The preparation method according to claim 16, wherein, The transition metal element is selected from at least one of Ni, Co, and Mn.

18. The preparation method according to claim 8, wherein, The precursors of Fe, Bi, Mo, A, B, and C are soluble compounds of the corresponding elements.

19. The preparation method according to any one of claims 8-18, wherein, The molar ratio of Fe, Bi, Mo, A, B, and C is 0.1-4:0.01-3:9-16:0-1:0-12.5:0-3.

20. The preparation method according to claim 19, wherein, The molar ratio of Fe, Bi, Mo, A, B, and C is 0.5-3:0.01-1.5:10-15:0.05-0.5:1-10:0.01-2.

21. The preparation method according to any one of claims 8-18, wherein, The molar ratio of Bi to Mo is 0.005-0.

5.

22. The preparation method according to claim 21, wherein, The molar ratio of Bi to Mo is 0.01-0.

25.

23. The preparation method according to any one of claims 8-18, wherein, The molar ratio of Fe to Mo is 0.02-1.

25.

24. The preparation method according to claim 23, wherein, The molar ratio of Fe to Mo is 0.1-1.

25. The preparation method according to claim 8, wherein, The amounts of Fe precursor, Bi precursor, optional A element precursor, optional B element precursor, optional C element precursor, fumed silica, and silica precursor are such that the content of Fe, Bi, Mo, A, B, and C, calculated as oxides, in the prepared catalyst is 30-70 wt% based on the total amount of catalyst, and the content of silica is 30-70 wt%.

26. The preparation method according to claim 25, wherein, The amounts of Fe precursor, Bi precursor, optional A element precursor, optional B element precursor, optional C element precursor, fumed silica, and silica precursor are such that the content of Fe, Bi, Mo, A, B, and C, calculated as oxides, in the prepared catalyst is 40-60 wt% based on the total amount of catalyst, and the content of silica is 40-60 wt%.

27. The preparation method according to claim 8, wherein, In step (b), the polycarboxylic acid is selected from at least one of citric acid, oxalic acid, tartaric acid, and ethylenediaminetetraacetic acid.

28. The preparation method according to claim 27, wherein, In step (b), the polycarboxylic acid is citric acid.

29. The preparation method according to claim 8, wherein, In step (b), the molar ratio of the amount of the added polycarboxylic acid to the total molar number of Fe, Bi, and Mo is 0.01-0.5:

1.

30. The preparation method according to claim 8, wherein, In step (b), the polycarboxylic acid is added after mixing the Fe precursor, Bi precursor, optional A element precursor, optional B element precursor and optional C element precursor.

31. The preparation method according to claim 8, wherein, In step (b), the aging conditions include: a temperature of 40-80℃, a time of 0.1-0.5h, and a stirring speed of 200-1000rpm.

32. The preparation method according to claim 8, wherein, In step (f), the conditions for boiling the slurry include: a temperature of 80-175℃, a time of 0.1-3h, and a stirring speed of 200-1000rpm.

33. The preparation method according to claim 8, wherein, In step (g), the drying method is spray drying, and the conditions for spray drying include: drying temperature of 250-400℃, drying time of 0.5-3h, and average diameter of spray droplets of 40-200μm.

34. The preparation method according to claim 8, wherein, In step (g), the calcination conditions include: calcination temperature of 200-750℃ and calcination time of 1-8h under an oxygen-containing atmosphere.

35. The use of the catalyst according to any one of claims 1-7 in the ammonia oxidation reaction.

36. The application according to claim 35, wherein, The application is in the ammoxidation reaction of olefins.

37. The application according to claim 36, wherein, The application is in the ammoxidation of propylene to produce acrylonitrile.

38. A method for preparing acrylonitrile, characterized in that, The method comprises: reacting propylene, an ammonia source, and an oxygen source in the presence of the catalyst described in any one of claims 1-7.

39. The method according to claim 38, wherein, The conditions for the contact reaction include: a molar ratio of propylene: ammonia source: oxygen source of 1:1-1.5:8-10.5 (based on ammonia gas). And / or, the reaction temperature is 400-470℃; And / or, the reaction pressure is 0.03-0.15 MPa; And / or, the reaction loading (WWH) is 0.045-0.15 h. -1 .

40. The method according to claim 39, wherein, The conditions for the contact reaction include: a molar ratio of propylene: ammonia source: oxygen source of 1:1-1.3:8.8-10 (based on ammonia gas). And / or, the reaction temperature is 410-450℃; And / or, the reaction pressure is 0.06-0.14 MPa; And / or, the reaction loading (WWH) is 0.06-0.12 h. -1 .

Citation Information

Patent Citations

  • Acrylonitrile catalyst for ammonia oxidation process

    CN107282060B

  • Acrylonitrile catalyst for propylene ammoxidation

    CN107282063B

  • Acrylonitrile catalysts and their preparation methods

    CN107282065B

  • Acrylonitrile catalyst for ammonia oxidation

    CN107282094B

  • Ammoxidation catalyst particles as well as preparation method and application thereof

    CN111744493A