High-strength ultra-thin copper foil with dispersion-strengthened copper composite structure and method for manufacturing the same
By vacuum magnetron sputtering copper plating on aluminum foil, followed by electroplating for thickening, rolling, and high-temperature internal oxidation, an ultra-thin copper foil with a dispersion-strengthened copper composite structure is formed. This solves the problems of the difficulty in preparing ultra-thin copper foil and its insufficient strength, achieving high strength, excellent conductivity, and corrosion resistance.
Patent Information
- Application Number
- CN202411951890.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-12-27
AI Technical Summary
In the existing technology, it is difficult to prepare ultra-thin copper foil and its strength performance is insufficient. In particular, ultra-thin copper foil with a thickness of less than 9μm is prone to curling, bending and mechanical properties are reduced during production and application.
Copper is plated on one side of aluminum foil using vacuum magnetron sputtering technology. The copper layer is thickened by electroplating and rolled to form an aluminum/copper-aluminum solid solution structure. The aluminum layer is peeled off by electrochemical treatment and a dispersion-strengthened copper composite structure is formed by high-temperature internal oxidation treatment. The interfacial bonding ability is improved by combining surface treatment agents.
The prepared ultrathin copper foil has excellent mechanical properties, electrical conductivity and high-temperature creep properties, improved tensile strength, enhanced surface corrosion resistance, and a dense oxide film formed on the surface of the copper foil.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of composite ultrathin copper foil manufacturing technology, specifically relating to high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure and its preparation method. Background Technology
[0002] Ultra-thin copper foil typically refers to copper foil with a thickness of less than 9μm. With the rapid development of electronic information technology, high-performance lithium batteries require copper foil to achieve both superior performance and thinner thickness. Therefore, the demand for ultra-thin copper foil is increasing, especially for foils with a thickness of 5μm or less. Due to limitations in production equipment, the thickness of rolled copper foil is difficult to reduce to less than 6μm. Currently, the production of ultra-thin copper foil mainly relies on electroplated copper foil, and the higher the performance requirements of lithium battery copper foil, the greater the processing difficulty. Because the thickness of ultra-thin copper foil is less than 9μm, it is prone to curling and bending during production and application. Furthermore, reducing the thickness of ultra-thin copper foil also leads to a decrease in mechanical properties, presenting a significant technical challenge.
[0003] Chinese invention patent CN114045536B discloses a method for preparing gradient ultrathin copper foil with both high strength and high ductility, comprising the following steps: Step S1, preparing a clean titanium foil substrate; Step S2, mixing and dissolving copper sulfate pentahydrate, concentrated sulfuric acid, and additives in a certain proportion to obtain a deposition electrolyte solution, wherein the amounts of copper sulfate pentahydrate and concentrated sulfuric acid are 140~240 g / L and 100~150 mM, respectively; Step S3, electrochemically depositing copper foil, with a current range of 0~700 mA / cm. 2 The temperature gradient is maintained between 30 and 50°C. The resulting copper foil exhibits a uniformly varied gradient structure, simultaneously improving its tensile strength and tensile properties while maintaining an ultra-thin thickness of 5–35 μm. However, existing technologies suffer from the technical challenges of fabricating extremely thin copper foils and insufficient strength performance. Summary of the Invention
[0004] The purpose of this invention is to provide a high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure and its preparation method, in order to solve the technical problems of the difficulty in preparing ultrathin copper foil and its insufficient strength performance in the prior art.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure includes the following steps: S1. After removing the oxide layer by sanding the aluminum foil with a thickness of 0.03~0.06μm, add 90~95wt% ethanol to clean for 5~10min, then clean with 5~10wt% acetic acid for 5~8min, and finally rinse with deionized water 2~3 times and dry at 40~60℃ to obtain the pretreated aluminum foil. S2. The pretreated aluminum foil is subjected to single-sided copper plating using vacuum magnetron sputtering technology, with the single-sided copper layer thickness controlled to be 30~60nm. Then, the copper layer is thickened by 3~5μm using electroplating technology to obtain copper-aluminum composite foil. S3. After rolling and compacting the copper-aluminum composite foil, place it in a resistance furnace and heat it at 300~400℃ for 2~4 hours to form a copper-aluminum composite foil with a three-layer structure of aluminum / copper-aluminum solid solution / copper. S4. Place the copper-aluminum composite foil into an electrolytic cell, with the copper layer as the negative electrode and the aluminum layer as the positive electrode. Electrolyze and dissolve the aluminum layer to obtain an extremely thin composite copper layer. S5. A surface treatment agent is coated on the surface of an extremely thin composite copper layer, and then heat-treated at a high temperature of 800~950℃ under an argon atmosphere to form a dispersion-strengthened copper composite foil.
[0006] Preferably, the vacuum degree of vacuum magnetron sputtering in S2 is lower than 2~3×10⁻⁶. -4 MPa, sputtering power of 50~60W, working pressure of 0.5~0.6Pa, aluminum foil temperature of 150~200℃, atmosphere of either argon or nitrogen, and target material of pure copper with a purity of 99.999% or higher.
[0007] Preferably, the copper plating solution in S2 is composed of 80-100 g / L copper sulfate, 0.05-0.1 g / L sodium chloride, 0.2-0.5 g / L polyethylene glycol, and 90-100 g / L sulfuric acid.
[0008] Preferably, in step S2, the electroplating temperature is 40~50℃, the copper plating solution circulation rate is 2~4L / min, and the current density range is 300~500A / m. 2 The coating time is 30~60s.
[0009] Preferably, the electrolyte in S4 is composed of 60-70 g / L sulfuric acid, 30-50 g / L copper sulfate, 3-6 g / L sodium carboxymethyl cellulose, 20-25 g / L potassium sodium tartrate, 1-2 g / L disodium ethylenediaminetetraacetate and 0.2-0.5 g / L sodium polydisulfide dipropane sulfonate.
[0010] Preferably, the current density in S4 is in the range of 100~800 A / m. 2 The voltage range of the electrolytic cell is 0.5~5V.
[0011] Preferably, the preparation method of the surface treatment agent in S5 includes the following steps: S11. Add 0.05~0.06 parts of copper acetate to 50 parts of deionized water, heat in an oil bath to 70~80℃, then add 20~30 parts of 70~80g / L sodium hydroxide solution dropwise, and finally add 5~6 parts of 300g / L glucose solution dropwise. React for 2~3 hours, filter to collect the solid, and dry at 50~60℃ to obtain nano cuprous oxide powder. S12. Add bis(trimethylsiloxymethylsilane) to deionized water and heat at 70-80℃ for 1-2 hours. Add nano-cuprous oxide powder while stirring, control the pH to 7.5-8.5, and react at 70-80℃ for 20-24 hours. Filter and dry to obtain modified nano-cuprous oxide powder. S13. Dissolve 0.5-0.6 parts of chitosan in 100 parts of deionized water, stir at 40-50℃ for 1-2 hours, add 0.5-0.8 parts of modified nano cuprous oxide powder and 0.3-0.5 parts of 1H-benzimidazole-5,6-diol to prepare a surface treatment agent.
[0012] Preferably, the mass ratio of bis(trimethylsiloxymethylsilane) to nano-cuprous oxide powder in S12 is 0.5~0.8:1.
[0013] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. Based on existing technology, this invention uses a method of single-sided copper plating on aluminum foil through vacuum magnetron sputtering, followed by electroplating to thicken the copper layer, followed by high-temperature treatment after rolling and electrochemical treatment to peel off the aluminum layer, and then high-temperature internal oxidation treatment to produce an ultra-thin copper foil with excellent mechanical properties, electrical conductivity and high-temperature creep resistance.
[0014] 2. This invention uses heat treatment to form a copper-aluminum alloy layer on the sputtered surface of the copper layer of the copper-aluminum composite foil. The copper foil is relatively thick, making it difficult to achieve sufficient diffusion of aluminum into the copper. The high-temperature internal oxidation treatment transforms the aluminum solute atoms into nano-Al2O3 reinforcing phase, which can effectively hinder the dislocation movement of the copper foil and has little impact on the conductivity of copper. Therefore, the copper foil with the dispersion-reinforced copper composite structure has good conductivity and improved tensile strength.
[0015] 3. This invention modifies nano-cuprous oxide powder with bis(trimethylsiloxymethylsilane), and then combines it with chitosan and 1H-benzimidazole-5,6-diol to obtain a surface treatment agent that enhances the interfacial bonding ability between the copper foil surface and the nano-cuprous oxide, making it easier for a dense oxide film to form on the copper foil surface, thereby improving the corrosion resistance of the copper foil. Detailed Implementation
[0016] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0017] Example 1: The preparation method of high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure in this example includes the following steps: S1. After removing the oxide layer by sanding the 0.06μm thick aluminum foil, it is cleaned in 95wt% ethanol for 10min, then cleaned in 5wt% acetic acid for 8min, and finally rinsed with deionized water 3 times and dried at 60℃ to obtain the pretreated aluminum foil. S2. The pretreated aluminum foil is then subjected to single-sided copper plating using vacuum magnetron sputtering technology. The vacuum degree of the vacuum magnetron sputtering is less than 3×10⁻⁶. -4 The sputtering pressure was set at MPa, sputtering power at 60W, working pressure at 0.6Pa, aluminum foil temperature at 200℃, and argon atmosphere. A pure copper target with a purity of 99.999% or higher was used. The single-sided copper layer thickness was controlled at 60nm. A copper plating solution composed of 100g / L copper sulfate, 0.05g / L sodium chloride, 0.2g / L polyethylene glycol, and 98g / L sulfuric acid was prepared. The circulation rate of the copper plating solution was set at 4L / min, and the current density at 300A / m². 2 The plating time is 40s, which increases the copper layer thickness by 3.5μm, resulting in a copper-aluminum composite foil; S3. After rolling and compacting the copper-aluminum composite foil, place it in a resistance furnace and heat it at 400℃ for 4 hours to form a copper-aluminum composite foil with a three-layer structure of aluminum / copper-aluminum solid solution / copper. S4. Prepare an electrolyte solution consisting of 65 g / L sulfuric acid, 40 g / L copper sulfate, 5 g / L sodium carboxymethyl cellulose, 20 g / L potassium sodium tartrate, 2 g / L disodium ethylenediaminetetraacetate, and 0.2 g / L sodium polydisulfide dipropane sulfonate. Place the copper-aluminum composite foil into the electrolytic cell, with the copper layer as the negative electrode and the aluminum layer as the positive electrode. The current density is 400 A / m. 2 The electrolytic cell voltage is 3V, and an extremely thin composite copper layer is obtained by electrolytically dissolving the aluminum layer. S5. A surface treatment agent is coated on the surface of an extremely thin composite copper layer, and then heat-treated at 850°C under an argon atmosphere to form a dispersion-strengthened copper composite foil.
[0018] The preparation method of the surface treatment agent in this embodiment includes the following steps: S11. Add 0.06 parts of copper acetate to 50 parts of deionized water, heat in an oil bath to 80°C, then add 20 parts of 75 g / L sodium hydroxide solution dropwise, and finally add 5 parts of 300 g / L glucose solution dropwise. React for 2.5 h, filter to collect the solid, and dry at 60°C to obtain nano cuprous oxide powder. S12. Add 0.025 parts of bistrimethylsiloxymethylsilane to deionized water, heat at 80°C for 2 hours, add 0.05 parts of nano cuprous oxide powder while stirring, control the pH to 8, react at 80°C for 24 hours, filter and dry to obtain modified nano cuprous oxide powder. S13. Dissolve 0.6 parts of chitosan in 100 parts of deionized water, stir at 50°C for 2 hours, add 0.5 parts of modified nano-cuprous oxide powder and 0.3 parts of 1H-benzimidazole-5,6-diol to prepare a surface treatment agent.
[0019] Example 2, the preparation method of high-strength ultrathin copper foil with dispersion-strengthened copper composite structure in this example includes the following steps: S1. After removing the oxide layer by sanding the 0.06μm thick aluminum foil, it is cleaned in 95wt% ethanol for 10min, then cleaned in 5wt% acetic acid for 8min, and finally rinsed with deionized water 3 times and dried at 60℃ to obtain the pretreated aluminum foil. S2. The pretreated aluminum foil is then subjected to single-sided copper plating using vacuum magnetron sputtering technology. The vacuum level of the vacuum magnetron sputtering is less than 2×10⁻⁶. -4 The sputtering pressure was 55 MPa, the sputtering power was 55 W, the working pressure was 0.5 Pa, the aluminum foil temperature was 160 °C, the sputtering atmosphere was argon, and the target material was pure copper with a purity of over 99.999%. The single-sided copper layer thickness was controlled at 55 nm. The copper plating solution consisted of 80 g / L copper sulfate, 0.1 g / L sodium chloride, 0.5 g / L polyethylene glycol, and 100 g / L sulfuric acid. The circulation rate of the copper plating solution was set to 2 L / min, and the current density was 500 A / m. 2 The plating time is 30s, which increases the copper layer thickness by 4μm to obtain copper-aluminum composite foil; S3. After rolling and compacting the copper-aluminum composite foil, place it in a resistance furnace and heat it at 350°C for 3 hours to form a copper-aluminum composite foil with a three-layer structure of aluminum / copper-aluminum solid solution / copper. S4. Prepare an electrolyte solution consisting of 70 g / L sulfuric acid, 40 g / L copper sulfate, 3 g / L sodium carboxymethyl cellulose, 21 g / L potassium sodium tartrate, 1.2 g / L disodium ethylenediaminetetraacetate, and 0.3 g / L sodium polydisulfide dipropane sulfonate. Place the copper-aluminum composite foil into the electrolytic cell, with the copper layer as the negative electrode and the aluminum layer as the positive electrode. The current density is 100 A / m. 2 The electrolytic cell voltage is 0.8V, and an extremely thin composite copper layer is obtained by electrolytically dissolving the aluminum layer. S5. A surface treatment agent is coated on the surface of an extremely thin composite copper layer, and then heat-treated at 800°C under an argon atmosphere to form a dispersion-strengthened copper composite foil.
[0020] The surface treatment agent in this embodiment is prepared using the same method as in Example 1.
[0021] Example 3, the preparation method of high-strength ultrathin copper foil with dispersion-strengthened copper composite structure in this example includes the following steps: S1. After removing the oxide layer by sanding the 0.06μm thick aluminum foil, it is cleaned in 95wt% ethanol for 10min, then cleaned in 5wt% acetic acid for 8min, and finally rinsed with deionized water 3 times and dried at 60℃ to obtain the pretreated aluminum foil. S2. The pretreated aluminum foil is then subjected to single-sided copper plating using vacuum magnetron sputtering technology. The vacuum degree of the vacuum magnetron sputtering is less than 3×10⁻⁶. -4 The sputtering pressure was 50W, the working pressure was 0.5Pa, the aluminum foil temperature was 180℃, the sputtering atmosphere was nitrogen, the target material was pure copper with a purity of 99.999% or higher, the single-sided copper layer thickness was controlled to be 60nm, and a copper plating solution composed of 85g / L copper sulfate, 0.075g / L sodium chloride, 0.5g / L polyethylene glycol and 90g / L sulfuric acid was prepared. The copper layer was thickened by 3μm by water electroplating technology to obtain copper-aluminum composite foil. S3. After rolling and compacting the copper-aluminum composite foil, place it in a resistance furnace and heat it at 450°C for 2 hours to form a copper-aluminum composite foil with a three-layer structure of aluminum / copper-aluminum solid solution / copper. S4. Prepare an electrolyte solution consisting of 65 g / L sulfuric acid, 50 g / L copper sulfate, 6 g / L sodium carboxymethyl cellulose, 25 g / L potassium sodium tartrate, 1.6 g / L disodium ethylenediaminetetraacetate, and 0.4 g / L sodium polydisulfide dipropane sulfonate. Place the copper-aluminum composite foil into the electrolytic cell, with the copper layer as the negative electrode and the aluminum layer as the positive electrode. The current density is 500 A / m. 2 The electrolytic cell voltage is 5V, and an extremely thin composite copper layer is obtained by electrolytically dissolving the aluminum layer. S5. A surface treatment agent is coated on the surface of an extremely thin composite copper layer, and then heat-treated at 950°C under an argon atmosphere to form a dispersion-strengthened copper composite foil.
[0022] The surface treatment agent in this embodiment is prepared using the same method as in Example 1.
[0023] Example 4: The preparation method of the high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure in this example includes the following steps: S1. After removing the oxide layer by sanding the 0.06μm thick aluminum foil, it is cleaned in 95wt% ethanol for 10min, then cleaned in 5wt% acetic acid for 8min, and finally rinsed with deionized water 3 times and dried at 60℃ to obtain the pretreated aluminum foil. S2. The pretreated aluminum foil is then subjected to single-sided copper plating using vacuum magnetron sputtering technology. The vacuum level of the vacuum magnetron sputtering is less than 2.5 × 10⁻⁶. -4 The sputtering pressure was set at MPa, sputtering power at 60W, working pressure at 0.6Pa, aluminum foil temperature at 190℃, and a nitrogen atmosphere. A pure copper target with a purity of 99.999% or higher was used. The single-sided copper layer thickness was controlled at 30nm. A copper plating solution was prepared, consisting of 100g / L copper sulfate, 0.06g / L sodium chloride, 0.5g / L polyethylene glycol, and 100g / L sulfuric acid. The circulation rate of the copper plating solution was set at 3L / min, and the current density at 500A / m². 2 The plating time is 60s, which increases the copper layer thickness by 5μm to obtain copper-aluminum composite foil; S3. After rolling and compacting the copper-aluminum composite foil, place it in a resistance furnace and heat it at 400℃ for 4 hours to form a copper-aluminum composite foil with a three-layer structure of aluminum / copper-aluminum solid solution / copper. S4. Prepare an electrolyte solution consisting of 70 g / L sulfuric acid, 30 g / L copper sulfate, 4 g / L sodium carboxymethyl cellulose, 20 g / L potassium sodium tartrate, 1 g / L disodium ethylenediaminetetraacetate, and 0.5 g / L sodium polydisulfide dipropane sulfonate. Place the copper-aluminum composite foil into the electrolytic cell, with the copper layer as the negative electrode and the aluminum layer as the positive electrode. The current density is 500 A / m. 2 The electrolytic cell voltage is 5V, and an extremely thin composite copper layer is obtained by electrolytically dissolving the aluminum layer. S5. A surface treatment agent is coated on the surface of an extremely thin composite copper layer, and then heat-treated at 900°C under an argon atmosphere to form a dispersion-strengthened copper composite foil.
[0024] The difference between the surface treatment agent in this embodiment and that in Example 1 is that the mass ratio of bis(trimethylsiloxymethylsilane) to nano-cuprous oxide powder is 0.8:1.
[0025] Comparative Example 1 differs from Example 1 in that it does not involve rolling but instead undergoes direct heat treatment in step S3.
[0026] Comparative Example 2 differs from Example 1 in that the surface treatment agent is replaced with chitosan and nano cuprous oxide powder.
[0027] Comparative Example 3 differs from Example 1 in that the thickness of the electroplated copper layer is replaced with 1 μm.
[0028] Performance testing The copper foils prepared in each embodiment and comparative example had their peel strength measured using a peel strength tester and their tensile strength measured using a universal testing machine. The test results are shown in Table 1 below: Serial Number Peel strength (N / mm) Tensile strength (MPa) Example 1 0.61 195 Example 2 0.55 201 Example 3 0.59 198 Example 4 0.57 205 Comparative Example 1 0.36 167 Comparative Example 2 0.54 188 Comparative Example 3 0.33 146 Table 1 The density of the copper foils prepared in each embodiment and comparative example was measured multiple times, and the average value was taken. The conductivity was measured using a benchtop conductivity meter, and the test results are shown in Table 2 below. Table 2 Serial Number <![CDATA[Density (g / cm 2 )]]> Electrical conductivity (S / m) Example 1 7.26 <![CDATA[5.76×10 7 ]]> Example 2 7.32 <![CDATA[5.77×10 7 ]]> Example 3 7.41 <![CDATA[5.71×10 7 ]]> Example 4 7.36 <![CDATA[5.73×10 7 ]]> Comparative Example 1 7.15 <![CDATA[5.63×10 7 ]]> Comparative Example 2 7.47 <![CDATA[5.70×10 7 ]]> Comparative Example 3 6.12 <![CDATA[5.56×10 7 ]]> The data in the table show that the peel strength of the copper foils prepared in Examples 1-4 is between 0.55 and 0.61 N / mm, and the tensile strength is between 195 and 205 MPa, indicating that the copper foils with the dispersion-reinforced copper composite structure obtained in this invention have excellent mechanical properties; the density of the copper foils prepared in Examples 1-4 is 7.26-7.41 g / cm³. 2 And the conductivity is 5.71×10 7 ~5.77×10 7 The ratio between S / m indicates that the copper foil obtained by the present invention is lighter and has excellent conductivity compared to pure copper foil. In contrast, the copper layer thickened by electroplating in Comparative Example 3 is only 1.5 μm. The subsequent process increases the content of dispersed aluminum in the copper layer through heat treatment, so its density is much lower than that of the embodiments. Moreover, the excessive content of dispersed aluminum leads to a significant decrease in its conductivity.
[0029] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
[0030] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure, characterized in that, Includes the following steps: S1. After removing the oxide layer by sanding the aluminum foil with a thickness of 0.03~0.06μm, add 90~95wt% ethanol to clean for 5~10min, then clean with 5~10wt% acetic acid for 5~8min, and finally rinse with deionized water 2~3 times and dry at 40~60℃ to obtain the pretreated aluminum foil. S2. The pretreated aluminum foil is subjected to single-sided copper plating using vacuum magnetron sputtering technology, with the single-sided copper layer thickness controlled to be 30~60nm. Then, the copper layer is thickened by 3~5μm using electroplating technology to obtain copper-aluminum composite foil. S3. After rolling and compacting the copper-aluminum composite foil, place it in a resistance furnace and heat it at 300~400℃ for 2~4 hours to form a copper-aluminum composite foil with a three-layer structure of aluminum / copper-aluminum solid solution / copper. S4. Place the copper-aluminum composite foil into an electrolytic cell, with the copper layer as the negative electrode and the aluminum layer as the positive electrode. Electrolyze and dissolve the aluminum layer to obtain an extremely thin composite copper layer. S5. Coat the surface of the ultra-thin composite copper layer with a surface treatment agent, and heat-treat it at a high temperature of 800~950℃ under an argon atmosphere to form a dispersion-strengthened copper composite foil. The preparation method of the surface treatment agent in S5 includes the following steps: S11. Add 0.05~0.06 parts of copper acetate to 50 parts of deionized water, heat in an oil bath to 70~80℃, then add 20~30 parts of 70~80g / L sodium hydroxide solution dropwise, and finally add 5~6 parts of 300g / L glucose solution dropwise. React for 2~3 hours, filter to collect the solid, and dry at 50~60℃ to obtain nano cuprous oxide powder. S12. Add bis(trimethylsiloxymethylsilane) to deionized water and heat at 70-80℃ for 1-2 hours. Add nano-cuprous oxide powder while stirring, control the pH to 7.5-8.5, and react at 70-80℃ for 20-24 hours. Filter and dry to obtain modified nano-cuprous oxide powder. S13. Dissolve 0.5-0.6 parts of chitosan in 100 parts of deionized water, stir at 40-50℃ for 1-2 hours, add 0.5-0.8 parts of modified nano cuprous oxide powder and 0.3-0.5 parts of 1H-benzimidazole-5,6-diol to prepare a surface treatment agent.
2. The method for preparing high-strength ultrathin copper foil with a dispersion-reinforced copper composite structure according to claim 1, characterized in that, The vacuum level controlled by vacuum magnetron sputtering in S2 is lower than 2~3×10⁻⁶. -4 MPa, sputtering power of 50~60W, working pressure of 0.5~0.6Pa, aluminum foil temperature of 150~200℃, atmosphere of either argon or nitrogen, and target material of pure copper with a purity of 99.999% or higher.
3. The method for preparing high-strength ultrathin copper foil with a dispersion-reinforced copper composite structure according to claim 1, characterized in that, The copper plating solution in S2 consists of 80-100 g / L copper sulfate, 0.05-0.1 g / L sodium chloride, 0.2-0.5 g / L polyethylene glycol, and 90-100 g / L sulfuric acid. The electroplating temperature is 40-50℃, the circulation rate of the copper plating solution is 2-4 L / min, and the current density range is 300-500 A / m. 2 The coating time is 30~60s.
4. The method for preparing high-strength ultrathin copper foil with a dispersion-reinforced copper composite structure according to claim 1, characterized in that, The electrolyte in S4 consists of 60-70 g / L sulfuric acid, 30-50 g / L copper sulfate, 3-6 g / L sodium carboxymethyl cellulose, 20-25 g / L potassium sodium tartrate, 1-2 g / L disodium ethylenediaminetetraacetate, and 0.2-0.5 g / L sodium polydisulfide dipropane sulfonate, with a current density range of 100-800 A / m. 2 The voltage range of the electrolytic cell is 0.5~5V.
5. The method for preparing high-strength ultrathin copper foil with a dispersion-reinforced copper composite structure according to claim 1, characterized in that, The mass ratio of bis(trimethylsiloxymethylsilane) to nano-cuprous oxide powder in S12 is 0.5~0.8:
1.
6. The high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure prepared by the method for preparing high-strength ultrathin copper foil with a dispersion-strengthened copper composite structure according to any one of claims 1 to 5.
Citation Information
Patent Citations
A method for preparing gradient ultrathin copper foil with both high strength and high ductility
CN114045536B
Aluminum-copper composite foil and preparation method thereof
CN114242940A
Lithium ion battery copper foil and preparation method and application thereof
CN118156515A