A method for desilication of celestite ore

By using grinding, desilication, alkali washing, and acid washing steps, and treating celestite powder with hydrochloric acid, ammonium fluoride, sodium hydroxide, and sulfuric acid solutions, the problem of difficult removal of silica in celestite ore is solved, achieving efficient desilication and low loss, which is suitable for industrial production.

CN119976923BActive Publication Date: 2026-11-20SICHUAN UNIVERSITY OF SCIENCE AND ENGINEERING
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510216993.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-02-26
Publication Date
2026-11-20
Estimated Expiration
2045-02-26

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively remove silica and other silicon compounds from celestite ore, resulting in low concentrate grades and impacting the purity and cost of the strontium salt industry.

Method used

The process involves grinding, desilication, alkali washing, and acid washing. Celestite powder is treated with hydrochloric acid, ammonium fluoride, sodium hydroxide, and sulfuric acid solutions, with temperature and time controlled to achieve efficient desilication.

Benefits of technology

It achieves a desilication rate of up to 97.5% and a strontium loss rate of less than 1.7%, reducing the preparation cost and time of high-purity strontium carbonate, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119976923B_ABST
    Figure CN119976923B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of ore processing and treatment, and particularly relates to a method for deep desilication of celestite ore, which comprises the following steps: S1, grinding operation: after celestite ore is ground and sieved, celestite powder is obtained; S2, desilication operation: hydrochloric acid solution and ammonium fluoride are added to the celestite powder, and after desilication, first filtration, first washing and first drying, desilicated celestite powder is obtained; S3, alkali washing operation: sodium hydroxide solution is added to the desilicated celestite powder, and after alkali washing, second filtration, second washing and second drying, alkali-washed celestite powder is obtained; S4, acid washing operation: sulfuric acid solution is added to the alkali-washed celestite powder, and after acid washing, third filtration, third washing and third drying, refined celestite powder is obtained. The method for deep desilication of celestite ore can effectively remove silicon at a low reaction temperature, while ensuring a low loss rate of strontium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of ore processing technology, specifically relating to a deep desilication method for celestite ore. Background Technology

[0002] Celestite ore, primarily composed of strontium sulfate, is an important mineral resource with wide applications in electronics, pharmaceuticals, military, and optics. However, with continuous mining, gangue impurities have become increasingly severe, significantly impacting celestite grade. Even after flotation or reverse flotation, celestite still contains impurities, mainly carbonates, metal oxides, silica, and other silicon-based compounds. Silicon-containing impurities constitute a significant proportion and are difficult to remove. While silicon content varies slightly across different celestite concentrates, it remains relatively high, sometimes even the highest. Existing pretreatment processes effectively remove carbonates and metal oxides from celestite ore, but are less effective at removing silica and other silicon compounds. Currently, the conventional desilication methods in the strontium salt industry are flotation or reverse flotation. These methods are suitable for celestite ore with high silica content, producing a concentrate grade of approximately 80%–90%, with silica and other silicon-based compounds accounting for about 3%–5%.

[0003] The crude strontium carbonate prepared by the existing process of single metathesis contains silicon compounds as acid-insoluble residues. It is necessary to carry out acid dissolution and then metathesis reaction again to obtain high-purity strontium carbonate. The preparation of strontium carbonate by metathesis has high requirements for the purity of the raw material celestite.

[0004] Therefore, a new desilication method for celestite ore is needed to achieve effective desilication of celestite ore with a simple and convenient process. Summary of the Invention

[0005] The problem this application aims to solve is to provide a desilication method for celestite ore that can effectively remove silicon while ensuring a low strontium loss rate, requiring only a relatively low reaction temperature.

[0006] To solve the above problems, this application adopts the following technical solution:

[0007] This application provides a method for desilication of celestite ore, comprising the following steps:

[0008] S1. Grinding operation: Celestite ore is ground and then sieved to obtain celestite powder;

[0009] S2. Desilication process: Hydrochloric acid solution and ammonium fluoride are added to the celestite powder, and after desilication, first filtration, first washing and first drying, desilication celestite powder is obtained.

[0010] S3. Alkali washing operation: Add sodium hydroxide solution to the desilication celestite powder, and perform alkali washing, second filtration, second washing and second drying to obtain alkali-washed celestite powder.

[0011] S4. Acid washing process: Add sulfuric acid solution to the alkaline-washed celestite powder, and perform acid washing, third filtration, third washing and third drying to obtain refined celestite powder.

[0012] Furthermore, the particle size of the celestite powder is 40–75 μm.

[0013] Furthermore, the concentration of the hydrochloric acid solution is 15–22 wt%.

[0014] Furthermore, the concentration of the sodium hydroxide solution is 20–30 wt%.

[0015] Furthermore, the concentration of the sulfuric acid solution is 35–45 wt%.

[0016] Furthermore, the solid-liquid ratio (g / mL) of the celestite powder, the hydrochloric acid solution, the sodium hydroxide solution, and the sulfuric acid solution is 1:(1.5~2.5):(0.8~1.4):(2~3).

[0017] Furthermore, the weight ratio of the celestite powder to the ammonium fluoride is 1:(0.20-0.6).

[0018] Furthermore, the desilication temperature is 70–80°C, and the desilication time is 50–60 minutes.

[0019] Furthermore, the temperature of the alkaline washing is 60–75°C, and the washing time is 50–60 minutes.

[0020] Furthermore, the pickling temperature is 60–75°C, and the pickling time is 50–60 minutes.

[0021] This application has the following beneficial effects:

[0022] (1) The desiliconization method for celestite ore provided in this application has a desiliconization rate of over 97.5%, which can effectively remove silicon from celestite ore and ensure low loss of effective components during the desiliconization process, with a strontium loss rate of less than 1.7%.

[0023] (2) The desilication method for celestite ore provided in this application is simple in steps, the raw materials involved are readily available, no high-temperature roasting is required, the reaction time is short, and it can reduce the preparation cost and preparation time of high-purity strontium carbonate, making it suitable for industrial production. Attached Figure Description

[0024] Figure 1This is a schematic flowchart of a desilication method for celestite ore according to this application. Detailed Implementation

[0025] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings, but the scope of protection of the present invention is not limited to the following description.

[0026] Example 1

[0027] Three celestite ore samples were randomly selected from a mine in Sichuan Province. The silicon and strontium content in these samples was analyzed using XRF, and the results are shown in Table 1. XRF detection procedure: 500g of each of the three samples was ground and passed through a 200-mesh sieve. The powder passing through the sieve was collected, pressed into tablets, and placed in the detection chamber of the detection equipment (Rigaku ZSX PrimusIII+ X-ray fluorescence spectrometer, Japan). The detection tube voltage was set to 50kV and the tube current to 60mA. After detection, the samples were recovered. The elemental content detection in subsequent embodiments followed the same procedure.

[0028] Table 1

[0029]

[0030] Example 2

[0031] Prepare refined celestite powder according to the following steps:

[0032] S1. Grinding operation: Select the celestite ore from Sample 1 in Example 1, grind it and pass it through a 400-mesh sieve. Collect the powder in the sieve and pass it through a 200-mesh sieve. Collect the powder that is sieved out to obtain celestite powder with a particle size of 40-75μm.

[0033] S2. Desilication process: Add 20 mL of 15 wt% hydrochloric acid to 10 g of the celestite powder, then add 6 g of ammonium fluoride solid and stir until dissolved. Perform desilication at 80°C for 60 min, then filter, wash three times with deionized water, and dry to obtain desilication celestite powder.

[0034] S3. Alkali washing operation: Add 10 mL of 20 wt% sodium hydroxide solution to the desilication celestite powder, perform alkali washing at 60℃ for 50 min, then filter, wash three times with deionized water and dry to obtain alkali washed celestite powder.

[0035] S4. Acid washing process: Add 30 mL of 45 wt% sulfuric acid solution to the alkaline-washed celestite powder, acid wash at 60°C for 50 min, then filter, wash three times with deionized water, and dry to obtain 9.71 g of refined celestite powder.

[0036] Example 3

[0037] Prepare refined celestite powder according to the following steps:

[0038] S1. Grinding operation: Select the celestite ore from Sample 2 in Example 1, grind it and pass it through a 400-mesh sieve. Collect the powder in the sieve and pass it through a 200-mesh sieve. Collect the powder that is sieved out to obtain celestite powder with a particle size of 40-75μm.

[0039] S2. Desilication process: Add 25 mL of 22 wt% hydrochloric acid to 10 g of the celestite powder, then add 2 g of ammonium fluoride solid and stir until dissolved. Perform desilication at 70°C for 50 min, then filter, wash three times with deionized water, and dry to obtain desilicationized celestite powder.

[0040] S3. Alkali washing operation: Add 8 mL of 30 wt% sodium hydroxide solution to the desilication celestite powder, perform alkali washing at 60°C for 55 min, then filter, wash three times with deionized water, and dry to obtain alkali-washed celestite powder.

[0041] S4. Acid washing process: Add 20 mL of 35 wt% sulfuric acid solution to the alkaline-washed celestite powder, acid wash at 75°C for 55 min, then filter, wash three times with deionized water, and dry to obtain 9.82 g of refined celestite powder.

[0042] Example 4

[0043] Prepare refined celestite powder according to the following steps:

[0044] S1. Grinding operation: Select the celestite ore from sample three in Example 1, grind it and pass it through a 400-mesh sieve. Collect the powder in the sieve and pass it through a 200-mesh sieve. Collect the powder that is sieved out to obtain celestite powder with a particle size of 40-75μm.

[0045] S2. Desilication process: Add 45 mL of 18.5 wt% hydrochloric acid to 30 g of the celestite powder, then add 12 g of ammonium fluoride solid and stir until dissolved. Perform desilication at 80°C for 55 min, then filter, wash three times with deionized water, and dry to obtain desilication celestite powder.

[0046] S3. Alkali washing operation: Add 42 mL of 25 wt% sodium hydroxide solution to the desilication celestite powder, perform alkali washing at 75°C for 60 min, then filter, wash three times with deionized water, and dry to obtain alkali-washed celestite powder.

[0047] S4. Acid washing operation: Add 80 mL of 40 wt% sulfuric acid solution to the alkaline-washed celestite powder, acid wash at 60°C for 60 min, then filter, wash three times with deionized water and dry to obtain 28.97 g of refined celestite powder.

[0048] Comparative Example 1

[0049] Prepare refined celestite powder according to the following steps:

[0050] S1. Grinding operation: The celestite ore of Sample 1 in Example 1 is ground and passed through a 400-mesh sieve. The powder in the sieve is collected and then passed through a 200-mesh sieve. The powder that is sieved out is collected to obtain celestite powder with a particle size of 40-75μm.

[0051] S2. Desilication process: Add 20 mL of 15 wt% hydrochloric acid to 10 g of the celestite powder, then add 6 g of ammonium fluoride solid and stir until dissolved. Perform desilication at 80°C for 60 min, then filter, wash three times with deionized water, and dry to obtain desilication celestite powder.

[0052] S3. Alkali washing operation: Add 10 mL of 20 wt% sodium hydroxide solution to the desilication celestite powder, perform alkali washing at 60℃ for 50 min, then filter, wash three times with deionized water and dry to obtain alkali washed celestite powder.

[0053] S4. Acid washing process: Add 30 mL of 15 wt% sulfuric acid solution to the alkaline-washed celestite powder, keep at 60°C for 50 min, then filter, wash three times with deionized water, and dry to obtain 9.87 g of refined celestite powder.

[0054] Comparative Example 2

[0055] Prepare refined celestite powder according to the following steps:

[0056] S1. Grinding operation: The celestite ore of Sample 1 in Example 1 is ground and passed through a 400-mesh sieve. The powder in the sieve is collected and then passed through a 200-mesh sieve. The powder that is sieved out is collected to obtain celestite powder with a particle size of 40-75μm.

[0057] S2. Desilication process: Add 20 mL of 15 wt% hydrochloric acid to 10 g of the celestite powder, then add 6 g of ammonium fluoride solid and stir until dissolved. Perform desilication at 80°C for 60 min, then filter, wash three times with deionized water, and dry to obtain desilication celestite powder.

[0058] S3. Alkali washing operation: Add 10 mL of 6 wt% sodium hydroxide solution to the desilication celestite powder, perform alkali washing at 60℃ for 50 min, then filter, wash three times with deionized water and dry to obtain alkali-washed celestite powder.

[0059] S4. Acid washing process: Add 30 mL of 45 wt% sulfuric acid solution to the alkaline-washed celestite powder, acid wash at 60°C for 50 min, then filter, wash three times with deionized water, and dry to obtain 9.74 g of refined celestite powder.

[0060] Comparative Example 3

[0061] Prepare refined celestite powder according to the following steps:

[0062] S1. Grinding operation: The celestite ore of Sample 1 in Example 1 is ground and passed through a 400-mesh sieve. The powder in the sieve is collected and then passed through a 200-mesh sieve. The powder that is sieved out is collected to obtain celestite powder with a particle size of 40-75μm.

[0063] S2. Desilication process: Add 20 mL of 15 wt% hydrochloric acid to 10 g of the celestite powder, then add 6 g of ammonium fluoride solid and stir until dissolved. Perform desilication at 80°C for 60 min, then filter, wash three times with deionized water, and dry to obtain desilication celestite powder.

[0064] S3. Alkali washing operation: Add 20 mL of 24 wt% ammonia solution to the desilication celestite powder, perform alkali washing at 60℃ for 50 min, then filter, wash three times with deionized water and dry to obtain alkali-washed celestite powder.

[0065] S4. Acid washing process: Add 30 mL of 45 wt% sulfuric acid solution to the alkaline-washed celestite powder, acid wash at 60°C for 50 min, then filter, wash three times with deionized water, and dry to obtain 9.72 g of refined celestite powder.

[0066] Comparative Example 4

[0067] Prepare refined celestite powder according to the following steps:

[0068] S1. Grinding operation: The celestite ore of Sample 1 in Example 1 is ground and passed through a 400-mesh sieve. The powder in the sieve is collected and then passed through a 200-mesh sieve. The powder that is sieved out is collected to obtain celestite powder with a particle size of 40-75μm.

[0069] S2. Desilication process: Add 20 mL of 15 wt% hydrochloric acid to 10 g of the celestite powder, then add 6 g of ammonium fluoride solid and stir until dissolved. Perform desilication at 80°C for 60 min, then filter, wash three times with deionized water, and dry to obtain desilication celestite powder.

[0070] S3. Alkali washing operation: Add 10 mL of 20 wt% sodium hydroxide solution to the desilication celestite powder, perform alkali washing at 60℃ for 50 min, then filter, wash three times with deionized water and dry to obtain alkali washed celestite powder.

[0071] S4. Acid washing process: Add 30 mL of 36 wt% hydrochloric acid solution to the alkaline-washed celestite powder, keep at 60°C for 50 min, then filter, wash three times with deionized water, and dry to obtain 7.18 g of refined celestite powder.

[0072] Experiment 1 verifies the silicon removal effect

[0073] The refined celestite powders obtained in Examples 2-4 and Comparative Examples 1-4 were analyzed using the XRF detection method described in Example 1 to obtain the final silicon content and final strontium content. The desilication rate and strontium loss rate were calculated. Then, 5g of the refined celestite powder obtained in Examples 2-4 or Comparative Examples 1-4 were weighed to prepare strontium carbonate. After adding 4.3g of ammonium carbonate solid (ammonium carbonate in excess), 15mL of deionized water was added, and the mixture was reacted at 75°C for 120min. The mixture was then filtered, washed three times with hot water, and dried to obtain strontium carbonate powder. The strontium carbonate content was detected according to the detection method in "HG / T 4508-2013 High Purity Strontium Carbonate", and the conversion rate during the preparation of strontium carbonate was calculated.

[0074] Desilication rate (%) = (m 原料 ×Wt 硅原料 -m 精制粉末 ×Wt 硅精制粉末 ) / m 原料 ×Wt 硅原料

[0075] Strontium loss rate (%) = (m 原料 ×Wt SrO原料 -m 精制粉末 ×Wt SrO精制粉末 ) / m 原料 ×Wt SrO原料

[0076] Carbonic acid conversion rate: = m 实际碳酸锶 / m 理论碳酸锶 (m 理论碳酸锶 It can be calculated from the chemical reaction SrSO4 + CO2-3 = SrCO3 + SO2-4.

[0077] Table 2

[0078]

[0079] The results show that the desilication method for celestite ore provided in this application can achieve a desilication rate of over 97.5%, and can control the strontium loss rate to below 1.7% during desilication, effectively control the residual fluorine element, and ensure that the desilication celestite has a conversion rate of over 90% in the subsequent preparation of strontium carbonate. It is a celestite desilication method with great industrial value.

[0080] The above description is merely a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the concept described herein through the above teachings or related technologies or knowledge. Modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.

Claims

1. A method for desilication of celestite ore, characterized in that, Includes the following steps: S1. Grinding operation: Celestite ore is ground and then sieved to obtain celestite powder; S2. Desilication process: Hydrochloric acid solution and ammonium fluoride are added to the celestite powder, and after desilication, first filtration, first washing and first drying, desilication celestite powder is obtained. S3. Alkali washing operation: Add sodium hydroxide solution to the desilication celestite powder, and perform alkali washing, second filtration, second washing and second drying to obtain alkali-washed celestite powder. S4. Acid washing operation: Add sulfuric acid solution to the alkaline washed celestite powder, and perform acid washing, third filtration, third washing and third drying to obtain refined celestite powder. The weight ratio of the celestite powder to the ammonium fluoride is 1:(0.20~0.6).

2. The desilication method according to claim 1, characterized in that, The particle size of the celestite powder is 40~75 μm.

3. The desilication method according to claim 1, characterized in that, The concentration of the hydrochloric acid solution is 15~22 wt%.

4. The desilication method according to claim 1, characterized in that, The concentration of the sodium hydroxide solution is 20-30 wt%.

5. The desilication method according to claim 1, characterized in that, The concentration of the sulfuric acid solution is 35-45 wt%.

6. The desilication method according to claim 1, characterized in that, The solid-liquid ratio of the celestite powder, the hydrochloric acid solution, the sodium hydroxide solution, and the sulfuric acid solution is 1:(1.5~2.5):(0.8~1.4):(2~3).

7. The desilication method according to claim 1, characterized in that, The desilication temperature is 70~80℃, and the desilication time is 50~60 min.

8. The desilication method according to claim 1, characterized in that, The alkaline washing temperature is 60~75℃, and the alkaline washing time is 50~60 min.

9. The desilication method according to claim 1, characterized in that, The pickling temperature is 60~75℃, and the pickling time is 50~60 min.

Citation Information

Patent Citations

  • Method for producing less-barium fine strontium salts from celestite

    CN102602974A