Organic phosphate radical intercalation layered metal hydroxide flame-retardant smoke-suppression hybrid material as well as preparation method and application of organic phosphate radical intercalation layered metal hydroxide flame-retardant smoke-suppression hybrid material

By introducing organic phosphate intercalated layered metal hydroxide into the TPU material, the problems existing in TPU materials are solved by the flammability of TPU materials and traditional LDH flame retardant smoke inhibitors are achieved, and the synchronous improvement of high-efficiency flame retardant and smoke inhibition are achieved and the environmental protection of the material is achieved.

CN120005282AActive Publication Date: 2025-05-16UNIV OF SCI & TECH OF CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510284698.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-11
Publication Date
2025-05-16
Estimated Expiration
2045-03-11

AI Technical Summary

Technical Problem

The existing thermoplastic polyurethane (TPU) materials are flammable and release a large amount of thick smoke and toxic gases during combustion. In addition, traditional layered bimetallic hydroxide (LDH) flame retardant and smoke inhibitors have problems with single cation types, anionic functional fragmentation and structural-function imbalance, making it difficult to achieve synchronous improvement of efficient flame retardant and smoke inhibition.

Method used

Through cationic regulation and organophosphate intercalation, a new flame-retardant smoke-retardant hybrid material with smoke-retardant structure was constructed, and the organic phosphate intercalation layered metal hydroxide was prepared by hydrothermal in-situ intercalation method, which was added to the TPU as an additive to improve its flame-retardant and smoke-retardant properties.

Benefits of technology

Low addition amount and high smoke-resistance and flame retardant efficiency are achieved, which significantly reduces smoke toxicity (64% reduction in CO production), and optimizes process economy and mechanical properties, so that the materials are pollution-free to the environment and the human body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120005282A_ABST
    Figure CN120005282A_ABST
Patent Text Reader

Abstract

The invention discloses an organic phosphate radical intercalation layered metal hydroxide flame-retardant smoke-suppression hybrid material as well as a preparation method and application thereof. The invention provides an organic phosphate radical intercalation layered metal hydroxide flame-retardant and smoke-suppressing hybrid material aiming at the problems of single component limitation, function imbalance and poor process economy of a traditional layered metal hydroxide smoke suppressant. Aiming at the problems that traditional LDH is not uniformly dispersed in a polymer matrix and the mechanical property is reduced, the flame-retardant smoke-suppression hybrid material with a novel smoke-suppression-flame-retardant structure is constructed through cation regulation and organic phosphate radical intercalation. Through theoretical calculation and performance analysis, a polymer material with a novel smoke suppression-flame retardant structure is constructed through interface regulation and control, and the polymer material is applied to a processing process in a polymer matrix, so that excellent flame retardant, smoke suppression and toxicity reduction effects are achieved, and meanwhile, no pollution is caused to the environment and human bodies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of flame retardant materials, and in particular relates to an organic phosphate intercalated layered metal hydroxide flame retardant and smoke suppression hybrid material and a preparation method and application thereof. Background Art

[0002] Thermoplastic polyurethane (TPU) is widely used in wire and cable sheaths, automotive interiors, electronic equipment, and medical devices due to its excellent wear resistance, high elasticity, and processing performance. However, as a polymer material, TPU's limiting oxygen index (LOI) is usually less than 20%, which makes it a flammable material. During combustion, it releases a large amount of smoke and toxic gases (such as carbon monoxide, hydrogen cyanide, nitrogen oxides, etc.). Especially in confined spaces or high-density electrification scenarios (such as underground rail transit and data centers), the burning smoke of TPU materials will seriously hinder the escape of personnel, aggravate fire hazards, and cause persistent pollution to the environment. Therefore, the development of TPU composite materials with both high-efficiency flame retardant and smoke suppression functions has become an urgent need to ensure public safety and meet environmental protection regulations.

[0003] In order to ensure industrial safety and ecological environment, the development of thermoplastic polyurethane (TPU) composite materials with both efficient flame retardant and smoke suppression properties has become a key issue. In the relevant technical field, layered double hydroxide (LDH) is regarded as an ideal candidate system for environmentally friendly flame retardant and smoke suppression materials due to its unique controllable layer structure and thermal decomposition and heat absorption characteristics. In the future, the development of environmentally friendly halogen-free and highly efficient TPU smoke suppression technology will be a research hotspot, and we will continue to explore more environmentally friendly and efficient methods, and widely apply them in fields such as intelligent manufacturing and sustainable development.

[0004] In recent years, the research on LDH flame retardant and smoke suppression TPU can be divided into three types: LDH and traditional flame retardants (such as ammonium polyphosphate, diethyl aluminum hypophosphite) synergistic flame retardant and smoke suppression TPU (Polym. Degrad. Stab, 2022, 202: 110043.Polym. Degrad. Stab, 2019, 165: 126-136.), LDH and high-efficiency phosphorus-containing flame retardants (such as DOPO, PEI) synergistic flame retardant and smoke suppression TPU (Appl. Clay Sci., 2024, 258: 107489. Polym. Degrad. Stab, 2020,178: 109179.), LDH and inorganic sheet materials (such as Mxene, MoS2) synergistic flame retardant and smoke suppression TPU (J. Polym. Sci., 2024, 62(24): 5693-5705.、Constr. Build. Mater., 2024, 457: 139478.). However, there are still some problems in the application of traditional LDH flame retardant and smoke suppressant. In the prior art, many studies have been conducted to improve the flame retardant properties of LDH by regulating the cationic composition or anionic intercalation of LDH, but there are still significant defects:

[0005] Single cation type: Traditional LDH mostly uses 2-3 metal combinations (such as Mg-Al, Zn-Fe), and the charge density distribution of the layer is uneven, which limits the free radical capture efficiency and toxic gas adsorption capacity;

[0006] Anion function separation: conventional intercalated anions (NO3⁻, CO3²⁻, etc.) only play a physical barrier or gas phase dilution role, lacking a chemical synergistic mechanism with flame retardant and smoke suppression active components;

[0007] Structural-functional imbalance: Cation regulation and anion intercalation are mostly isolated optimizations, and the simultaneous improvement of flame retardancy and smoke suppression performance cannot be achieved through the electronic coupling effect between ions.

[0008] Among them, anionic phosphate intercalated layered metal hydroxide (CN110218508A) is used as a flame retardant material. The phosphate intercalation technology aims to improve the flame retardant properties of epoxy acrylate flame retardant materials and also improve their mechanical properties. However, the flame retardant properties of the material are reduced to a low degree in this work, and there is a lack of characterization and research on smoke, and there are deficiencies in the research on the material. Organic phosphate intercalated layered metal hydroxide (CN115926812A) is used as a composite flame retardant material for electrodes. Although organic phosphate is still used as an additive material for layered metal hydroxide as a battery separator or negative electrode, when the flame retardant material is added, the oxygen index of the composite material is less improved, and most of the matrix materials are still at the standard of combustible materials. At the same time, the flame retardant and smoke performance are not specifically analyzed and characterized. The mass of flame retardant added to the composite material is large (30%-50%), and there is a large gap in mechanical properties. The mechanism and role of organic phosphate are not clearly explained. Although there have been many studies on composite organic acid intercalated layered metal hydroxides as flame retardant materials, there is still a lack of research on their flame retardant applications in high-performance TPU materials. It is of great research value to design an organic phosphate intercalated layered metal hydroxide as a smoke suppression and toxicity reduction hybrid material with low addition and high flame retardant and smoke suppression efficiency for TPU. Summary of the invention

[0009] In view of the problems existing in the above-mentioned prior art, the present invention provides an organic phosphate intercalated layered metal hydroxide flame retardant and smoke suppression hybrid material and a preparation method and application thereof.

[0010] The present invention constructs a flame retardant and smoke suppression hybrid material with a novel smoke suppression and flame retardant structure through cation regulation and organic phosphate intercalation, and uses it in a processing process in a polymer matrix to obtain excellent flame retardant and smoke suppression and toxic reduction effects, while also being non-polluting to the environment and human body. The smoke suppression and toxic reduction composite material preparation process of the present invention has low cost, simple and green operation, strong controllability, and can be prepared in batches.

[0011] The preparation method of the flame retardant and smoke suppressing hybrid material of the organic phosphate intercalated layered metal hydroxide of the present invention adopts a hydrothermal in-situ intercalation method, and comprises the following steps:

[0012] Step 1: Mix a divalent metal salt and a trivalent metal salt and dissolve them in deionized water, add a precipitant and an organic phosphate compound, and stir continuously at a temperature range of 25-30° C. to mix them evenly to obtain a suspension.

[0013] Step 2: Transfer the suspension obtained in step 1 to a high-pressure reactor, perform a hydrothermal reaction at 100° C.-150° C., filter to obtain a precipitated product, wash with ethanol and deionized water, and dry to obtain an organophosphate intercalated LDH hybrid material.

[0014] In step 1, the metal active components in the divalent metal salt and the trivalent metal salt include one or more of iron, cobalt, nickel, copper, and magnesium. The total metal salt content is 0.5-1 mol / L. The content of organic phosphate is 0.4-2 mol / L.

[0015] Furthermore, in the divalent metal salt and the trivalent metal salt, the molar ratio of the divalent metal to the trivalent metal is 2:1 to 3:1, such as 2:1, 2.5:1, 3:1.

[0016] Furthermore, the divalent metal is Ni 2+ 、Co 2+ , Cu 2+ Mg 2+ One or more of the following, the trivalent metal is Fe 3+ .

[0017] The precipitant is a triethanolamine aqueous solution, and the molar ratio of the precipitant addition amount to the metal salt is between 2:1 and 4:1.

[0018] The organic phosphate compound is phenylphosphite (PPA) or diphenylphosphonic acid (DPA), and the molar ratio of the organic phosphate to the metal salt is between 1:2 and 1:2.

[0019] In the flame-retardant and smoke-suppressing hybrid material of the organic phosphate intercalated layered metal hydroxide of the present invention, the layered metal hydroxide presents a stacked sheet, whisker or rod-like structure, and the particle size is 30nm-2μm.

[0020] The application of the flame retardant and smoke suppression hybrid material of the organic phosphate intercalated layered metal hydroxide of the present invention is to add the organic phosphate intercalated layered metal hydroxide as an auxiliary agent into thermoplastic polyurethane to improve the flame retardant and smoke suppression properties of the material.

[0021] Furthermore, when the organic phosphate intercalated layered metal hydroxide is added as an additive to thermoplastic polyurethane, a melt blending method is used to construct a TPU composite material, comprising the following steps:

[0022] (1) The TPU masterbatch is dried in an oven to remove moisture.

[0023] (2) The dried TPU masterbatch is added into an internal mixer for melting, and the organic phosphate intercalated LDH hybrid material is added and mixed evenly to obtain a TPU composite material.

[0024] (3) The TPU composite material is hot pressed on a flat vulcanizer to obtain a regular sheet.

[0025] Furthermore, the addition amount of the organic phosphate intercalated LDH hybrid material is 1-3wt% of the total mass of the polymer composite material.

[0026] In the scheme of the present invention:

[0027] Cationic multivariate design: introduction of Fe 3+ / Cu 2+ / Co 2+ / Ni 2+ / Mg 2+ Multivalent metals such as 2-Hydroxy-2-nitrogen (2-Hydroxy-2-nitrogen) and 2-Hydroxy-2-nitrogen (2-Hydroxy-2-nitrogen) are used to construct high charge density layers to enhance the free radical quenching and acid gas (HCl, HCN) chemical adsorption capabilities.

[0028] Anion functionalized intercalation: Organic phosphate intercalation is used. Its abundant phosphate groups not only increase the residual carbon rate (>35%) by catalyzing carbonization, but also form POM covalent bonds with multi-metal cations to stabilize the laminate structure (thermal stability>400℃).

[0029] Ion synergy: The multi-metal cations and organic phosphate anions in the laminate are constructed through charge matching and electron transfer channels to achieve a dual flame retardant and smoke suppression mechanism of condensed phase carbonization and gas phase free radical inhibition, significantly reducing smoke toxicity (CO generation is reduced by 64%).

[0030] In view of the problems of high cost, high toxicity, poor flame retardancy, etc. of current thermoplastic polyurethane materials, the present invention provides an organic phosphate intercalated layered metal hydroxide flame retardant and smoke suppression hybrid material and its preparation method and application. In the present invention, unlike traditional flame retardants containing a large amount of toxic elements, which may have a negative impact on the environment and health, a large amount of toxic gases may be released during fire combustion. In view of the problems of traditional LDH, the present invention focuses on the dual requirements of flame retardant performance optimization and low smoke and low toxicity, achieves multiple effects of process economy and mechanical performance optimization, and completes the balancing process of synergistic flame retardancy, smoke suppression and other properties.

[0031] The beneficial effects of the present invention are embodied in:

[0032] 1. The present invention aims to solve the problems of traditional LDH, such as the limitation of component singleness, functional imbalance and poor process economy, and provides a flame retardant and smoke suppression hybrid material of organic phosphate intercalated layered metal hydroxide. Through surface reconstruction and metal element regulation, the formation of defect sites and lattice oxidation in LDH are promoted, and the changing law of the influence of LDH on polymer combustion heat release and smoke toxicity is revealed. Molecular dynamics and theoretical analysis methods are used to effectively predict the distance between LDH anion layers and intercalation structure, and the breakage and recombination of groups during the combustion process are deeply analyzed. Through efficient synergistic flame retardancy, it is used to prepare polyurethane composite materials, achieving low addition amount and high smoke suppression-flame retardant efficiency.

[0033] 2. The present invention prepares composite materials by a one-step hydrothermal method, with a short process route, cheap raw materials and no flammable and explosive reagents involved, a controllable process, and high precision in metal ratio regulation, which has great reference significance for industrial production. It is used in the processing and production of thermoplastic polyurethane elastomers to achieve the dual requirements of efficient flame retardant optimization and low smoke and low toxicity, and achieve multiple effects of process economy and mechanical property optimization, and is safe and environmentally friendly, can reduce environmental pollution, and can be used in practical applications.

[0034] 3. The preparation process of the present invention is easy to operate, green, low in production cost, simple in process, and high in efficiency. Through theoretical calculation and performance analysis, a new type of smoke-suppressing and flame-retardant polymer material is constructed through interface regulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0037] Figure 1 The scanning electron microscope images of Ni-Fe LDH prepared by different preparation methods in Examples 1-4. Among them: a is a scanning electron microscope image of Ni-Fe LDH prepared by triethanolamine as a precipitant in Example 1, which is a stacked small lamellar structure with a size of 20-50nm (a1 and a2 are different magnification scales); b is a stacked whisker structure of Ni-Fe LDH prepared by urea as a precipitant in Example 2, with a size of 500nm-1μm (b1 and b2 are different magnification scales); c is a stacked rod-like structure of Ni-Fe LDH after freeze-drying by coprecipitation method in Example 3, with a size of 1μm-5μm (c1 and c2 are different magnification scales); d is a stacked particle structure of Ni-Fe LDH after oven drying by coprecipitation method in Example 4, with a size of 50nm-100nm (d1 and d2 are different magnification scales). In the preferred embodiment 1, the Ni-Fe LDH prepared by using triethanolamine as a hydrothermal precipitant was subjected to subsequent experiments, and the stacked small sheet structure was the optimized structure of LDH.

[0038] Figure 2The scanning electron microscope images of Ni-Fe LDH prepared by reactants of different ratios in Example 5. Among them: a, b are morphological images of LDH when the metal salt Ni:Fe is 1:4, and the LDH material is an independent spherical structure; c, d are morphological images of LDH when the metal salt Ni:Fe is 1:3, and the LDH material is an irregular spherical structure with certain adhesion; e, f are morphological images of LDH when the metal salt Ni:Fe is 1:2, and the LDH material is an adhesion spherical structure; g, h are morphological images of LDH when the metal salt Ni:Fe is 1:1, and the LDH material is an adhesion irregular spherical structure; i, j are morphological images of LDH when the metal salt Ni:Fe is 2:1, and the LDH material is an adhesion small lamellar structure; k, l are morphological images of LDH when the metal salt Ni:Fe is 3:1, and the LDH material is a large number of adhesion small lamellar structures; the preferred reactant ratio Ni:Fe is 2:1 for subsequent experiments to ensure the lamellar structure of LDH.

[0039] Figure 3 The scanning electron microscope images of Ni-Fe LDH prepared at different hydrothermal reaction temperatures in Example 6. Among them: a, b are scanning electron microscope images of Ni-Fe LDH prepared at a hydrothermal temperature of 60°C, and the sample is an irregular small lamellar structure; c, d are scanning electron microscope images of Ni-Fe LDH prepared at a hydrothermal temperature of 90°C, and the sample is a stacked small lamellar structure; e, f are scanning electron microscope images of Ni-Fe LDH prepared at a hydrothermal temperature of 110°C, and the sample is a stacked large lamellar structure; g, h are scanning electron microscope images of Ni-Fe LDH prepared at a hydrothermal temperature of 130°C, and the sample is a stacked rod-like structure; the hydrothermal temperature is preferably 110°C for subsequent experiments to ensure the lamellar structure of LDH.

[0040] Figure 4The thermogravimetric temperature curve of Ni-Fe LDH prepared in the preferred embodiment 1 and the corresponding scanning electron microscope images at different thermogravimetric temperatures. Wherein: a is the thermogravimetric temperature and derivative thermogravimetric analysis curve of Ni-Fe LDH in a nitrogen environment. It can be seen from the figure that LDH has multiple weight loss peaks, indicating that the material itself has different substances removed under thermal heating conditions, corresponding to the removal of adsorbed H2O, the removal of interlayer CO2, the removal of interlayer H2O, and the formation of metal oxides. b is a SEM image of the morphology of LDH, and c is a SEM image of LDH corresponding to the weight loss peak at about 100°C, corresponding to the removal of adsorbed H2O, and the material is still a small lamellar structure. d is the SEM image of the weight loss peak of Ni-Fe LDH at about 300℃-380℃, corresponding to the removal of interlayer CO2, and the small flakes of the material gradually agglomerate; i is the SEM image of the weight loss peak of Ni-Fe LDH at about 380℃-460℃, corresponding to the removal of interlayer H2O, and the material begins to form metal oxides; j is the SEM image of the weight loss peak of Ni-Fe LDH at about 600℃, corresponding to the complete generation of metal oxides, and the metal particles continue to agglomerate. e, f are transmission electron microscopy images of the morphology of LDH, and the material is a small flake structure; g, h are transmission electron microscopy images of the morphology of LDH after thermogravimetric testing, and the material is an agglomerated particle structure.

[0041] Figure 5 The SEM-EDS mapping diagram of the Ni-Fe LDH prepared in the preferred embodiment 1. Wherein: a, b are the structural SEM images of the material itself, c, d, e are the SEM-EDS mapping diagrams of the Ni-Fe LDH, corresponding to the elements C, Ni and Fe, respectively.

[0042] Figure 6 N2 adsorption-desorption diagram and pore size distribution diagram of Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Mg-Fe LDH prepared in Example 1 and Examples 7-9.

[0043] Figure 7 XPS spectra of Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Mg-Fe LDH prepared in Example 1 and Examples 7-9.

[0044] Figure 8 FT-IR spectra of Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Mg-Fe LDH prepared in Example 1 and Examples 7-9.

[0045] Fig. 9 Thermogravimetric temperature curves of Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Mg-Fe LDH prepared in Example 1 and Examples 7-9.

[0046] Fig.10 These are the microcalorimetric test results of the materials after the Ni-Fe LDH / PPA prepared in Example 10 was compounded with TPU in different proportions; the peak heat release of the material with an addition amount of 3wt% was the lowest, and the addition amount of 3wt% was preferred for the test study.

[0047] Fig.11 The cone calorimeter test results of the materials after the Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Mg-FeLDH prepared in Examples 1 and Examples 7-9 were compounded with TPU at 35kW; a is the heat release rate curve of the material, b is the total heat release curve, c is the smoke release rate curve, d is the total smoke release curve, e is the CO generation rate curve, and f is the CO2 generation rate curve; the addition effect of Ni-Fe LDH is the best, with the peak heat release reduced by up to 21.4% and the total heat release reduced by up to 36.8%. Ni-Fe LDH is preferred for organic acid and intercalation research.

[0048] Fig.12 This is a prediction and analysis diagram of the decomposition reaction pathway of organic phosphate.

[0049] Fig.13 Figure 2 is a N2 adsorption-desorption diagram of Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Examples 10 and 11.

[0050] Fig.14 FT-IR spectra of Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Examples 10 and 11.

[0051] Fig.15 Cone calorimeter test results of the materials after Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Examples 10 and 11 were composited with TPU at 35kW; a is the heat release rate curve of the material, b is the total heat release curve, c is the smoke release rate curve, d is the total smoke release curve, e is the CO generation rate curve, and f is the CO2 generation rate curve; after organic acid intercalation of Ni-Fe LDH, the heat release and smoke release of the composite material are further reduced, among which Ni-Fe LDH / PPA / TPU has the highest effect, with the peak heat release reduced by up to 38.58% and the total smoke release reduced by up to 38.78%, indicating that the fire safety performance of the material is further improved after organic acid intercalation with PPA.

[0052] Fig.16The combustion smoke density test results of the materials prepared in Examples 10 and 11 after Ni-Fe LDH / PPA and Ni-Fe LDH / DPA were compounded with TPU at 25kW; a is the smoke density curve of the material, b is the bar graph of the maximum smoke release, and c is the bar graph of the time to reach the maximum smoke release. Before intercalation, the addition of Ni-Fe LDH reduced the smoke density of the material to a certain extent, by 10.6%; after the material was intercalated, the smoke density of the composite material was significantly reduced, and the intercalation effect of DPA was the best, which greatly reduced the smoke density of the composite material (63.9%), reflecting the excellent smoke suppression effect of Ni-Fe LDH / DPA on TPU material.

[0053] Fig.17 Scanning electron microscope images of carbon residues after combustion of the materials after Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Examples 10 and 11 were compounded with TPU. a, b and c are SEM images of carbon residues after combustion of TPU, and the carbon residues are loose and broken; c, d and e are SEM images of carbon residues after combustion of Ni-Fe LDH / TPU, and the carbon residues are more compact; g, h and i are SEM images of carbon residues after combustion of Ni-Fe LDH / PPA / TPU, and the carbon residues become loose and complete; j, k and l are SEM images of carbon residues after combustion of Ni-Fe LDH / DPA / TPU, and the carbon residues become loose and complete. The looseness of the material proves that the intercalated Ni-Fe LDH has an inhibitory effect on the combustion of TPU, and the loose and complete carbon layer is conducive to the inhibition of material combustion and has a certain barrier effect.

[0054] Fig.18 The tensile performance diagram of the materials after the Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Examples 10 and 11 were compounded with TPU. a is the tensile performance diagram, b is the maximum tensile strength, and c is the elongation at break. The addition of Ni-Fe LDH has a significant reduction in the mechanical properties of TPU due to the uneven distribution of the material. After the organic acid root intercalation of Ni-Fe LDH, due to the presence of organic ions, the interface properties of the material are optimized through organic-inorganic interaction, which in turn improves the mechanical properties of TPU to a certain extent. DETAILED DESCRIPTION

[0055] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0056] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0057] During the experiment, the present invention firstly prepares layered metal hydroxides by hydrothermal method and co-precipitation method, and then screens out suitable reaction methods and reaction conditions by comparing and optimizing the morphologies of different methods, and then further in-situ intercalates with organic phosphate.

[0058] The specific steps include:

[0059] S1. preparing layered metal hydroxide by combining coprecipitation method and hydrothermal method;

[0060] S11. Select different preparation methods (co-precipitation method and hydrothermal method) to prepare LDH. For the hydrothermal method, triethanolamine or urea is selected as the precipitant, and for the co-precipitation method, sodium carbonate is selected as the precipitant.

[0061] S12. The preparation method of the hydrothermal method is: mix nickel chloride and ferric chloride (the molar ratio of divalent metal salt to trivalent metal salt in the metal active component is 2:1-3:1, and the total metal salt content is 0.1-0.2 mol) and dissolve in deionized water; use triethanolamine aqueous solution as a hydrothermal precipitant to add to the metal precursor aqueous solution, and stir continuously in the temperature range of 25-30°C to mix evenly; illustratively, the nickel chloride is 0.09 mol and the ferric chloride is 0.06 mol.

[0062] S13, transferring the suspension to a high-pressure reactor, and performing a hydrothermal reaction at 100° C.-150° C. Filtering to obtain a precipitated product, washing with ethanol and deionized water, collecting to obtain a precipitated product, and drying the precipitated product in a forced air oven to obtain Ni-Fe LDH.

[0063] S14. The preparation method of the coprecipitation method is: nickel chloride and ferric chloride (the molar ratio of divalent metal salt to trivalent metal salt in the metal active component is 2:1-3:1, and the total metal salt content is 0.1-0.2 mol) are mixed and dissolved in deionized water, and stirred continuously in the temperature range of 25-30°C to mix evenly; sodium carbonate aqueous solution is added to the metal precursor aqueous solution as a coprecipitation precipitant (the concentration of sodium carbonate solution is 0.5-1 mol / L), and the drop rate is 1d / s until the pH of the suspension reaches 10, and the pH of the suspension is kept stable in the temperature range of 25-30°C, and stirred for 1-2h. The precipitated product is filtered, washed with ethanol and deionized water, and the precipitated product is collected, and the precipitated product is placed in a blast oven to dry to obtain Ni-FeLDH. For example, the nickel chloride is 0.8 mol, the ferric chloride is 0.6 mol, and the concentration of the sodium carbonate solution is 1 mol / L.

[0064] The preparation methods of S15, Mg-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Ni-Fe LDH are similar, but the selected metals are somewhat different. Mg-Fe LDH selects Mg and Fe; Co-Fe LDH selects Co and Fe; Cu-Fe LDH selects Cu and Fe.

[0065] S2. Use phosphorus-containing organic acid to in-situ intercalate LDH to obtain organic acid intercalated LDH.

[0066] S21. Organic phosphates such as phenylphosphite (PPA) or diphenylphosphonic acid (DPA) will be in situ intercalated into layered metal hydroxides prepared by hydrothermal method.

[0067] S22. Mix nickel chloride and ferric chloride (the molar ratio of divalent metal salt to trivalent metal salt in the metal active component is 2:1-3:1, and the total metal salt content is 0.1-0.2 mol) and dissolve them in deionized water; use an aqueous solution containing organic phosphoric acid, phenylphosphite (PPA) and triethanolamine as a hydrothermal precipitant to add to the metal precursor aqueous solution, and stir continuously in the temperature range of 25-30°C to mix evenly; illustratively, the nickel chloride is 0.8 mol, the ferric chloride is 0.6 mol, and the phenylphosphite is 0.6 mol.

[0068] S23, transferring the suspension to a high-pressure reactor, and performing a hydrothermal reaction at 100° C.-150° C. Filtering to obtain a precipitated product, washing with ethanol and deionized water, collecting to obtain a precipitated product, and drying the precipitated product in a forced air oven to obtain Ni-Fe / PPA LDH.

[0069] The preparation methods of S24, DPA intercalated Ni-Fe-LDH and PPA intercalated Ni-Fe-LDH are similar. The selected organic phosphate is replaced by diphenylphosphoric acid (DPA) from phenyl hypophosphorous acid (PPA) to prepare DPA intercalated Ni-Fe-LDH, which is recorded as Ni-Fe / DPA LDH.

[0070] The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0071] Embodiment 1:

[0072] Chloride salts of different metal precursors are selected to prepare layered metal hydroxides (LDH). Taking the hydrothermal method to prepare Ni-FeLDH as an example, the metal salt precursors include nickel chloride hexahydrate and ferric chloride nonahydrate.

[0073] 1. Mix hexahydrate and nickel chloride, nonahydrate and ferric chloride in a certain ratio (in the metal cation active component, the molar ratio of nickel chloride to ferric chloride is 2:1, and the total metal salt content is 0.15 mol), dissolve in 200 ml of deionized water, and stir continuously to mix evenly. The stirring rate is 300 rpm, the stirring temperature is 25°C, and the stirring time is 1 hour. The mixed solution is recorded as solution A.

[0074] 2. Dissolve 15 g of triethanolamine in 100 ml of deionized water, stirring at 300 rpm, 25°C, and 0.5 h. The mixed solution is recorded as solution B.

[0075] 3. Slowly add solution B to solution A for mixing, with a stirring rate of 300 rpm, a stirring temperature of 25°C, and a stirring time of 1 h. Transfer the mixed solution to a Teflon-lined stainless steel autoclave and perform a hydrothermal reaction at 110°C for 12 hours. After the hydrothermal reaction, collect the precipitated product by centrifugation, wash with ethanol and deionized water until the pH is approximately equal to 7, the centrifugal speed is 6000 rpm, the centrifugal time is 5 min, collect the precipitated product, and place it in a blast oven to dry for 12 hours at 60°C. Obtain Ni-Fe LDH.

[0076] Embodiment 2:

[0077] Example 2 is basically the same as Example 1, the main difference being that the hydrothermal precipitant is different, the hydrothermal precipitant is changed to urea, and the synthesis is performed by changing the precipitant according to the stoichiometric ratio. The metal salt precursor includes hexahydrate and cobalt chloride and nonahydrate and ferric chloride. Ni-Fe LDH is prepared.

[0078] Embodiment 3:

[0079] The Ni-Fe LDH is prepared by a co-precipitation method, wherein the metal salt precursors include nickel chloride hexahydrate and ferric chloride nonahydrate, and sodium carbonate is selected as a precipitant in the co-precipitation method.

[0080] 1. Mix hexahydrate and nickel chloride, nonahydrate and ferric chloride in a certain ratio (in the metal cation active component, the molar ratio of nickel chloride to ferric chloride is 2:1, and the total metal salt content is 0.15 mol), dissolve in 200 ml of deionized water, and stir continuously to mix evenly. The stirring rate is 300 rpm, the stirring temperature is 25°C, and the stirring time is 1 hour. The mixed solution is recorded as solution A.

[0081] 2. Dissolve sodium carbonate in deionized water at a stirring rate of 300 rpm, a stirring temperature of 25°C, a stirring time of 0.5 h, and a concentration of 1 mol / L of the sodium carbonate solution. The mixed solution is recorded as solution B.

[0082] 3. Slowly add solution B to solution A for coprecipitation reaction, with a drop rate of 1d / s, until the pH of the suspension reaches 10, the stirring rate is 300rpm, the stirring temperature is 25℃, the pH of the suspension remains stable, and stirring is continued for 2h. Filter the precipitated product, wash with ethanol and deionized water until the pH of the filtrate is approximately equal to 7, and collect the precipitated product. Evenly mix the precipitated product with 10ml of deionized water, prefreeze the suspension in a -40℃ refrigerator for 12h, and freeze-dry the frozen suspension in a freeze dryer for 48h. The vacuum degree of the freeze dryer is 10 -3 Pa, Ni-Fe LDH was obtained.

[0083] Embodiment 4:

[0084] Example 4 is basically the same as Example 3, the main difference being that the drying method of the coprecipitation method is different. The drying method of the precipitate product prepared by the coprecipitation method is changed from freeze drying to oven drying. The precipitate product is placed in a forced air oven and dried for 12 hours at a temperature of 60° C. Ni-Fe LDH is obtained.

[0085] Embodiment 5:

[0086] Example 5 is basically the same as Example 1, the main difference being that the ratio of the metal salt precursor reactants is different. The ratio of the metal salt precursor is changed from 2:1 to 3:1, 1:1, 1:2, 1:3 and 1:4, and the synthesis is performed by changing the metal salt according to the stoichiometric ratio. The metal salt precursor includes hexahydrate and cobalt chloride and nonahydrate and ferric chloride. Ni-Fe LDH with different reactant ratios is prepared.

[0087] Embodiment 6:

[0088] Example 6 is basically the same as Example 1, the main difference being that the hydrothermal reaction temperature is different, the hydrothermal reaction temperatures are 60°C, 90°C, 110°C and 130°C, respectively, and the hydrothermal reaction time is the same. The metal salt precursor includes hexahydrate and cobalt chloride and nonahydrate and ferric chloride. Ni-Fe LDH with different reactant ratios is prepared.

[0089] Embodiment 7:

[0090] Example 7 is basically the same as Example 1, the main difference being that the metal salt precursor is different to a certain extent, and the synthesis is performed by changing the metal salt according to the stoichiometric ratio. The metal salt precursor includes hexahydrate and cobalt chloride and nonahydrate and ferric chloride. Co-Fe LDH is prepared.

[0091] Embodiment 8:

[0092] Example 8 is basically the same as Example 1, the main difference being that the metal salt precursor is different to a certain extent, and the synthesis is performed by changing the metal salt according to the stoichiometric ratio. The metal salt precursor includes dihydrate and copper chloride and nonahydrate and ferric chloride. Cu-Fe LDH is prepared.

[0093] Embodiment 9:

[0094] Example 9 is basically the same as Example 1, the main difference being that the metal salt precursor is different to a certain extent, and the synthesis is performed by changing the metal salt according to the stoichiometric ratio. The metal salt precursor includes hexahydrate and magnesium chloride and nonahydrate and ferric chloride. Mg-Fe LDH is prepared.

[0095] Embodiment 10:

[0096] Phosphorus-containing organic acid was selected to intercalate Ni-Fe LDH to achieve high flame retardancy and tensile properties, and phenylphosphite (PPA) was selected to perform in-situ intercalation experiments on Ni-Fe LDH. Metal salt precursors include nickel chloride hexahydrate and ferric chloride nonahydrate.

[0097] 1. Mix hexahydrate and nickel chloride, nonahydrate and ferric chloride in a certain ratio (in the metal cation active component, the molar ratio of nickel chloride to ferric chloride is 2:1, and the total metal salt content is 0.15 mol), dissolve in 200 ml of deionized water, and stir continuously to mix evenly. The stirring rate is 300 rpm, the stirring temperature is 25°C, and the stirring time is 1 hour. The mixed solution is recorded as solution A.

[0098] 2. Dissolve 15g of triethanolamine in 100ml of deionized water, add phenylphosphite PPA (phenylphosphite to LDH metal molar ratio is 0.5-2), stir at 300rpm, stir at 25℃, and stir for 1h. The mixed solution is recorded as solution B.

[0099] 3. Slowly add solution B to solution A for mixing, with a stirring rate of 300 rpm, a stirring temperature of 25°C, and a stirring time of 1 h. Transfer the mixed solution to a Teflon-lined stainless steel autoclave and perform a hydrothermal reaction at 110°C for 12 hours. After the hydrothermal reaction, collect the precipitated product by centrifugation, wash with ethanol and deionized water until the pH is approximately equal to 7, the centrifugal speed is 6000 rpm, the centrifugal time is 5 min, collect the precipitated product, and place it in a blast oven to dry for 12 hours at 60°C. Obtain PPA-intercalated Ni-Fe LDH, recorded as Ni-Fe LDH / PPA.

[0100] Embodiment 11:

[0101] Example 11 is basically the same as Example 10, the main difference being that the phosphorus-containing organic acid is different. Diphenylphosphoric acid (DPA) is selected to perform an in-situ intercalation experiment on Ni-Fe LDH, and the metal salt precursors include nickel chloride hexahydrate and ferric chloride nonahydrate. DPA intercalated Ni-Fe LDH is obtained, which is recorded as Ni-Fe LDH / DPA.

[0102] Experimental Example 1:

[0103] The morphology of the Ni-Fe LDH prepared in Examples 1-6 was analyzed by scanning electron microscopy. The morphologies of the Ni-Fe LDH prepared by different preparation methods were different. Figure 1As shown. In Example 1, the Ni-Fe LDH prepared using triethanolamine as a hydrothermal precipitant is a stacked small lamellar structure with a size of 20-50nm. In Example 2, urea is used as a hydrothermal precipitant to form a stacked whisker structure with a size of 500nm-1μm. In Example 3, the Ni-FeLDH after freeze-drying by co-precipitation is a stacked rod-like structure with a size of 1μm-5μm. In Example 4, the Ni-Fe LDH after oven-drying by co-precipitation is a stacked granular structure with a size of 50nm-100nm. The Ni-Fe LDH prepared using triethanolamine as a hydrothermal precipitant in the preferred embodiment 1 is subjected to subsequent experiments, and the stacked small lamellar structure is the optimized structure of LDH.

[0104] The Ni-Fe LDH prepared by reactants in different ratios in Example 5 has different structures, see Figure 2 As shown, when Ni:Fe is 2:1, the material has a lamellar structure, when Ni:Fe is 3:1, there is a lot of adhesion in the small lamellar layers of the material, when the Fe ratio increases, the material gradually becomes spherical, and when Ni:Fe is 1:4, the material has an independent spherical structure. The preferred reactant ratio Ni:Fe is 2:1 for subsequent experiments to ensure the lamellar structure of LDH.

[0105] The Ni-Fe LDH prepared at different hydrothermal reaction temperatures in Example 6 has different structures, see Figure 3 As shown in the figure, when the hydrothermal temperature is 60°C, the sample is a small lamellar structure; when the hydrothermal temperature is 90°C, the sample is a small lamellar structure; when the hydrothermal temperature is 110°C, the sample is a stacked large lamellar structure; when the hydrothermal temperature is 130°C, the sample is a rod-like structure. The subsequent experiments are preferably performed at a hydrothermal temperature of 110°C to ensure the lamellar structure of LDH.

[0106] Experimental Example 2:

[0107] The preferred Ni-Fe LDH prepared in Example 1 was analyzed by thermogravimetric and scanning electron microscopy, see Figure 4 and Figure 5As shown. The Ni-Fe LDH prepared in Example 1 has multiple thermal weight loss peaks, corresponding to the removal of adsorbed H2O, the removal of interlayer CO2, the removal of interlayer H2O, and the formation of metal oxides. The weight loss peak of Ni-Fe LDH at around 100°C corresponds to the removal of adsorbed H2O. It can be seen from the SEM image that the material is still a small lamellar structure. The weight loss peak of Ni-Fe LDH at around 300°C-380°C corresponds to the removal of interlayer CO2. It can be seen from the SEM image that the small lamellar layers of the material gradually agglomerate to form a large lamellar structure. The weight loss peak of Ni-Fe LDH at around 380°C-460°C corresponds to the removal of interlayer H2O. It can be seen from the SEM image that the material begins to form metal oxides and metal particles are generated on the surface of the layer. As the temperature continues to rise, layer rupture begins to occur and agglomerated metal particles are generated.

[0108] The Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Mg-Fe LDH prepared in Example 1 and Examples 7-9 were analyzed by thermogravimetric analysis, see Fig. 9 As shown, all four LDHs have multiple thermogravimetric peaks, corresponding to the removal of adsorbed H2O, the removal of interlayer CO2, the removal of interlayer H2O, and the formation of metal oxides.

[0109] Experimental Example 3:

[0110] The Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH, Mg-Fe LDH, Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Example 1, Examples 7-9 and Examples 10-11 were subjected to N2 adsorption and desorption analysis to analyze the specific surface area and pore size distribution of the synthesized materials. Figure 6 and Fig.12 As shown in the figure, from the pore size distribution, it can be seen that the four synthesized LDHs are all mesoporous materials, and the N2 adsorption and desorption graphs are all type IV hysteresis loops. Ni-Fe LDH and Co-Fe LDH are H4 type hysteresis loops, corresponding to the typical curves of lamellar materials containing narrow crack pores, and Cu-Fe LDH and Mg-Fe LDH are H3 type hysteresis loops, corresponding to the pores generated in the particles. After organic acid intercalation, the hysteresis loop of the material remains unchanged. The Ni-Fe LDH after intercalation is an H4 type hysteresis loop, corresponding to the typical curve of lamellar materials containing narrow crack pores, indicating that the pore structure of the material has not changed after intercalation.

[0111] Experimental Example 4:

[0112] The composition of the Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH and Mg-Fe LDH prepared in Example 1 and Examples 7-9 was analyzed by XPS. Figure 7As shown in the figure, among the four kinds of LDH synthesized, the elements of the materials can correspond one to one, and different metal elements can be detected.

[0113] Experimental Example 5:

[0114] The compositions of the Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH, Mg-Fe LDH, Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Examples 1, 7-9 and 10-11 were analyzed by FT-IR. Figure 8 and Fig.14 As shown. The characteristic peaks of interlayer water, CO and CH can all be detected in the four LDHs synthesized. The infrared spectrum of phenylphosphinoic acid is very similar to that of diphenylphosphoric acid. The main characteristic peaks of phenylphosphate include 1629.18, 1438.49, 960.93 cm -1 Peaks, etc. After LDH was intercalated with organic acid, the characteristic peak of phenyl phosphate appeared in LDH; it can also be seen that the peak position of P=O was red-shifted after diphenyl phosphate lost its proton, indicating that diphenyl phosphate successfully entered the interlayer.

[0115] Experimental Example 6:

[0116] The decomposition reaction path prediction analysis diagram of organic phosphates uses materials studio software to perform molecular simulations on diphenyl phosphate and phenyl hypophosphite. The results are as follows Fig.12 As shown, the total reaction ∆G of diphenylphosphate is 1456.72 kJ·mol -1 The reaction generates PO2· free radical, phenyl free radical and phenyl anion, and the total reaction ∆G of phenyl hypophosphite is 1470.19 kJ·mol -1 , the reaction generates PO2· free radicals, hydrogen free radicals and phenyl anions. In the decomposition process of phenyl hypophosphorous acid, hydrogen free radicals may promote the combustion reaction of phenyl hypophosphorous acid before the generation of PO2· free radicals. This makes the flame retardancy of diphenyl phosphate intercalated LDHs designed with PO2· as the flame retardant active substance stronger than that of phenyl hypophosphite intercalated LDHs. When phenyl hypophosphite intercalated LDHs are used as fillers, they may promote the decomposition of polymers to a certain extent and accelerate the combustion reaction. Although it does not affect the decomposition process of the organic polymer itself, hydrogen free radicals diffuse into the combustion system and are easily oxidized to intensify the combustion. After the decomposition of diphenyl phosphate, phenyl is released, which is a free radical that is more stable than hydrogen. In the presence of PO2·, it is likely to combine with other chain free radicals to form an aromatic condensed ring structure, or directly act as a carbon nucleus to generate carbon. It is predicted that it has a better effect on flame retardancy.

[0117] Experimental Example 7:

[0118] The smoke suppressant and toxic reduction hybrid material is added as an additive to thermoplastic polyurethane. A composite material is constructed by melt blending, the TPU masterbatch is dried and melted in an internal mixer, and then an LDH smoke suppressant is added to mix evenly to obtain a TPU composite material; the composite material is hot pressed on a flat vulcanizer to obtain a regular plate.

[0119] (1) Dry the TPU masterbatch in an oven for 6 hours to remove moisture for later use;

[0120] (2) The dried TPU masterbatch was melted in an internal mixer, wherein the temperature of the internal mixer was 180°C and the speed of the internal mixer was 140 rpm. After the TPU was melted, the prepared LDH smoke suppressant was added into the internal mixer under stirring conditions, wherein the amount of the smoke suppressant added was 3 wt%. The mixture was stirred for 5 minutes to be evenly mixed, and then a TPU composite material was obtained.

[0121] (3) The obtained irregular TPU composite material is hot pressed to obtain a regular plate. The specific material size and standard are formulated according to the national standard for combustion test. The hot pressing process is carried out on a flat vulcanizer, where the hot pressing temperature is 185°C, the pressure is 10 MPa, the preheating time is 3-5 minutes, and the hot pressing time is 1-3 minutes.

[0122] The smoke suppressant materials are selected from Ni-Fe LDH, Co-Fe LDH, Cu-Fe LDH, Mg-Fe LDH, Ni-Fe LDH / PPA and Ni-Fe LDH / DPA prepared in Example 1, Examples 7-9 and Examples 10-11, respectively. According to different smoke suppressant materials, the prepared composite materials are named Ni-Fe LDH / TPU, Co-Fe LDH / TPU, Cu-Fe LDH / TPU, Mg-Fe LDH / TPU, Ni-Fe LDH / PPA / TPU and Ni-Fe LDH / DPA / TPU.

[0123] The prepared flame retardant TPU composite materials (Ni-Fe LDH / TPU, Co-Fe LDH / TPU, Cu-Fe LDH / TPU, Mg-Fe LDH / TPU, Ni-Fe LDH / PPA / TPU and Ni-Fe LDH / DPA / TPU) and TPU materials were tested for heat release rate, total heat release, smoke release rate and total smoke release in a cone calorimeter at 35kW, see Fig.11 and Fig.15As shown, it shows the influence of different smoke suppressants on the combustion process of TPU materials. First, the composite materials of Ni-FeLDH, Co-Fe LDH, Cu-Fe LDH, Mg-Fe LDH and TPU prepared in Examples 1 and 7-9 were analyzed. The addition of Ni-Fe LDH had the best effect, with the peak heat release reduced by up to 21.4% and the total heat release reduced by up to 36.8%. Therefore, Ni-Fe LDH was selected for organic acid intercalation research.

[0124] After organic acid and PPA intercalation of Ni-Fe LDH, the heat release and smoke release of the composite material were further reduced. Among them, Ni-Fe LDH / PPA / TPU had the highest effect, with the peak heat release reduced by up to 38.58% and the total smoke release reduced by up to 38.78%, indicating that the fire safety performance of the material was further improved after organic acid and PPA intercalation.

[0125] Experimental Example 8:

[0126] The smoke density of the flame retardant TPU composite materials (Ni-Fe LDH / TPU, Ni-Fe LDH / PPA / TPU and Ni-Fe LDH / DPA / TPU) prepared in Experimental Example 7 was tested when burning at 25 kW. Fig.16 Before intercalation, the addition of Ni-Fe LDH reduced the smoke density of the material to a certain extent, by 10.6%; after the material was intercalated, the smoke density of the composite material was significantly reduced, and DPA had the best intercalation effect, greatly reducing the smoke density of the composite material (63.9%), which reflects the excellent smoke suppression effect of Ni-Fe LDH / DPA on TPU materials.

[0127] Experimental Example 9:

[0128] The flame retardant TPU composite materials (Ni-Fe LDH / TPU, Ni-Fe LDH / PPA / TPU and Ni-Fe LDH / DPA / TPU) prepared in Experimental Example 7 and the carbon residue after the combustion of the TPU materials were tested by scanning electron microscopy. Fig.17 As shown in the figure, it can be seen that the carbon residue after TPU combustion is loose and broken, and the carbon residue after the addition of Ni-Fe LDH becomes more dense. After organic acid root intercalation of Ni-Fe LDH, the carbon residue becomes loose and complete. The looseness of the material proves that the intercalated Ni-Fe LDH has an inhibitory effect on the combustion of TPU. The loose and complete carbon layer is conducive to the inhibition of material combustion and has a certain barrier effect.

[0129] Experimental Example 10:

[0130] The flame retardant TPU composite materials (Ni-Fe LDH / TPU, Ni-Fe LDH / PPA / TPU and Ni-Fe LDH / DPA / TPU) prepared in Experimental Example 7 were subjected to tensile tests as well as TPU materials. Fig.18 As shown in the figure, the addition of Ni-Fe LDH has a significant reduction in the mechanical properties of TPU due to the uneven distribution of the material. However, after the organic acid intercalation of Ni-Fe LDH, due to the presence of organic ions, the interface properties of the material are optimized through organic-inorganic interaction, which improves the mechanical properties of TPU to a certain extent. Organic acid intercalation LDH can achieve high flame retardancy and tensile strength retention at high filling.

[0131] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an organic phosphate intercalated layered metal hydroxide flame retardant and smoke suppression hybrid material, using a hydrothermal in-situ intercalation method, characterized in that The steps include: Step 1: Mix a divalent metal salt and a trivalent metal salt and dissolve them in deionized water, add a precipitant and an organic phosphate compound, and stir continuously at a temperature range of 25-30° C. to mix them uniformly to obtain a suspension; Step 2: Transfer the suspension obtained in step 1 to a high-pressure reactor, perform a hydrothermal reaction at 100° C.-150° C., filter to obtain a precipitated product, wash with ethanol and deionized water, and dry to obtain an organophosphate intercalated LDH hybrid material.

2. The preparation method according to claim 1, characterized in that: In step 1, the metal active components in the divalent metal salt and the trivalent metal salt include one or more of iron, cobalt, nickel, copper and magnesium.

3. The preparation method according to claim 2, characterized in that: The divalent metal is Ni 2+ 、Co 2+ , Cu 2+ Mg 2+ One or more of the following, the trivalent metal is Fe 3+ .

4. The preparation method according to claim 2, characterized in that: In the divalent metal salt and the trivalent metal salt, the molar ratio of the divalent metal to the trivalent metal is 2:1 to 3:

1.

5. The preparation method according to claim 1, characterized in that: The precipitant is triethanolamine, and the molar ratio of the precipitant addition amount to the metal salt is between 2:1 and 4:

1.

6. The preparation method according to claim 1, characterized in that: The organic phosphate compound is phenyl hypophosphorous acid or diphenyl phosphoric acid, and the molar ratio of the organic phosphate to the metal salt is between 1:2 and 1:

2.

7. An organic phosphate intercalated layered metal hydroxide flame retardant and smoke suppression hybrid material, prepared according to any one of the preparation methods of claims 1-6.

8. The use of the flame retardant and smoke suppressing hybrid material of the organic phosphate intercalated layered metal hydroxide according to claim 7, characterized in that: The organic phosphate intercalated layered metal hydroxide is added as an auxiliary agent into thermoplastic polyurethane to improve the flame retardant property and smoke suppression property of the material.

9. The use according to claim 8, characterized in that: The addition amount of the organic phosphate intercalated LDH hybrid material is 1-3wt% of the total mass of the composite material.

Citation Information

Patent Citations

  • Phosphate-radical-intercalated layered-like hydroxide containing zinc, aluminum and tin, preparation method thereof and application thereof in flame retardant material

    CN110218508A

  • Composite flame-retardant material, preparation method thereof, isolating membrane, negative pole piece, secondary battery and electric device

    CN115926812A

  • Mg-Al based hydrotalcite-type particles, chlorine-containing resin stabilizer and process for producing the particles

    US6413639B1