A composite light stabilizer, its preparation method and application
The preparation of composite light stabilizers has solved the problem of mechanical property loss of plastic film under ultraviolet light irradiation, improved the recycling rate of plastic film, and reduced "white pollution".
Patent Information
- Application Number
- CN202311516626.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-14
AI Technical Summary
Existing light stabilizers, when used to modify agricultural films, result in a loss of mechanical properties, reduce the recycling rate of agricultural films, and prevent them from maintaining their mechanical properties under ultraviolet light irradiation.
A composite light stabilizer is used, which consists of a light stabilizer, an ultraviolet light crosslinking agent, a nucleating agent, and rubber particles with a crosslinking structure. It is prepared by physical blending and works synergistically to improve the mechanical properties of the resin film, while maintaining them or improving them slowly.
The modified resin membrane exhibits low mechanical property loss under ultraviolet light irradiation, improving the recycling rate of membrane materials and reducing "white pollution".
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of light stabilizers, and more specifically, to a composite light stabilizer, its preparation method, and its application. Background Technology
[0002] Discarded agricultural film fragments enter arable land, affecting soil permeability, reducing soil moisture content, weakening drought resistance, causing secondary salinization, leading to soil compaction and decreased fertility, hindering crop water absorption and root growth, and gradually deteriorating arable land quality, causing serious damage to the agricultural ecological environment. Residual film left in fields and along roadsides is blown by the wind to areas around houses, treetops, rivers, and ponds, affecting the appearance of villages and towns. How to maintain a relatively constant film thickness while significantly improving its weather resistance and tear resistance to increase film recycling rates and reduce "white pollution" has become an urgent and important problem to be solved.
[0003] In existing technologies, light stabilizers are typically used to modify the matrix to improve the strength of the mulch film material after use and increase its recyclability. However, simply adding light stabilizers will result in the loss of some mechanical properties of the material, leading to a consistently low recycling rate of agricultural films after use.
[0004] Therefore, how to provide a composite light stabilizer that keeps the mechanical properties of the modified polyolefin membrane essentially unchanged, and further, how to minimize the loss of mechanical properties with increasing UV irradiation time, thus ensuring the mechanical properties during membrane recycling and improving the membrane recycling rate, is a technical problem that needs to be solved. Summary of the Invention
[0005] To address the aforementioned technical problems, the purpose of this invention is to provide a composite light stabilizer, its preparation method, and its application. This invention provides a composite light stabilizer that, after modification, maintains the basic mechanical properties of the resin film (e.g., mulch film or cotton packaging film). With increasing ultraviolet irradiation time, the loss rate of its mechanical properties is low, and in some cases, it even increases slowly, effectively ensuring the mechanical properties of the film material during recycling. It can be widely used for the mechanical recycling of agricultural films, improving the recycling rate of agricultural films, and is of great significance in reducing "white pollution."
[0006] The first aspect of the present invention is to provide a composite light stabilizer comprising a light stabilizer, an ultraviolet crosslinking agent, a nucleating agent, and rubber particles having a crosslinking structure. By mass, relative to 1 part of the light stabilizer, the total amount of the nucleating agent and the rubber particles having a crosslinking structure in the composite light stabilizer is 0.2 to 2 parts, and the content of the ultraviolet crosslinking agent is 0.5 to 3.5 parts.
[0007] In a preferred embodiment of the present invention, the mass ratio of the rubber particles to the nucleating agent is (3~7):(7~3).
[0008] In a preferred embodiment of the present invention, the nucleating agent is selected from at least one of sorbitol derivative nucleating agents, organic carboxylic acid nucleating agents, organic carboxylate nucleating agents, and organic phosphate nucleating agents; more preferably, the nucleating agent is selected from at least one of nucleating agent NA11, nucleating agent NA21, and nucleating agent 20E.
[0009] In a preferred embodiment of the present invention, the rubber particles having a cross-linked structure have at least one of the following characteristics: The average particle size of the rubber particles is 0.02~2 micrometers, preferably 0.1~1 micrometers, more preferably 0.2~0.5 micrometers; and / or, The rubber particles are spherical; and / or, The rubber particles have a gel content of 60 wt% or higher, preferably 80 wt% or higher.
[0010] In a preferred embodiment of the present invention, the rubber particles are at least one of the following rubber particles having a cross-linked structure: natural rubber, styrene-butadiene rubber, carboxylated styrene-butadiene rubber, nitrile rubber, carboxylated nitrile rubber, chloroprene rubber, polybutadiene, acrylate rubber, styrene-butadiene pyridine rubber, isoprene rubber, butyl rubber, ethylene propylene rubber, polysulfide rubber, acrylate-butadiene rubber, polyurethane rubber, fluororubber, and ethylene-vinyl acetate rubber.
[0011] The cross-linked rubber particles of this invention can be prepared using the method described in patent CN1402752. This involves adding a cross-linking agent such as TMPTA to a rubber latex containing uncross-linked rubber particles with a particle size of 20-2000 nm, irradiating it with a high-energy ray source, and then spray-drying it. The resulting cross-linked rubber particles are easily dispersed and can act as a carrier, assisting in the more uniform dispersion of nucleating agents and light stabilizers into the matrix resin, significantly improving the overall mechanical properties of the resin composition and meeting the requirements of cotton baling. During the transportation and storage of cotton bales, the polyethylene molecular chains break due to the combined effects of ultraviolet light and heat, generating a large number of free radicals. At this time, the ultraviolet cross-linking agent in the composition can not only absorb free radicals but also react with the cross-linked rubber particles, promoting the formation of the cross-linked structure. Therefore, it can effectively maintain the mechanical properties of the composition, enabling the packaging film to meet the requirements of high strength and high weather resistance during storage and transportation.
[0012] In this invention, the nucleating agent and the rubber particles with cross-linked structures can be added to the resin composition as separate raw materials, or commercially available products containing both can be used.
[0013] In another preferred embodiment of the present invention, the rubber particles and the nucleating agent are derived from a resin nucleating agent containing both the rubber particles and the nucleating agent; preferably, the resin nucleating agent is selected from at least one of VP101B, VP101C, and VP801E.
[0014] In a preferred embodiment of the present invention, the ultraviolet crosslinking agent is selected from at least one of crosslinking agents capable of undergoing isocyanate internal crosslinking and / or ketone hydrazine room temperature self-crosslinking reactions, preferably at least one of crosslinking agents capable of undergoing isocyanate internal crosslinking and / or ketone hydrazine room temperature self-crosslinking reactions at room temperature, for example, at 22-28°C; preferably, The ultraviolet crosslinking agent is selected from at least one of trimethylolpropane triacrylate, benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, diphenyl ethyl ketone, α,α-dimethoxy-α-phenyl acetophenone, α,α-diethoxyacetophenone, α-hydroxyalkyl phenyl ketone, α-aminealkyl phenyl ketone, aromatic phosphine oxide, bisbenzoylphenylphosphine oxide, benzophenone, 2,4-dihydroxybenzophenone, thiopropoxythioxanthrone, and isopropylthioxanthrone.
[0015] According to the present invention, the light stabilizer can be selected from a wide range. In a preferred embodiment of the present invention, the light stabilizer is selected from at least one of the following light stabilizers: Salicylic acid ester light stabilizers, benzoic acid ester light stabilizers, benzophenone light stabilizers, benzotriazole light stabilizers, triazine light stabilizers, substituted acrylonitrile light stabilizers, oxalamide light stabilizers, organonitrile complex light stabilizers, and hindered amine light stabilizers; Preferably, the light stabilizer is selected from hindered amine light stabilizers, more preferably from at least one of light stabilizer 944, light stabilizer 362 and light stabilizer 622, and even more preferably from light stabilizer 944 and light stabilizer 622.
[0016] The light-stabilizing additives described in this invention may also contain at least one additive commonly used in plastic processing, the dosage of which is the conventional dosage or may be adjusted according to actual requirements.
[0017] A second aspect of the present invention is to provide a method for preparing the composite light stabilizer described in the first aspect, comprising the step of mixing raw materials including the light stabilizer, an ultraviolet crosslinking agent, a nucleating agent and rubber particles having a crosslinking structure.
[0018] The mixing method is a conventional technique in the field, including but not limited to mixing by high-speed stirring.
[0019] The composite light stabilizer of the present invention is prepared by physical blending of all components, including commercially available light stabilizers, ultraviolet crosslinking agents, nucleating agents, and rubber particles with crosslinking structures. It has good compatibility with polymers and their additives and has light stability, thermal stability, and chemical stability.
[0020] The method of this invention is simple and easy to implement, has universal applicability, and is easy to industrialize.
[0021] A third aspect of the present invention is to provide the use of the composite light stabilizer described in the first aspect or the composite light stabilizer obtained by the preparation method described in the second aspect in a resin composition.
[0022] The aforementioned composite light stabilizer is suitable for modified polyethylene, polypropylene and other matrix resins, and is especially suitable for mulch films with a thickness of about 10 μm, for use under extreme heat and ultraviolet conditions.
[0023] A fourth aspect of the present invention is to provide a resin composition comprising a matrix resin, a composite light stabilizer, and optional additives; The composite light stabilizer is selected from the composite light stabilizer described in the first aspect or the composite light stabilizer obtained by the preparation method described in the second aspect; preferably, The content of the composite light stabilizer is 0.3-2 parts by weight relative to 100 parts of the base resin; and / or, the base resin is selected from polyethylene; and / or, the additive is selected from antioxidants.
[0024] A fifth aspect of the present invention is to provide a method for preparing the resin composition described in the fourth aspect, comprising melt-blending raw materials including a matrix resin, a composite light stabilizer and optional additives to obtain the resin composition.
[0025] The resin composition of the present invention is prepared by melt blending, a common process in rubber and plastics processing, using conventional rubber and plastics blending equipment to melt blend the raw material components, including the matrix resin and others, described above, in a single process.
[0026] During the preparation process, the blending temperature of the materials corresponds to the typical processing temperature of the base polyethylene resin, and should be selected within a range that ensures complete melting of the base polyethylene resin without causing its decomposition. Depending on processing requirements, appropriate amounts of conventional plastic processing additives can be added to the blended materials. During the blending process, the components can be simultaneously added to a melt blending device via metering or other methods for melt blending; alternatively, the components can be pre-mixed uniformly using general-purpose mixing equipment, and then melt-blended and extruded in a rubber-plastic blending device to obtain the modified resin composition.
[0027] The rubber-plastic blending equipment used in the preparation method of this invention can be an open mill, internal mixer, single-screw extruder, twin-screw extruder, or torque rheometer, etc. The material mixing equipment is selected from commonly used mechanical mixing equipment in the art, such as high-speed mixers and kneaders.
[0028] A sixth aspect of the present invention is to provide the application of the resin composition described in the fourth aspect or the resin composition obtained by the preparation method described in the fifth aspect in agricultural films, polyolefin roofing tiles, and polyolefin rotomolding.
[0029] The resin composition containing a composite light stabilizer described in this invention is prepared by a one-time melt blending method of all components, including the matrix resin and the composite light stabilizer. The preparation method is simple, and it does not bloom or ooze during processing and use. The resin composition containing this composite light stabilizer exhibits light stability, thermal stability, and chemical stability, and does not change due to heat during processing and use, with minimal heat loss due to volatilization. It is hydrolysis-resistant, inexpensive, and easy to promote and use. It can be widely used in the agricultural field, such as greenhouse films, mulch films, stretch films, and geotextiles, and also in the construction field for TPO roofing materials, building exterior walls, wall panels, polyolefin roofing tiles; louvers, polyolefin roofing and wall panels, solar energy products, sports ceramic tiles, and polyolefin molding compounds and roll forming materials, etc.
[0030] The advantages of this invention are: This invention provides a composite light stabilizer using specific raw material types and ratios. The resin film modified with this stabilizer (such as mulch film or cotton packaging film) retains its mechanical properties essentially unchanged. With increasing ultraviolet irradiation time, the loss rate of its mechanical properties is low, and in some cases, it even increases slowly. This effectively ensures the mechanical properties of the film material during recycling and can be widely used for the mechanical recycling of agricultural films, improving the recycling rate of agricultural films and playing an important role in reducing "white pollution".
[0031] The inventors of this invention believe that the above advantages are due to the following reasons: The light stabilizer, UV crosslinking agent, nucleating agent, and crosslinked rubber particles in the composite light stabilizer have a synergistic effect. The addition of the nucleating agent in the composite light stabilizer increases the crystallinity of the resin, accelerates its crystallization rate, and reduces the amorphous region. Its synergistic effect with the light stabilizer and UV crosslinking agent helps maintain the mechanical properties of the material. Under thermal and UV light conditions, the UV crosslinking agent can absorb energy of a certain wavelength, generating free radicals and cations, thereby initiating monomer polymerization and crosslinking. Within the molecule, under the raw materials and proportions of this invention, crosslinking and degradation occur simultaneously. The free radicals and cations provided by the UV crosslinking agent facilitate crosslinking between molecular chains, maintaining molecular weight and thus ensuring good retention of mechanical properties. With increasing UV irradiation time, its mechanical properties remain essentially unchanged, essentially equivalent to before use, increasing the service life of the matrix material and facilitating recycling in agricultural machinery, thereby improving recycling efficiency. Detailed Implementation
[0032] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0033] The scope of the invention is not limited to these embodiments, but is set forth in the appended claims.
[0034] The experimental data in this embodiment were measured using the following instruments and methods: The tensile load and nominal strain at break of the specimens were tested according to the national standard GB / T1040.3-2006. Type 2 specimens were used, with a width of 10 mm. The initial mark distance between the fixtures was 50 mm. The test speed (no load) was 500 mm / min. The specimens were stretched until they broke, and the maximum tensile load was measured to an accuracy of 0.01 N. All prepared specimens were clearly marked with their specimen number and sampling direction (transverse or longitudinal).
[0035] The nominal fracture strain is calculated using the following formula: ε=ΔL / L×100 In the formula: ε — nominal fracture strain, %; ΔL ——— Increment of the distance between fixtures, in millimeters (mm); L — Initial distance between fixtures, in millimeters (mm).
[0036] The test shall be conducted in accordance with QB / T1130-1991, with single-piece sample testing, accurate to 0.1N.
[0037] The test method for right-angle tear is as follows: The experiment is conducted according to the QB / T 1130-91 standard. The initial mark distance between the fixtures is 55 mm, the test speed (no load) is 200 mm / min, and the specimen is stretched until it breaks. The maximum tensile load is measured to an accuracy of 0.01 N. All prepared specimens are clearly marked with specimen number and sampling direction (transverse or longitudinal).
[0038] The prepared tensile and right-angle tear specimens need to undergo comparative experiments with artificial ultraviolet aging. The specific conditions for ultraviolet aging are as follows: referring to GB / T16422.3-2014, the light source is a fluorescent ultraviolet lamp, UV-A340 tube, at a wavelength of 340nm, the irradiance is 0.76W / (m²). 2 •nm), and irradiated with ultraviolet light according to the pattern of light temperature 60℃, radiation time 8h (bright); condensation temperature 50℃, condensation time 4h (dark), for a total irradiation time of 288 hours.
[0039] In the following examples, 1076 refers to antioxidant 1076 produced by BASF Chemicals; 168 refers to antioxidant 168 produced by BASF Chemicals; and 944 refers to light stabilizer 944 produced by Beijing Tiangang Chemicals. VP801E refers to VP801E produced by Sinopec Beijing Research Institute of Chemical Industry. VP801E contains nucleating agent NA11 and EVA rubber particles with a cross-linked structure. The average particle size of the rubber particles is 0.2 micrometers, and the gel content of the rubber particles is 90 wt%. The mass ratio of the rubber particles to the nucleating agent is 3:7.
[0040] In the following Examples 1-6 and Comparative Examples 1-4: The initial mixing and melt blending process of the materials is as follows: First, all materials are weighed according to the proportion and initially mixed in a high-speed mixer for 20 seconds. Then, melt blending and granulation are carried out using a twin-screw extruder. The mixing equipment is a Coperon 35 twin-screw extruder with a speed of 200 r / min and a temperature setting of 170℃, 180℃, 190℃, 200℃, 200℃, and 200℃. The resulting granules are placed in a tray and treated in a 70℃ oven for 4 hours to remove moisture.
[0041] Films were prepared using a blown film blowing method: the equipment was a Colin blown film machine from Germany, with the temperatures of each section set to 160℃, 180℃, 200℃, 210℃, 210℃, 210℃, and 210℃, the feed rate to be 25%, and the winding rate to be 10m / min. The resulting film had a smooth surface, an average width of 22cm, and an average thickness of 10μm.
[0042] Comparative Example 1 and Comparative Example 2 Using 1600g of LLDPE resin 1802 provided by Zhenhai Petrochemical as the matrix, and 0.80g of antioxidant 1076 and 1.6g of antioxidant 168 produced by BASF Chemical, the materials were initially mixed and melt-blended under the above conditions. The resulting granules were blown into films, and tensile and right-angle tear samples were prepared as comparative example 1.
[0043] The resulting Comparative Example 1 sample, after being subjected to accelerated artificial ultraviolet aging, was labeled as Comparative Example 2.
[0044] Comparative Example 3 and Comparative Example 4 Using 1600g of LLDPE resin 1802 provided by Zhenhai Petrochemical as the matrix, it was mixed with 0.80g of antioxidant 1076 and 1.6g of antioxidant 168 produced by BASF Chemical, and 4.8g of light stabilizer 944 produced by Beijing Tiangang Chemical. The materials were initially mixed and melt-blended. The resulting granules were blown into films, and tensile and right-angle tear samples were prepared as comparative example 3.
[0045] The resulting Comparative Example 3 sample, after being subjected to accelerated artificial ultraviolet aging, was labeled as Comparative Example 4.
[0046] Example 1 and Example 2 Using 1600g of LLDPE resin 1802 provided by Zhenhai Petrochemical as the matrix, it was initially mixed and melt-blended with 0.80g of 1076 and 1.6g of 168 produced by BASF Chemical, 4.8g of 944 produced by Beijing Tiangang Chemical, 1.28g of VP801E produced by Sinopec Beijing Chemical Research Institute, and 3.2g of trimethylolpropane triacrylate (TMPTA) produced by Tianjin Tianjiao Chemical Co., Ltd. The resulting granules were used to prepare films by blow molding. Tensile and right-angle tear test samples were prepared, which is Example 1.
[0047] The resulting sample, after being subjected to accelerated aging under artificial ultraviolet light, was labeled as Example 2.
[0048] Example 3 and Example 4 Using 1600g of LLDPE resin 1802 provided by Zhenhai Petrochemical as the matrix, it was initially mixed and melt-blended with 0.80g of 1076 and 1.6g of 168 produced by BASF Chemical, 4.8g of 944 produced by Beijing Tiangang Chemical, 1.28g of VP801E produced by Sinopec Beijing Chemical Research Institute, and 8g of trimethylolpropane triacrylate (TMPTA) produced by Tianjin Tianjiao Chemical Co., Ltd. The resulting granules were used to prepare films by blow molding. Tensile and right-angle tear test samples were prepared, which is Example 3.
[0049] The resulting sample, after being subjected to accelerated aging under artificial ultraviolet light, was labeled as Example 4.
[0050] Examples 5 and 6 Using 1600g of LLDPE resin 1802 provided by Zhenhai Petrochemical as the matrix, it was initially mixed and melt-blended with 0.80g of 1076 and 1.6g of 168 produced by BASF Chemical, 4.8g of 944 produced by Beijing Tiangang Chemical, 1.28g of VP801E produced by Sinopec Beijing Chemical Research Institute, and 16g of trimethylolpropane triacrylate (TMPTA) produced by Tianjin Tianjiao Chemical Co., Ltd. The resulting granules were used to prepare films by blow molding. Tensile and right-angle tear test samples were prepared, which is Example 5.
[0051] The resulting sample, after being subjected to accelerated aging under artificial ultraviolet light, was labeled as Example 6.
[0052] Table 1
[0053] As shown in the table above, the transverse tensile load decreased slightly after aging compared to before aging, and the transverse tensile loads of the various samples were basically the same. The longitudinal tensile load of the sample modified with the composite light stabilizer after aging was approximately 2.6 N, higher than the 1.8 N of the unmodified sample and the 2.3 N of the sample modified with 944. The nominal transverse and longitudinal strains of the sample modified with the composite light stabilizer remained essentially unchanged after artificial aging. The right-angle tear strength of the sample without added light stabilizer decreased significantly after artificial aging. The longitudinal right-angle tear strength of the sample modified with both light stabilizer and 944 was around 1.2 N and the transverse right-angle tear strength was approximately 1.0 N after artificial UV aging. Even after 288 hours of UV irradiation, the transverse right-angle tear strength of the film sample with the composite light stabilizer remained approximately 1.0 N. With the increase of TMPTA content in the composite light stabilizer, the longitudinal right-angle tear strength of the composite light stabilizer-modified film increased significantly. The modified film formulation with 1% TMPTA added has a longitudinal right-angle tear strength of 1.305, which is significantly higher than other formulations. Moreover, after artificial UV aging for 288 hours, this strength value increased by 15%.
[0054] The above data shows that, in a polyethylene-based film system, the addition of the composite light stabilizer described in this invention, under ultraviolet light irradiation, effectively improves both the longitudinal tensile load and longitudinal right-angle tear strength of the film material. During the aging process, some of the free radicals react with the ultraviolet crosslinking agent to form a micro-crosslinked structure, which makes the connections between polyethylene molecular chains tighter, thus increasing tensile load and tear strength. This phenomenon helps maintain the strength of the film in high-heat and high-UV environments, thereby improving its service life and recyclability.
[0055] The above embodiments illustrate the technical effects of the composite light stabilizer of the present invention in 10μm mulch films. The composite light stabilizer of the present invention also exhibits excellent performance in thick films (e.g., cotton packaging films), as illustrated in the following embodiments: Among the following raw materials, the cross-linked EVA rubber particles produced by Beijing Institute of Chemical Technology have an average particle size of 0.2 micrometers and a gel content of 85 wt%; and the nucleating agent HPN20E from MILIKEN.
[0056] Comparative Examples 1B to 5B Using 2000g of LLDPE resin 1802 powder provided by Zhenhai Petrochemical as the matrix, it was initially mixed and melt-blended with 0.80g of 1076 and 1.6g of 168 produced by BASF, and 8g of 944 produced by Beijing Tiangang Chemical. The resulting granules were then blown into films, and tensile and dart impact test specimens were prepared, designated as Comparative Example 1B. The obtained specimens were subjected to accelerated artificial UV aging for 240h, 480h, 720h, and 960h, and were subsequently labeled as Comparative Example 2B, Comparative Example 3B, Comparative Example 4B, and Comparative Example 5B, respectively.
[0057] The specific process conditions are as follows: The initial mixing and melt blending processes are as follows: First, all materials are weighed according to the proportions and initially mixed in a high-speed mixer for 20 seconds. Then, melt blending and granulation are carried out using a twin-screw extruder. The mixing equipment is a Coperon 35 twin-screw extruder with a speed of 200 r / min and temperatures set at 170℃, 180℃, 190℃, 200℃, 200℃, and 200℃. The resulting granules are placed in trays and heated at 70℃. o Process in a high-temperature oven for 4 hours to remove moisture.
[0058] Films were prepared using a blown film extrusion method. The equipment was a Colin blown film extrusion machine from Germany. The temperatures of each section were set to 160℃, 180℃, 200℃, 210℃, 210℃, 210℃, and 210℃. The feed rate was 50%, and the winding rate was 2m / min. The resulting film had a smooth surface, an average width of 22cm, and an average thickness of 140μm.
[0059] The prepared tensile and right-angle tear specimens need to undergo comparative experiments with artificial ultraviolet aging. The specific conditions for ultraviolet aging are as follows: referring to GB / T16422.3-2014, the light source is a fluorescent ultraviolet lamp, UV-A340 tube, at a wavelength of 340nm, the irradiance is 0.76W / (m²). 2 •nm), and ultraviolet light was applied according to the rule of light temperature 60℃, radiation time 8h (bright); condensation temperature 50℃, condensation time 4h (dark), and irradiation time was 240h, 480h, 720h, and 960h.
[0060] The dart impact test was conducted according to the standard GB / T9639, using method B. The conditioning time was 8 hours and the test temperature was 23℃. The impact failure mass value was obtained.
[0061] The tensile load and nominal strain at break of the specimens were tested according to the national standard GB / T1040.3-2006. Type 2 specimens were used, with a width of 10 mm. The initial mark distance between the fixtures was 50 mm. The test speed (no load) was 500 mm / min. The specimens were stretched until fracture, and the maximum tensile load was measured to an accuracy of 0.01 N. All prepared specimens were clearly marked with specimen number and sampling direction (transverse or longitudinal). The method for calculating the nominal strain at break was the same as above.
[0062] Examples 1B to 5B Using LLDPE resin 1802 powder provided by Zhenhai Petrochemical as the matrix, with a weight of 2000g, it was mixed with 0.80g of 1076 and 1.6g of 168 produced by BASF, 8g of 944 produced by Beijing Tiangang Chemical, 4.8g of cross-linked EVA rubber particles produced by Beijing Institute of Chemical Technology, 11.2g of MILIKEN nucleating agent HPN20E, and 10g of trimethylolpropane triacrylate (TMPTA) from Tianjin Tianjiao Chemical Co., Ltd. The materials were initially mixed and melt-blended. The resulting granules were blown into films, and tensile and dart impact test specimens were prepared, designated as Example 1B. The obtained samples were subjected to accelerated artificial UV aging for 240h, 480h, 720h, and 960h, and were subsequently labeled as Example 2B, Example 3B, Example 4B, and Example 5B, respectively.
[0063] The specific process conditions and testing methods are the same as those for Comparative Examples 1B to 5B.
[0064] Table 2
[0065] Data from comparative samples 1-5 show that with increasing aging time, the tensile load, nominal strain at break, and dart impact fracture mass of the comparative samples all decreased significantly. Comparative sample 5, with an aging time of 960 hours, exhibited a decrease in tensile load of approximately 30% and a decrease in dart impact fracture mass of 23%. This is because the large number of free radicals generated during the aging process significantly damages the long molecular chains in polyethylene, shortening them and reducing their tensile load and dart impact fracture mass.
[0066] Data from Examples 1-5 show that after the composite light stabilizer is used to modify polyethylene resin, the tensile load loss rate of the sample remains at a low level, approximately 10-15%, as the aging time increases; the nominal strain at break remains basically unchanged, and the loss rate of dart impact damage also remains at around 10%.
[0067] As shown in Table 1, the comparative film samples without the composite light stabilizer of the present invention had significantly lower tensile load and dart impact strength before aging than the sample of the example, indicating that the addition of the composite light stabilizer can improve the mechanical properties of the thick film (140 μm) resin composition.
[0068] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.
[0069] All publications, patent applications, patents, and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings commonly understood by those skilled in the art. In case of conflict, the definitions in this specification shall prevail.
[0070] When this specification uses the prefixes “known to those skilled in the art,” “prior art,” or similar terms to derive materials, substances, methods, steps, apparatus, or components, the objects derived from such prefixes cover those commonly used in the art at the time of this application, but also include those that are not currently commonly used but will become generally recognized in the art as suitable for similar purposes.
[0071] The endpoints and any values of the ranges disclosed in this application are not limited to the precise ranges or values; such ranges or values should be understood to include values close to them. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. In principle, various technical solutions can be combined with each other to obtain new technical solutions, which should also be considered as specifically disclosed herein.
[0072] In the context of this specification, except where expressly stated otherwise, any matters or issues not mentioned shall apply directly to those known in the art without any modification.
[0073] Furthermore, any implementation described herein can be freely combined with one or more other implementations described herein, and the resulting technical solutions or technical ideas shall be regarded as part of the original disclosure or original record of the present invention, and should not be regarded as new content not disclosed or anticipated herein, unless those skilled in the art consider the combination to be obviously unreasonable.
Claims
1. A resin composition comprising a matrix resin, a composite light stabilizer, and optional additives; The composite light stabilizer includes a light stabilizer, an ultraviolet crosslinking agent, a nucleating agent, and rubber particles with a crosslinking structure. By mass, relative to 1 part of the light stabilizer, the total amount of the nucleating agent and the rubber particles with a crosslinking structure in the composite light stabilizer is 0.2 to 2 parts, and the content of the ultraviolet crosslinking agent is 0.5 to 3.5 parts; the ultraviolet crosslinking agent is selected from trimethylolpropane triacrylate. Based on parts by weight, the content of the composite light stabilizer is 0.3-2 parts relative to 100 parts of the base resin; the additives are selected from antioxidants; The method for preparing the resin composition includes melt blending raw materials, including a matrix resin, a composite light stabilizer, and optional additives, to obtain the resin composition.
2. The resin composition according to claim 1, characterized in that: The mass ratio of the rubber particles to the nucleating agent is (3~7):(7~3); and / or, The nucleating agent is selected from at least one of sorbitol derivative nucleating agents, organic carboxylic acid nucleating agents, organic carboxylate nucleating agents, and organic phosphate nucleating agents.
3. The resin composition according to claim 1, characterized in that: The nucleating agent is selected from at least one of nucleating agent NA11, nucleating agent NA21, and nucleating agent 20E.
4. The resin composition according to claim 1, characterized in that: The average particle size of the rubber particles is 0.02~2 micrometers; and / or, The rubber particles are spherical; and / or, The rubber particles have a gel content of 60 wt% or higher.
5. The resin composition according to claim 1, characterized in that: The average particle size of the rubber particles is 0.1~1 micrometer; and / or, The rubber particles have a gel content of 80 wt% or higher.
6. The resin composition according to claim 1, characterized in that: The rubber particles are at least one of the following rubber particles having a cross-linked structure: Natural rubber, styrene-butadiene rubber, carboxylated styrene-butadiene rubber, nitrile rubber, carboxylated nitrile rubber, chloroprene rubber, polybutadiene, acrylate rubber, styrene-butadiene pyridine rubber, isoprene rubber, butyl rubber, ethylene propylene rubber, polysulfide rubber, acrylate-butadiene rubber, polyurethane rubber, fluororubber.
7. The resin composition according to claim 1, characterized in that: The rubber particles and nucleating agent are derived from a resin nucleating agent that contains both the rubber particles and the nucleating agent.
8. The resin composition according to claim 7, characterized in that: The resin nucleating agent is selected from at least one of VP101B, VP101C, and VP801E.
9. The resin composition according to any one of claims 1-8, characterized in that: The light stabilizer is selected from at least one of the following light stabilizers: Salicylic acid ester light stabilizers, benzoic acid ester light stabilizers, benzophenone light stabilizers, benzotriazole light stabilizers, triazine light stabilizers, substituted acrylonitrile light stabilizers, oxalamide light stabilizers, organonitrile complex light stabilizers, and hindered amine light stabilizers.
10. The resin composition according to any one of claims 1-8, characterized in that: The light stabilizer is selected from hindered amine light stabilizers.
11. The resin composition according to claim 10, characterized in that: The light stabilizer is selected from at least one of light stabilizer 944, light stabilizer 362 and light stabilizer 622.
12. The resin composition according to any one of claims 1-8, characterized in that: The method for preparing the composite light stabilizer includes the step of mixing raw materials comprising the light stabilizer, ultraviolet crosslinking agent, nucleating agent and rubber particles with crosslinking structure.
13. The resin composition according to claim 1, characterized in that: The matrix resin is selected from polyethylene.
14. A method for preparing a resin composition according to any one of claims 1-13, comprising melt-blending raw materials including a matrix resin, a composite light stabilizer, and optional additives to obtain the resin composition.
15. Use of a resin composition according to any one of claims 1-13 in agricultural films, polyolefin roofing tiles or polyolefin rotomolding.
Citation Information
Patent Citations
Composite powder rubber, its preparation method and application
CN1412229A
Crosslinked elastic fibers
US20020064653A1