Method of forming oxide-nitride-oxide stack for non-volatile memory and integration with CMOS process flow

By employing ALD tools to fabricate multilayer tunneling and blocking dielectrics in SONOS memory cells, the problems of charge retention and threshold voltage degradation during the scaling process of ONO stacks were solved, enabling efficient integration into CMOS process flows.

CN120052068BActive Publication Date: 2026-11-24INFINEON TECHNOLOGIES LLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380068614.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-09-27
Filing Date
2023-09-26
Publication Date
2026-11-24
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

Existing SONOS memory cells face challenges such as charge retention, threshold voltage degradation, and migration during scaling, and are difficult to integrate into baseline CMOS process flows.

Method used

Atomic layer deposition (ALD) tools were used to perform free radical oxidation and oxide deposition processes to form multilayer tunnel dielectric and barrier dielectric layers. By adjusting process parameters, the film thickness, uniformity and stoichiometry were controlled to optimize the manufacturing process of ONO stacking.

Benefits of technology

It improves the ability of ONO stacks to vary composition, enhances membrane stoichiometry and thickness uniformity, reduces charge leakage, and improves the performance and integration of memory cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120052068B_ABST
    Figure CN120052068B_ABST
Patent Text Reader

Abstract

A method for fabricating a semiconductor device is described. Typically, this method includes forming a customizable oxide-nitride-oxide (ONO) stack over a substrate in an in-situ atomic layer deposition (ALD) tool or chamber. A radical oxidation or oxide deposition process step is performed to form a tunnel dielectric layer covering the substrate. A silicon nitride deposition process step is also performed to form a multilayer charge trapping (CT) layer, wherein at least some process parameters of the silicon nitride deposition process step are adjusted during the formation of a first and second CT sublayer of the multilayer CT layer. Subsequently, a radical oxidation or oxide deposition process step is performed in the ALD tool to form a barrier dielectric layer covering the multilayer CT layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application is an international application of U.S. Non-Provisional Application No. 17 / 954,141, filed on September 27, 2022, the contents of which are incorporated herein by reference. Technical Field

[0003] This disclosure generally relates to non-volatile memory (NVM) cells or devices, and more specifically to NVM cells or devices based on silicon (semiconductor)-oxide-nitride-oxide-silicon (semiconductor) (SONOS) and methods for manufacturing the same. Background Technology

[0004] NVM is widely used for storing data in computer systems, typically including memory arrays or other configurations with a large number of NVM cells arranged in rows and columns. For decades, the scaling of features in integrated circuits has been a driving force behind the ever-evolving semiconductor industry. Scaling to increasingly smaller features allows for increased density of functional units within the limited space of a semiconductor chip. However, the pursuit of greater capacity is not without its challenges. The need to optimize the performance of each device while scaling has become increasingly important.

[0005] In some implementations, an NVM cell may include at least non-volatile elements, such as a charge-trapping field-effect transistor (FET) or a floating-gate transistor, which can be programmed or erased by applying a voltage of appropriate polarity, amplitude, and duration between the control / storage gate and the substrate or the drain / source region. For example, in an n-channel charge-trapping FET, a positive gate-substrate voltage causes electrons to tunnel through the channel and be trapped in the charge-trapping dielectric layer via the Fermi-Nordheim (FN) tunneling effect, thereby increasing the transistor threshold voltage (Vth). T Or reduce its drain current (I) D A negative gate-channel voltage causes holes to tunnel through the channel and be trapped in the charge-trapping dielectric layer, thereby reducing the Vo of the SONOS transistor. T Or improve its I D In some implementations, SONOS-based memory arrays are used and operated as digital data storage devices, wherein two different V arrays based on SONOS cells are stored. T Or I D The binary bits (0 and 1) of the level or value data.

[0006] There is a need to use NVM technologies such as SONOS for analog memory and processing because they have the ability to configure multiple different Vs with achievable high precision.T and I D (More than two) levels. SONOS memory cells provide the low latency, low power consumption, and low noise operation expected for analog processing, including edge inference computing, such as neuromorphic computing in artificial intelligence (AI) applications. However, multi-level SONOS memory cells may introduce more challenges during scaling, such as charge retention in the ONO stack, V... T Degeneration and / or migration.

[0007] Therefore, the object of the present invention is to provide an improved manufacturing process for forming ONO stacks in SONOS memory cells; and to integrate such a process into a baseline complementary metal-oxide-semiconductor (CMOS) process flow. Attached Figure Description

[0008] The invention will be more fully understood from the following detailed description, the accompanying drawings, and the claims, in which:

[0009] Figure 1 This is a block diagram showing a cross-sectional side view of a SONOS-based non-volatile memory transistor or device;

[0010] Figure 2A This is a representative flowchart illustrating an embodiment of a method for manufacturing an oxide-nitride-oxide (ONO) stack in a SONOS-based non-volatile memory transistor according to an embodiment of the present disclosure;

[0011] Figure 2B This is a representative diagram showing an example of an atomic layer deposition (ALD) chamber or tool;

[0012] Figures 3A to 3D It is shown in accordance with Figure 2A A representative cross-sectional view of the tunnel dielectric portion of a SONOS-based non-volatile memory transistor during the fabrication process;

[0013] Figures 4A to 4E It is shown in accordance with Figure 2A A representative cross-sectional view of the charge trapping dielectric portion of a SONOS-based non-volatile memory transistor during fabrication.

[0014] Figures 5A to 5D It is shown in accordance with Figure 2A A representative cross-sectional view of the top or blocking dielectric portion of a SONOS-based non-volatile memory transistor during the manufacturing process;

[0015] Figure 5E This is a representative cross-sectional view showing a memory stack including an ONO barrier dielectric stack of floating gate memory transistors according to an embodiment of the present disclosure;

[0016] Figure 6 This is a block diagram showing a portion of a SONOS-based non-volatile memory cell or device according to an embodiment of the present disclosure;

[0017] Figure 7 This is a representative flowchart illustrating an embodiment of a manufacturing method for integrating SONOS-based memory transistors into a MOS transistor process flow according to an embodiment of the present disclosure; and

[0018] Figures 8A to 8E It shows the basis Figure 7 A representative cross-sectional view of the SONOS-based storage device portion of the method. Detailed Implementation

[0019] The following description sets forth numerous specific details, such as examples of particular systems, components, methods, etc., to provide a good understanding of several embodiments of the subject matter. However, it will be apparent to those skilled in the art that at least some embodiments can be practiced without these specific details. In other instances, well-known components or methods are not described in detail or presented in a simple block diagram format to avoid unnecessarily obscuring the techniques described herein. Therefore, the specific details set forth below are merely exemplary. Specific implementations may differ from these exemplary details and are still considered to be within the spirit and scope of the subject matter.

[0020] This document describes, with reference to the accompanying drawings, embodiments of memory cells including SONOS-based transistors with or without metal-oxide-semiconductor (MOS) transistors or field-effect transistors (FETs), and methods of manufacturing thereof. However, specific embodiments may be practiced without one or more of these specific details or in combination with other known methods, materials, and apparatus in the relevant art. In the following description, numerous specific details, such as specific materials, dimensions, concentrations, and process parameters, are set forth to provide a thorough understanding of the subject matter. In other instances, well-known semiconductor design and manufacturing techniques have not been described in particular detail to avoid unnecessarily obscuring the subject matter. The terms "embodiment," "one embodiment," "example embodiment," "some embodiments," and "various embodiments" used in the specification mean that a specific feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the subject matter. Furthermore, the phrases "embodiment," "one embodiment," "example embodiment," "some embodiments," and "various embodiments" appearing in different places in the specification do not necessarily refer to the same embodiment.

[0021] The specification includes references to the accompanying drawings, which form part of the detailed description. The drawings illustrate exemplary embodiments. These embodiments, which may also be referred to herein as “examples,” are described in sufficient detail to enable those skilled in the art to practice embodiments of the claimed subject matter described herein. Embodiments may be combined, other embodiments may be utilized, or structural, logical, and electrical changes may be made without departing from the scope and spirit of the claimed subject matter. It should be understood that the embodiments described herein are not intended to limit the scope of the subject matter, but rather to enable those skilled in the art to practice, make, and / or use the subject matter.

[0022] As used herein, the terms "above," "below," "between," and "on" refer to the relative position of one layer with respect to other layers. Thus, for example, a layer deposited or disposed above or below another layer may be in direct contact with said other layer, or may have one or more intermediate layers. Furthermore, a layer deposited or disposed between layers may be in direct contact with each layer, or may have one or more intermediate layers. Additionally, assuming that operations of depositing, modifying, and removing films relative to a starting substrate are performed without considering the absolute orientation of the substrate, the relative position of one layer with respect to other layers is provided.

[0023] Unless otherwise specifically stated, as will be apparent from the following discussion, it should be understood that the use of terms such as “processing,” “computation,” “operation,” “determine,” etc., throughout this specification refers to the actions and / or processing of a computer or computing system or similar electronic computing device that manipulate data represented as physical (e.g., electronic) quantities in the registers and / or memory of the computing system, and / or convert such data into other data represented as physical quantities in the memory, registers, or other such information storage, transmission, or display devices of the computing system.

[0024] Summary of the topic

[0025] According to one embodiment of a method for manufacturing a semiconductor device, the method may include the following steps: dividing a substrate into a first region and a second region, and forming a customizable oxide-nitride-oxide (ONO) stack in the first region; performing at least one of a first radical oxidation process step and a first oxide deposition process step in an atomic layer deposition (ALD) tool to form a tunnel dielectric layer covering the substrate; performing a plurality of silicon nitride deposition process steps in the ALD tool to form a multilayer charge trapping (CT) layer; determining process parameters for the first silicon nitride deposition process step in the plurality of silicon nitride deposition process steps to form a first CT sublayer; modifying at least one of the process parameters; performing a second silicon nitride deposition process step to form a second CT sublayer covering the first CT sublayer; and performing at least one of a second radical oxidation process step and a second oxide deposition process step in the ALD tool to form a barrier dielectric layer covering the multilayer CT layer in the first region.

[0026] In one embodiment, the formed silicon nitride may include oxygen-containing silicon oxynitride.

[0027] In one implementation, customizable ONO stacking process steps are performed in situ using the same ALD tool.

[0028] In one embodiment, the silicon, oxygen, and nitrogen film compositions of silicon nitride in the first CT sublayer and the second CT sublayer are different. In one embodiment, the first CT sublayer is oxygen-rich silicon nitride, resulting in it being substantially free of charge traps, while the second CT sublayer is oxygen-depleted silicon nitride, resulting in it being substantially densely packed with charge traps.

[0029] According to one embodiment of a method for manufacturing a semiconductor device, the method may further include performing a plurality of third silicon nitride deposition process steps to form a plurality of third CT sublayers disposed between a first CT sublayer and a second CT sublayer. In this step, process parameters of the plurality of third silicon nitride deposition process steps are adjusted such that the oxygen enrichment levels of the plurality of third CT sublayers fall between the oxygen enrichment levels of the first CT sublayer and the second CT sublayer. In one embodiment, the method further includes performing at least one of a third radical oxidation process step and a third oxide deposition process step in the same ALD tool to form a thin oxide film covering the first CT sublayer and beneath the second CT sublayer, wherein forming the thin oxide film reduces the tunneling of electron charge accumulated at the boundary of the second CT sublayer into the first CT sublayer.

[0030] In one embodiment, the process parameters for the first radical oxidation process step and the second radical oxidation process step may include: the type of reactant gas including O2 / H2 gas; the flow rate of the reactant gas into the ALD tool; the reaction time for each reactant gas; the order in which the reactant gas enters the ALD tool; and the number of repetitions and the repetition order, wherein the process parameters are configured to control at least one of the thickness, density, and mass of the oxide formed in the tunnel dielectric layer.

[0031] In one embodiment, the process parameters for the first oxide deposition process step and the second oxide deposition process step may include: the type of silicon source precursor gas including HCD; the type of reactant gas including O2 / H2 gas; the flow rates of the reactant gas and the silicon source precursor gas; the reaction time for each of the reactant gas and the silicon source precursor gas; and the order in which the reactant gas and the silicon source precursor gas enter the ALD tool, wherein the process parameters are configured to control at least one of the thickness, density, and mass of the oxide formed in the barrier dielectric layer.

[0032] In one embodiment, the process parameters for the first silicon nitride deposition process step and the second silicon nitride deposition process step may include: the type of silicon source precursor gas including HCD; the type of reaction gas including NH3 / N2O gas; the flow rates of the reaction gas and the silicon source precursor gas; the reaction time for each of the reaction gas and the silicon source precursor gas; the order in which the reaction gas and the silicon source precursor gas enter the ALD tool; and the number of repetitions and the repetition order.

[0033] In one embodiment, at least one of the multiple silicon nitride deposition process steps may be plasma-enhanced.

[0034] In one embodiment, the first radical oxidation process step and the first oxide deposition process step can be repeated individually, alternately, or in combination thereof to form a tunnel dielectric layer, and the second radical oxidation process step and the second oxide deposition process step can be repeated individually, alternately, or in combination thereof to form a barrier dielectric layer, wherein the process parameters of the first radical oxidation process step and the second radical oxidation process step, as well as the first oxide deposition process step and the second oxide deposition process step, are adjusted during the repetition of the process steps to customize the tunnel dielectric layer and the barrier dielectric layer.

[0035] According to one embodiment of a method for manufacturing a semiconductor device, the method further includes the step of forming a high-voltage (HV) gate oxide layer, an input / output (I / O) gate oxide layer, and a low-voltage (LV) gate oxide layer in a second region of a substrate, wherein a barrier dielectric layer of a customizable ONO layer in the first region and at least one of the HV gate oxide layer, the I / O gate oxide layer, and the LV gate oxide layer are simultaneously formed by at least one of a second radical oxidation process step and a second oxide deposition process step.

[0036] In one embodiment, a multilayer CT layer may include at least three CT sublayers, and wherein the process parameters of a plurality of silicon nitride deposition process steps are modified such that the top CT sublayer adjacent to the barrier dielectric layer is the most oxygen-depleted in the multilayer CT layer, while the bottom CT sublayer adjacent to the tunnel dielectric layer is the most oxygen-rich.

[0037] According to one embodiment of a method for manufacturing a memory device, the method may include the following steps: forming a tunnel oxide layer in a memory region and a logic region of a substrate; forming a customizable charge trapping (CT) layer and a capping layer covering the tunnel oxide layer, wherein the customizable CT layer includes a plurality of CT sublayers, and wherein each CT sublayer is formed by one or more silicon nitride deposition process steps performed in an atomic layer deposition (ALD) chamber; patterning the tunnel oxide layer, the customizable CT layer, and the capping layer to form a memory stack in the memory region while removing these layers in the logic region; and performing at least one radical oxidation process step in the ALD chamber to simultaneously: converting at least the silicon nitride in the capping layer to form a barrier oxide layer covering the customizable CT layer, and converting silicon in the substrate to form a first gate oxide layer in the logic region.

[0038] In one embodiment, the method may further include performing at least one oxide deposition process step in the ALD chamber to simultaneously increase the thickness of the first gate oxide layer and the barrier oxide layer in the logic region.

[0039] In one embodiment, the process parameters for one or more silicon nitride deposition process steps may include: the type of silicon source precursor gas including HCD, the type of reaction gas including NH3 / N2O gas, the flow rates of the reaction gas and silicon source precursor gas, the reaction time for each of the reaction gas and silicon source precursor gas, and the order in which the reaction gas and silicon source precursor gas enter the ALD chamber.

[0040] In one embodiment, process parameters of one or more silicon nitride deposition process steps can be adjusted to produce a CT sublayer having a different thickness, density, and at least one of the Si, O, and N film compositions of silicon nitride in the CT sublayer.

[0041] According to one embodiment of a method for manufacturing a SONOS-based memory device, the method may include the step of forming a memory cell comprising a SONOS transistor and a transport transistor in a memory region of a substrate, the step comprising: forming a tunnel oxide layer in a memory region and a logic region of the substrate; forming a customizable charge trapping (CT) layer and a capping layer covering the tunnel oxide layer, wherein the customizable CT layer comprises a plurality of CT sublayers, and wherein each CT sublayer is formed by one or more silicon nitride deposition process steps performed in an atomic layer deposition (ALD) chamber; patterning the tunnel oxide layer, the customizable CT layer, and the capping layer to form a memory stack in the memory region while removing these layers in the logic region; and forming a barrier oxide layer covering the customizable CT layer and a first gate oxide layer of the transport transistor in the memory region; the method further includes the step of forming an HV gate oxide layer of a high voltage (HV) transistor, an I / O gate oxide layer of an input / output (I / O) transistor, and an LV gate oxide layer of a low voltage (LV) transistor in the logic region. In one embodiment, at least one of the HV gate oxide layer, I / O gate oxide layer, and LV gate oxide layer is formed at least in part by performing at least one radical oxidation process step in an ALD chamber to simultaneously perform the following operations: converting silicon nitride in at least the capping layer in the memory region to form a barrier oxide layer and converting silicon to form a first gate oxide layer, and converting silicon in the substrate in the logic region to at least partially form at least one of the HV gate oxide layer, I / O gate oxide layer, and LV gate oxide layer.

[0042] In one embodiment, the method may further include: performing at least one oxide deposition process step in an ALD chamber to simultaneously increase the thickness of a barrier oxide layer and a first gate oxide layer in the storage region.

[0043] In one embodiment, the transmission transistor and the HV transistor may be of the same type, and the first gate oxide layer and the HV gate oxide layer are formed simultaneously and have approximately the same thickness.

[0044] In one embodiment, process parameters of one or more silicon nitride deposition process steps can be adjusted to produce CT sublayers in which the Si, O, and N film compositions of silicon nitride differ, and wherein, in a customizable CT layer, the top CT sublayer is the most oxygen-deficient, while the bottom CT sublayer is the most oxygen-rich.

[0045] In one embodiment, oxide deposition, radical oxidation, and silicon nitride deposition processes are performed in situ in an ALD chamber, and the process temperature is controlled to be below 650°C.

[0046] In one embodiment, the method may further include the step of forming a barrier oxide layer covering the SONOS transistor and a high-k metal gate (HKMG) covering a first gate oxide layer covering the transport transistor.

[0047] Description of implementation methods

[0048] Figure 1 This is a block diagram showing a cross-sectional side view of a SONOS-based NVM device. Figure 1 In one embodiment shown, the NVM transistor 100 is configured to store a binary value (“0” or “1”) or a multi-level analog value (e.g., 0 to 2) corresponding to the amount and polarity of the trapped charge it holds. n -1) SONOS-type charge-trapping NVM transistor. (See reference...) Figure 1 The NVM cell includes a storage gate (MG) stack 150 formed over a substrate 102. The NVM transistor 100 also includes a source / drain region 104 formed on either side of the MG stack 150 within a shallow positive well (SPW—not shown) in the substrate 102, or optionally within the substrate 102. The SPW may be at least partially encapsulated within a deep negative well (DNW—not shown). In one embodiment, the source / drain region 104 is connected via a channel region 116 beneath the MG stack 150. The NVM transistor 100 includes a tunnel dielectric layer 106, a charge trapping layer 108, and a barrier dielectric layer 110, thereby forming an ONO stack 120. In one embodiment, the charge trapping layer 108 may be multilayered and traps charge injected from the substrate 102 via the FN tunneling effect or other mechanisms. The VNVM of the NVM transistor 100... T and I D The value can vary at least in part due to the amount and polarity of the trapped charge. In one embodiment, a high-k dielectric layer may form at least a portion of the barrier dielectric layer 110. A polysilicon or metal gate layer 112 is configured to cover the ONO stack 120 and may be used as a control gate (CG) or a storage gate (MG). The NVM transistor 100 may also include spacers 114 for providing electrical insulation to adjacent devices or other devices.

[0049] In various implementations, the ONO stack 120 can be formed through a series of process steps, including (thermal and / or radical and / or other) oxidation, (physical, chemical, etc.) deposition, etching, and / or cleaning. These process steps can be performed in a single process chamber / tool ​​or multiple process chambers / tools. In some implementations, current ONO processes limit the compositional variations that can be achieved in the thin layers of the SONOS stack, which are critical at advanced technology nodes such as 22 nm or below. Current ONO formation processes / tools may also suffer from marginality regarding film stoichiometry and uniformity of thickness (e.g., wafer-to-wafer (WTW) thickness and in-wafer (WIW) thickness). This can negatively impact productivity and the quality of the ONO stack by limiting batch sizes to around 50 wafers and reducing the manufacturing plant's capacity to produce the relevant products. At advanced technology nodes, the thermal budgets for certain ONO processes, such as in-situ vapor generation (ISSG) oxidation, in-furnace dry or wet oxidation, and chemical vapor deposition of oxides and nitrides, may be too high. The high thermal budgets of these processes may be sufficient to significantly alter the parameters of baseline CMOS devices, which in turn may require changes to the model of baseline FETs.

[0050] Figure 2A This illustrates the fabrication of a SONOS-based non-volatile memory transistor (e.g., according to embodiments of this disclosure). Figure 1 A representative flowchart illustrating an implementation of a method for stacking oxide-nitride-oxide (ONO) components in an NVM transistor 100. (Refer to...) Figure 2A and Figure 3A The process can begin with a series of pre-steps (step 202), including forming multiple isolation structures or shallow trench isolation (STI) 301 in the wafer or substrate 302. In some embodiments, the pre-steps may also include forming channels, for example... Figure 1 Channel 116 in the middle Figure 1 The source / drain 104, and / or deep wells and / or wells, are located within the substrate. Various processes, including pad oxide formation, wet / dry etching or cleaning, tunnel mask application, and dopant implantation, can be performed according to the practice of those skilled in the art. It will be understood that the aforementioned pre-steps or other pre-steps may be omitted or partially performed prior to the formation of the tunnel dielectric layer. Subsequently, a pre-cleaning process is performed on the substrate surface 303 to remove pad oxide (if present) and / or other residual oxides; this can be a wet or dry process. In one embodiment, it can be a wet process using HF followed by standard cleaning (SC1) and (SC2), and is highly selective for the material of the substrate 302.

[0051] Reference Figure 2A and Figure 2BONO layer, for example Figure 1 The ONO stack 120 best illustrated begins with the formation of a tunneling dielectric in step 204. The tunneling dielectric can be any material and has any thickness suitable for allowing charge carriers to tunnel into the overlying charge trapping layer under applied gate bias, while maintaining a suitable leakage barrier when the transistor is not biased. In some embodiments, the tunneling dielectric can be silicon dioxide, silicon nitride such as oxides of nitride, or combinations thereof, and can be deposited and / or grown by a thermal oxidation process in a furnace utilizing ISSG or radical oxidation. As described above, forming a very thin (e.g., less than 20 Å) tunneling dielectric layer with uniform film stoichiometry and WTW / WIW thickness using the above-described processes under thermal budget conditions below 650°C is challenging. In one embodiment, which may be referred to as a preferred embodiment, a multilayer silicon oxide tunneling dielectric layer 306 can be formed in a single in-situ atomic layer deposition (ALD) chamber capable of radical oxidation, thermal ALD, or plasma-enhanced ALD (PEALD) using batch or single-tooling. In one implementation, both the radical oxidation and ALD deposition processes can be performed in the same ALD chamber. The sequential nature of ALD deposition and radical oxidation, along with the self-limiting surface reaction characteristics, facilitates atomic-level control of film thickness and uniformity with relatively low thermal budgets (e.g., below 650°C). (Refer to...) Figure 2B An example of an ALD chamber or tool 90 is shown. The ALD chamber 90 can be a batch processing tool in which multiple wafers (substrates) can be processed simultaneously. A precursor gas, such as HCD, can be introduced as a silicon source. Other reactive gases, such as ammonia or nitrous oxide, can be enhanced by a plasma source, such as inductively coupled plasma (ICP), before entering the chamber through a buffer nozzle with electrodes. Other reactive gases, such as H2 / O2, can be introduced via a cross-flow injector. It will be understood that... Figure 2B The ALD chamber 90 shown in the best example is merely an example of an ALD tool capable of performing radical oxidation, thermal ALD, and PEALD treatments, and should not be construed as limiting. Other ALD tools capable of performing the radical oxidation and ALD deposition disclosed in this patent document may be used depending on manufacturing requirements and other considerations.

[0052] Reference Figure 3BIn one embodiment, a tunnel dielectric sublayer 306a is formed in an ALD chamber via radical oxidation. This process involves introducing reactant hydrogen (H2) and oxygen (O2) into the ALD chamber in an approximately 1:4 ratio or other configurable ratio without the need for an external ignition event, such as plasma formation. H2 and O2 are allowed to react at temperatures ranging from approximately 300°C to approximately 650°C and at pressures ranging from approximately 0.5 Torr to approximately 10 Torr to form radicals, such as OH radicals, HO2 radicals, or O diradicals, at the surface of substrate 302, which ultimately react directly with and are consumed by a portion of the exposed surface of the silicon substrate 302. An example process / operation table for performing radical oxidation in an ALD chamber in one embodiment is shown below:

[0053] Table 1:

[0054]

[0055] The thickness, quality, and uniformity of the formed tunnel dielectric sublayer 306a can be fine-tuned or customized by modifying or adjusting the process gas sequence, flow rate, order, duration, temperature, gas flow ratio, or other process parameters according to the requirements of the manufactured device.

[0056] Reference Figure 3C Alternatively, a deposition workflow can be used in the same or similar ALD chamber to form the tunnel dielectric sublayer 306b. In one embodiment, a chlorosilane, such as hexachlorosilane Si2Cl6 (HCD), can be a precursor gas or a silicon source gas. Hydrogen (H2) and oxygen (O2) are introduced into the ALD chamber in an approximately 1:4 ratio without the need for an external ignition event, such as plasma formation. H2 and O2 are allowed to react at a temperature approximately in the range of about 300°C to about 400°C and at a pressure approximately in the range of about 0.5 Torr to about 10 Torr to form free radicals, such as OH radicals, HO2 radicals, or O diradicals, which ultimately react with the HCD to form deposited silicon oxide over the surface of the substrate 302. During the same process, the generated free radicals can also react directly with the silicon substrate 302 to form silicon oxide, as explained in the radical oxidation described above. In one embodiment, an example process / operation table for performing silicon oxide deposition in an ALD chamber is as follows:

[0057] Table 2:

[0058]

[0059] Similar to radical oxidation, the thickness, quality, and uniformity of the resulting tunnel dielectric sublayer 306b can be fine-tuned or customized by modifying the process gas sequence, flow rate, duration, temperature, gas flow ratio, or other process parameters according to the requirements of the device being manufactured. In one embodiment, even with reduced thickness, the tunnel dielectric sublayers 306a and 306b produced in radical oxidation or ALD deposition processes can be denser and more uniform per cubic centimeter (cm²) than tunnel dielectric layers formed by other methods via wet oxidation techniques. 3 It consists of essentially fewer hydrogen atoms. The uniform thickness of the tunnel dielectric layer 306, particularly around the STI corner, reduces the non-uniformity of FN injection at the STI 301 corner of the final SONOS device, thereby improving I... D or V T The sigma decreases.

[0060] In implementation, multiple tunnel dielectric sublayers 306a to 306d can be produced by repeating the process individually or alternately with or without modification of process parameters, in combination of both, or in any specified order, such as the radical oxidation described in Table 1 and the ALD oxidation deposition described in Table 2. Each sublayer can be formed up to a predetermined thickness by only one or more radical oxidation process steps (e.g., as shown in Table 1 or modified), only one or more ALD oxidation deposition steps (e.g., as shown in Table 2 or modified), or a combination thereof; and each sublayer can be formed to a thickness reduced to 2 Å or less. Figure 3D As best illustrated, the final tunnel dielectric layer 306 is a stack of multiple tunnel dielectric sublayers 306a to 306d. By controlling and adjusting process parameters such as flow rate, reactants, duration, and temperature in the radical oxidation and ALD deposition processes, a tunnel dielectric layer 306 with customizable desired thickness (WTW and WIW), uniformity, oxide-silicon substrate interface conditions, and film stoichiometry can be achieved. It will be understood that... Figure 3D The four-sublayer tunnel dielectric layer 306 shown is merely an example to illustrate the proposed ALD oxidation / deposition method and should not be construed as limiting. The tunnel dielectric layer 306 may have one or more sublayers, and each sublayer can have different thicknesses, film stoichiometry, densities, or other physical and chemical properties by fine-tuning the ALD radical oxidation and deposition process steps. In one embodiment, the tunnel dielectric layer 306 may be formed with a thickness in the range of approximately 5 Å to 30 Å.

[0061] Reference Figure 2AIn step 206, multiple layers of silicon nitride or oxide nitride (SiO2) can be formed in the same ALD chamber. x O y N z A charge trapping layer. In embodiments, silicon nitride or oxide nitride can have different proportions of silicon (x), oxygen (y), and nitrogen (z) in the formed film. The charge trapping layer can be composed of materials and have a thickness suitable for storing charge and thus changing the threshold voltage of the subsequently formed SONOS device. (See reference...) Figure 4A The charge-trapping dielectric sublayer 308a is formed in the same or similar in-situ ALD chamber used for the tunnel dielectric layer 306. In one embodiment, the process involves flowing a precursor gas HCD as the silicon source, ammonia (NH3) as the nitrogen source, and nitrous oxide (N2O) as the oxygen source. In other embodiments, other chlorosilane gases can be used as the silicon source, and other nitrogen or oxygen source gases can be used, in accordance with the practice of those skilled in the art. In another embodiment, the ammonia or nitrous oxide gas can be plasma-enhanced before being introduced into the ALD chamber to potentially achieve higher silicon nitride deposition rates and better uniformity at lower temperatures. In one embodiment, the silicon nitride ALD deposition process is performed at 650°C, below the temperature of most thermal and chemical vapor deposition processes. In one embodiment, silicon nitride layers as low as 2 Å can be formed in the ALD chamber. An example process / operation table for performing silicon nitride deposition in an ALD chamber is provided below:

[0062] Table 3:

[0063]

[0064] Similar to the silicon oxide ALD process described above, the thickness, uniformity, and oxygen, nitrogen, and / or silicon ratio in the formed silicon nitride can be customized to produce a customizable charge-trapping dielectric sublayer 308a. In one embodiment, the silicon nitride ALD process can leave the already formed tunnel dielectric layer 306 substantially unaffected. (Refer to...) Figure 4B Another charge-trapping dielectric sublayer 308b can be formed on the charge-trapping dielectric sublayer 308a. In one embodiment, the charge-trapping dielectric sublayer 308b can be formed in the same ALD chamber using the process parameters described in Table 3 or any modified process parameters. For example, the flow rate and / or flow time of N2O gas can be increased to produce an oxygen-rich nitride layer, or the flow rate and / or flow time of HCD gas and ammonia gas can be adjusted or otherwise increased or decreased to produce a silicon-rich nitride layer and a nitrogen-rich nitride layer, respectively. (Refer to...) Figure 4CA similar ALD deposition process as described in Table 3 can be used to form another charge-trapping dielectric sublayer 308c on charge-trapping dielectric sublayer 308b, with or without modification of process parameters. In one embodiment, charge-trapping dielectric sublayers 308a to 308c can collectively form the charge-trapping dielectric layer 308 of the finished SONOS device. It will be understood that... Figure 4C The three-layer charge-trapping dielectric layer 308 shown is merely an example to illustrate the proposed silicon nitride ALD deposition method and should not be construed as limiting. The charge-trapping dielectric layer 308 may have one or more sublayers, and each sublayer may have different thicknesses, Si, O, and N film compositions in the silicon nitride, or other physical and chemical properties by fine-tuning the ALD deposition process. In one embodiment, the charge-trapping dielectric layer 308 may be a multilayer silicon nitride with an oxygen-rich gradient increasing from top to bottom, wherein the top sublayer 308c is the silicon nitride sublayer with the least oxygen content, and the bottom sublayer 308a is the silicon nitride sublayer with the most oxygen content.

[0065] As used herein, the terms “oxygen-rich” and “silicon-rich” are relative to stoichiometric silicon nitride of (Si3N4) composition and a refractive index (RI) of about 2.0, as commonly used in the art. Therefore, “oxygen-rich” silicon nitride necessarily shifts from stoichiometric silicon nitride, or sometimes referred to as silicon nitride or oxide nitride (oxygen-containing silicon nitride), to a higher weight percent of silicon and oxygen (i.e., nitrogen reduction). Thus, oxygen-rich silicon nitride or oxide nitride films are more like silicon dioxide, and the RI decreases to 1.45 RI of pure silicon dioxide. Similarly, films described herein as “silicon-rich” necessarily shift from stoichiometric silicon nitride to a higher weight percent of silicon, where oxygen is less than in “oxygen-rich” films. Thus, silicon-rich silicon nitride films are more like silicon, and the RI increases to 3.5 RI of pure silicon. Throughout this document, “silicon nitride” and “silicon oxide nitride” will be used interchangeably, and the resulting films may or may not have an oxygen content.

[0066] In one implementation, it may be desirable to produce a charge-trapping dielectric film in which most of the charge trappings are distributed in the upper portion of the film. This minimizes charge leakage through the underlying tunneling dielectric layer. Figure 4C Taking the charge-trapping dielectric layer 308 as an example, the process parameters during ALD deposition of the charge-trapping dielectric sublayer 308a can be configured to produce an oxygen-rich, nitrogen-poor silicon nitride film. Using the same ALD chamber and adjusting the process parameters, the charge-trapping dielectric sublayer 308c can be formed as an oxygen-poor, nitrogen-rich silicon nitride film containing most of the charge traps in the entire multilayer charge-trapping dielectric layer 308.

[0067] In some embodiments, a thin silicon oxide film can be formed within the charge-trapping nitride layer and between two nitride layers. (See also...) Figure 4D A thin dielectric film 330 can be formed on the lower charge-trapping dielectric layer 308'. The lower charge-trapping dielectric layer 308' is one or more silicon nitride sublayers formed similarly to the charge-trapping dielectric layer 308. The thin dielectric film 330 can be silicon oxide or highly oxygen-rich silicon nitride, and can be formed using ALD radical oxidation or ALD oxide deposition similar to the formation of the tunnel dielectric sublayers 306a to 306d described above. Silicon oxide can be deposited directly above the lower charge-trapping dielectric layer 308', or radicals can convert a portion of the silicon nitride in the lower charge-trapping dielectric layer 308' into silicon oxide or highly oxygen-rich nitride. In embodiments, the thin dielectric film can be a single layer or have multiple sublayers, and each sublayer is formed in the same ALD chamber using the ALD radical oxidation or oxide deposition process steps described above.

[0068] Reference Figure 4E Subsequently, an upper charge-trapping dielectric layer 332 is formed over the thin dielectric film 330, making the finished charge-trapping dielectric layer 350 a nitride (332)-oxide (330)-nitride (308') (bottom) (NON) stack 350 with a total thickness in the range of approximately 50 Å to 150 Å. In one embodiment, similar to the bottom charge-trapping dielectric layer 308', the upper charge-trapping dielectric layer 332 includes one or more silicon nitride sublayers (not shown) formed similarly to the charge-trapping dielectric sublayers 308a to 308c. The upper charge-trapping dielectric layer 332 is also customizable; and by fine-tuning the ALD deposition process, each silicon nitride sublayer can have a different thickness, the Si, O, N film ratio in the formed silicon nitride, or other physical and chemical properties. In one embodiment, the thin dielectric film 330 significantly reduces the probability of electrons accumulating at the boundary of the upper charge trapping layer 332 during programming tunneling into the lower charge trapping layer 308', thereby achieving lower leakage current than conventional memory devices. In a preferred embodiment, the nitride sublayer in the upper charge trapping dielectric layer 332 can be customized to be oxygen-depleted to contain most of the charge traps, while the nitride sublayer in the lower charge trapping dielectric layer 308' is oxygen-rich.

[0069] Reference Figure 2AIn step 208, a barrier dielectric layer 310 is formed over the charge-trapping dielectric layer 308 or the non-charge-trapping dielectric layer 350. This process begins with the formation of a barrier dielectric sublayer 310a over the charge-trapping dielectric layer 308 or 350. In one embodiment, the barrier dielectric sublayer 310a is silicon oxide and is formed by radical oxidation as previously described in Table 1 or by ALD oxide deposition as described in Table 2, or by modifications, combinations, and variations thereof. Silicon oxide is deposited over the charge-trapping dielectric layer 308 or 350, or radicals can convert a portion of the silicon oxynitride in the charge-trapping dielectric layer 308 or 350 into silicon oxide. (Refer to...) Figure 5B Subsequently, other barrier dielectric sublayers 310b to 310c can be formed. In one embodiment, the barrier dielectric sublayers 310b to 310c can be formed as a silicon oxide film by similar radical oxidation or ALD oxide deposition, the silicon oxide film having a thickness, uniformity, and quality that can be customized by modifying the process performed in the ALD chamber. Therefore, the barrier dielectric layer 310 can be a single layer or multiple layers of silicon oxide with a total thickness in the range of approximately 10 Å to 100 Å. (Refer to...) Figure 5C Then, an ONO stack layer 320 is formed over at least a portion of the substrate 302, all of which is performed using the same in-situ ALD tool. (See reference...) Figure 5D In one implementation, the ONO stack layer 320 can be patterned to form one or more ONO stacks 320' for SONOS-based transistors, and Figure 1 The NVM transistor 100 has a similar ONO stack 120. A mask may be formed on or over the ONO stack 320, and the ONO stack 320 may be etched to form one or more ONO stacks 320' covering the substrate 302. In step 210, the manufacturing process may continue with the remaining processes. Process steps such as source / drain formation, spacer formation, and memory gate formation will be performed in accordance with the practice of those skilled in the art. It will be understood that the above process steps may be performed before, during, or after the formation of the ONO stack 320 (in steps 204 to 208) without departing from the principles of this disclosure.

[0070] In one alternative implementation, refer to Figure 5EInstead of forming an ONO stack directly above the substrate 302 as a SONOS-based transistor, the ONO stack layer 320 can be formed as part of the storage stack layer 540 of the floating gate transistor 550. In one embodiment, the ONO stack layer 320, which serves as the barrier dielectric layer of the floating gate transistor 550, is formed above the tunnel oxide layer 502 and the floating gate layer 504. The tunnel oxide layer 502, which is primarily silicon oxide, and the floating gate layer 504, which can be polysilicon, can be formed in the same ALD chamber as the ONO stack layer 320, or using other techniques practiced by those skilled in the art.

[0071] Reference Figure 6 This illustration shows a portion of a SONOS-based non-volatile memory (NVM) device 600 formed over a single substrate 102. In one embodiment, the substrate 102 is divided into a memory region where memory cells 620 are disposed and a logic region where HV MOS 604, I / O MOS 606, and LV MOS 608 are disposed. In one embodiment, only individual devices of each type (i.e., memory cells 620, HV MOS 604, I / O MOS 606, and LV MOS 608) are shown for illustrative purposes. Multiple devices of each type and other semiconductor devices may be disposed within the SONOS-based NVM device 600 and may be formed simultaneously or sequentially. Figure 6 As best shown in the diagram, the NVM transistor 100 may have a polysilicon or high-k metal gate (HKMG) layer 634 configured to cover the ONO stack 320' and may serve as the control gate (CG) or storage gate (MG) of the memory cell 620.

[0072] like Figure 6 As best illustrated, in a dual-transistor (2T) configuration, memory cell 620 also includes a transfer transistor or select transistor 602 disposed adjacent to the SONOS-based NVM transistor 100 (or referred to as a memory transistor). The transfer transistor 602 is, for example, a conventional MOSFET sharing a common substrate connection or internal node with the NVM transistor 100. In one embodiment, the transfer transistor 602 includes a high-k metal gate (HKMG) or polysilicon select gate (collectively, “SG”) 632 configured to cover an oxide or high-k dielectric gate dielectric layer 612. The SG 632 is appropriately biased to turn on or off the channel beneath the transfer transistor 602. In another embodiment, memory cell 620 may employ a single-transistor (1T) configuration and have only the NVM transistor 100.

[0073] Reference Figure 6In the logic region, the HV MOS transistor 604, I / O MOS transistor 606, and LV MOS transistor 608 are field-effect transistors (FETs), each having a logic gate 632 covering an HKMG gate or polysilicon gate formed by the HV gate oxide layer 614, I / O gate oxide layer 616, and LV gate oxide layer 618. In one embodiment, the HV gate oxide layer 614 has the greatest thickness, followed by the I / O gate oxide layer 616, and then the LV gate oxide layer 618. In one embodiment, the transfer transistor 602 in the memory region may have a similar or identical structure and dimensions to one of the HV MOS transistor 604, I / O MOS transistor 606, and LV MOS transistor 608.

[0074] Figure 7 This is a process flow diagram illustrating key manufacturing steps of integrating SONOS or NVM transistors (in the memory region) into a baseline complementary metal-oxide-semiconductor (CMOS) process flow (in the logic region) according to one embodiment of this disclosure. (Refer to...) Figure 7 The process begins with several pre-steps, including forming multiple isolation structures or shallow trench isolation (STI) in step 702, forming pad oxide, forming source / drain electrodes, forming wells, pre-cleaning the substrate, etc. Pad oxide 870 can be formed over substrate 102 in either the memory region or the logic region. In one embodiment, pad oxide 870 can be silicon dioxide (SiO2) with a thickness from about 10 nanometers (nm) to about 20 nm and can be formed in an ALD chamber using radical oxidation or oxide deposition processes as described above, or other oxidation or deposition processes known in the art. It will be understood that in some embodiments, pad oxide 870 may not be necessary or may not be formed. Dopant is infused into substrate 102 through pad oxide 870 (if present) to form (deep and shallow) wells, source / drain electrodes, or channels for one or more transistors, namely NVM transistor 100 and transport transistor 602 in the memory region, and MOS transistors 604, 606, 608 in the logic region. It will be understood that, without departing from the principles of this disclosure, one or more pre-steps may be performed later in the manufacturing process.

[0075] Next, refer to Figure 7 and Figure 8A In steps 704 and 702, the surface of substrate 102 in the storage region is cleaned or pre-cleaned, and multiple dielectric layers are formed. Subsequently, in step 706, a mask is formed on or overlaying the dielectric layers, and the dielectric layers are etched to form an NV gate stack in the storage region. Pre-cleaning can be a wet or dry process to remove pad oxide 870 on substrate 102 (at least in the storage region).

[0076] Reference Figure 7 and Figure 8A In step 704, the dielectric layer or NV gate stack layer process begins by forming a tunnel dielectric layer 306 in the memory region and can extend to the logic regions where MOS transistors 604, 606, and 608 will be formed. In one embodiment, the tunnel dielectric layer 306 can be any material and has any thickness suitable for allowing charge carriers to tunnel into the overlying charge trapping layer under applied gate bias, while maintaining a suitable leakage barrier when the multi-stage NVM transistor is not biased. As previously at least in Figure 2A and Figures 3A to 3D As described in the corresponding description, in a preferred embodiment, the tunnel dielectric layer 306 may include one or more layers formed by elements in an ALD chamber, for example... Figure 2B The silicon oxide sublayer is formed by a radical oxidation or ALD oxide deposition process in the ALD chamber 90. By controlling and modifying process parameters such as flow rate, reactants, duration, and temperature in the radical oxidation and ALD deposition processes, tunnel dielectric layers 306 with customizable desired thickness (WTW and WIW), uniformity, oxide-silicon substrate interface conditions, and film stoichiometry can be achieved.

[0077] Refer again Figure 8A In step 704, a charge trapping layer 308 or 350 is formed on or covering the tunnel dielectric 306. In one embodiment, the charge trapping layer 308 or 350 may be formed by means of, for example, previously, Figures 4A to 4E The multilayer silicon nitride (one or more sublayers) formed by the ALD deposition process steps described in their respective descriptions. In one embodiment, as... Figure 4E As best illustrated, the charge trapping layer may have at least one sublayer (e.g., as shown in the diagram). Figure 4C The multilayer charge trapping layer 308 (308a to 308c) is best shown in the figure, and each sublayer can have different thicknesses, Si, O, N film ratios, or other physical and chemical properties by fine-tuning the ALD deposition process steps.

[0078] In another embodiment, the charge trapping dielectric layer 350 is a NON layer comprising multiple layers, including: a lower charge trapping layer 308', which is at least physically closer to the tunnel dielectric layer 306; and an upper charge trapping layer 332, which has one or more nitride sublayers and is oxygen-deficient relative to the oxygen-rich lower charge trapping layer 308', which also has one or more sublayers, and includes most of the charge traps distributed within the multilayer charge trapping layer 350. Figure 4EAs best illustrated, a thin oxide film may be formed between the upper charge-trapping dielectric layer 332 and the lower charge-trapping dielectric layer 308' to significantly reduce the probability of electron charge accumulating at the boundary of the upper charge-trapping layer 332 tunneling into the lower charge-trapping layer 308' during programming, thereby producing lower leakage current than conventional memory devices. In one embodiment, all sublayers of the charge-trapping dielectric layer 308 or 350 may be formed in the same ALD chamber (in situ) via radical oxidation, oxide deposition, or nitride deposition process steps.

[0079] Refer again Figure 7 and Figure 8A In step 706, a capping layer 802 is formed on or covering the charge trapping layer 308 or 350. In some embodiments, as shown, the capping layer 802 is a multilayer capping layer that includes at least a lower capping layer or a first capping layer 802a covering the charge trapping layer 308 or 350 and a second capping layer 802b covering the first capping layer 802a.

[0080] In one embodiment, the first capping layer 802a may comprise a high-temperature oxide (HTO), such as silicon oxide (SiO2), with a thickness between 2.0 nm and 4.0 nm, deposited using a low-pressure chemical vapor deposition (LPCVD) thermal oxidation process. In one embodiment, the second capping layer 802b may comprise a silicon nitride, silicon-rich silicon nitride, or silicon-rich silicon oxynitride layer with a thickness between 2.0 nm and 4.0 nm, formed using a CVD process employing a mixture of N2O / NH3 and DCS / NH3 gases. In another embodiment, the capping layer 802 may also be formed in an ALD chamber using radical oxidation, oxide deposition, or nitride deposition process steps as described in the preceding paragraphs, such as Tables 1 to 3 and their corresponding descriptions.

[0081] Still refer to Figure 7 and Figure 8A In step 706, a sacrificial oxide layer 806 is formed on or covering the capping layer 802. In one embodiment, the sacrificial oxide layer 806 may comprise a high-temperature oxide (HTO) layer with a thickness between 2.0 nm and 4.0 nm, grown by a thermal oxidation process or free radical oxidation. In another embodiment, the sacrificial oxide layer 806 may be formed in an ALD chamber using free radical oxidation or oxide deposition process steps as described above.

[0082] Next, still refer to Figure 7 and Figure 8A A patterned mask layer 850 is formed on or covering the sacrificial oxide layer 806, and references... Figure 8BThe sacrificial oxide layer 806, capping layer 802, and charge trapping layers 308 or 350, as well as the tunnel dielectric layer 306, are etched or patterned to form an NV gate stack 860. In one embodiment, the NV gate stack 860 may be configured to substantially cover the channel of the NVM transistor 100 in the memory region. The etching or patterning process may also remove the individual dielectric layers of the NV gate stack 860 from the logic region (step 706). The patterning mask layer 850 may include a photoresist layer patterned using standard photolithography techniques, and the NV gate stack 860 layers in the logic region may be etched or removed using a dry etching process comprising one or more individual steps to stop on the surface of the substrate 102 or the unremoved pad oxide 870 (if present). In one embodiment, a well (not shown) may be formed in the logic region. It will be understood that Figure 8B It is a representative image and one or more NV gate stacks 860 can be formed in the same patterning process step, in the memory region or other region on the substrate 102.

[0083] Reference Figure 7 and Figure 8C In a highly selective cleaning process, the top portion or substantially all of the second capping layer 802b in the sacrificial oxide layer 806 and the multilayer capping layer 802 is removed from the NV gate stack 860 (step 708). This cleaning process further removes any oxides remaining in the memory regions and logic regions outside the NV gate stack 860, such as oxides in the tunnel dielectric layer 306 and / or the pad oxide 870, to prepare the substrate 102 for oxide formation.

[0084] Next, refer to Figure 7 and Figure 8DIn step 710, a barrier dielectric layer 310 of the NVM transistor 100, a transfer transistor gate oxide layer 612 in the memory region (in the presence of a 2T configuration), and an LV gate oxide layer 618, an I / O gate oxide layer 616, and an HV gate oxide layer 614 are formed. In one embodiment, an oxidation process is performed to oxidize the remaining portions of the first capping layer 802a and / or the second capping layer 802b of the multilayer capping layer 802, and optionally to oxidize a portion of the charge trapping dielectric layer 308 or 350 to form a barrier dielectric layer 310 covering the charge trapping dielectric layer 308 or 350. In one embodiment, the oxidation process is adapted to oxidize or consume the remainder of the first capping layer 802a or the second capping layer 802b, or optionally oxidize or consume a portion of the charge trapping dielectric layer 308 or 350, to form the barrier dielectric layer 310 and the gate oxide layer 612 (if present) of the transfer transistor 602 in the storage region, while oxidizing at least a portion of the substrate 102 in which the I / O MOS 606, LV MOS 608, or HV MOS 604 is disposed, to form the gate oxide layer in the logic region. In one embodiment, the oxidation process may include in-situ radical oxidation performed in an ALD chamber, such as ALD chamber 90. This in-situ radical oxidation process can be compared with Table 1, Figures 5A to 5C And similar to the ALD radical oxidation process steps described in its corresponding description, wherein one or more silicon oxide sublayers are formed in the NVM transistor 100 in the storage region (e.g., as... Figure 5B(310a to 310c are best shown in the diagram). In one embodiment, the silicon oxide in the barrier dielectric layer 310 is formed by a radical reaction or by ultimately converting the capping layer 802 or possibly the top portion of the charge-capped dielectric layer 308 or 350 into nitrides or oxides of nitride. In one embodiment, radicals such as OH radicals, HO2 radicals, or O diradicals generated during the in-situ ALD radical oxidation process step may also react and consume the silicon substrate 102 to form one or more sublayers in the gate oxide layer 612 of the transport transistor in the memory region and the gate oxide layers 614, 616, 618 in the logic region. The process parameters of the in-situ ALD radical oxidation process step (e.g., Table 1) can be modified to produce oxide sublayers with different thicknesses, qualities, uniformities, stoichiometry, or other chemical and physical properties in both the memory and logic regions. The free radical oxidation process steps can be repeated, alternately repeated, or modified to achieve the ideal thickness T1 of the barrier dielectric layer 310, the ideal thickness T2 of the gate oxide layer 612 of the transport transistor, and the ideal thicknesses T3, T4, and T5 of the gate oxide layers 614, 616, and 618 of the HV MOS 604, I / O MOS 606, and LV MOS 608, respectively. In one embodiment, T1 can be in the approximate range of 30 Å to 50 Å, T2 can be in the approximate range of 50 Å to 150 Å, T3 can be in the approximate range of 50 Å to 150 Å, T4 can be in the approximate range of 50 Å to 150 Å, and T5 can be in the approximate range of 10 Å to 30 Å.

[0085] Alternatively or additionally, in-situ ALD oxide deposition (e.g., as shown in Table 2 or modified thereof) can be performed in the same ALD chamber to form one or more oxide sublayers in at least one of the barrier dielectric layer 310 and the gate oxide layers 612, 614, 616, 618. (See Table 2.) Figures 5A to 5CAs previously described in its corresponding description, the free radicals generated in the ALD chamber can react with silicon source gases such as HCD or oxynitride / nitride or silicon substrate to form one or more silicon oxide sublayers. In embodiments, in-situ ALD oxide deposition and free radical oxidation processes, which can be performed in the same ALD chamber, can be repeated, modified, alternated, or combined as described above until predetermined thicknesses T1 to T5 of the respective dielectric / oxide layers 310, 612, 614, 616, 618 are achieved. In alternative embodiments, sometimes the in-situ ALD oxide deposition or free radical oxidation processes may not be applied to all regions. A mask (not shown) can be applied to protect one or more regions so that the gate oxide layer therein is not affected by subsequent free radical oxidation or ALD oxide deposition processes. In one example, a mask (not shown) can be used to protect the gate oxide layer 618 of the LV MOS 608 in the logic region after thickness T5 is reached so that no additional oxide is added to its thickness in subsequent in-situ ALD process steps (free radical oxidation, deposition, or both). In another example, the gate oxide layer 612 of the transfer transistor 602 and the gate oxide layer 614 of the HV MOS 604 can be substantially identical and can be formed simultaneously or sequentially in the same process step. A primary objective and advantage of fabricating one or more gate oxides of the barrier dielectric layer 310 of the NVM transistor and the gate oxides of the MOS transistors 602, 604, 606, and 608 in in-situ ALD process steps (both radical oxidation and oxide deposition) in the same or similar ALD chamber / tool ​​is that the oxide sublayers and individual layers are formed with a relatively low thermal budget (below 650°C), allowing the CMOS process flow in the logic region to be unaffected. Another objective and advantage is that the NON stack 320 of the NVM transistor 100 and the gate oxide layers 612, 614, 616, and 618 are highly customizable by changing the configuration of the in-situ process steps in the ALD chamber or tool. In one implementation, the ONO layer of the SONOS transistor and the gate oxide layers 612, 614, 616, 618 of all FETs are formed in situ within the same ALD chamber or tool.

[0086] In alternative embodiments, at least a portion of the gate oxide layers 612, 614, 616, 618 may be formed using RTO, furnace oxidation, free radical oxidation, CVD, in-situ vapor generation (ISSG), or combinations thereof. These oxidation process steps may be performed in separate process tools.

[0087] In this embodiment, the LV gate oxide layer 618, the I / O gate oxide layer 616, and the HV gate oxide layer 614 can be formed simultaneously or individually. Subsequently, in Figure 8E As best illustrated, in step 710, the LV gate oxide layer 618, the I / O gate oxide layer 616, and the HV gate oxide layer 614 are patterned. Although only one of each type of transistor (SONOS NVM transistor, transport transistor, HV MOS transistor, I / O MOS transistor, LV MOS transistor) is shown, it will be understood that each type ( Figure 8D Multiple transistors (not shown) can be manufactured simultaneously or sequentially using the methods and process steps described above.

[0088] Finally, a standard or baseline CMOS process flow is continued to substantially complete the front-end device fabrication (step 712). The process flow may include forming HKMG, spacers, channels, source / drain regions, etc., for each type of transistor. In one embodiment, the completed NVM transistor 100, along with HV transistor 604, I / O transistor 606, or LV MOS transistor 608, may be configured to form an NVM cell 620. In an alternative embodiment, the transfer transistor 602 may have a different structure than the HV transistor 604, I / O transistor 606, or LV MOS transistor 608, for example, a different gate oxide thickness. In another alternative embodiment, the memory cell 620 may contain only the NVM transistor 100 in a single-transistor configuration.

[0089] Therefore, embodiments of SONOS-based non-volatile memory, including manufacturing methods for customizable ONO stacks, and methods for integration into baseline CMOS process flows are described. Although this disclosure has been described with reference to specific exemplary embodiments, it will be apparent that various modifications and changes can be made to these embodiments without departing from the broader spirit and scope of this disclosure. Therefore, the specification and drawings should be considered illustrative rather than restrictive.

[0090] An abstract of this disclosure is provided in accordance with 37 CFR §1.72(b) to enable the reader to quickly determine the nature of one or more embodiments of the technical disclosure. The abstract is submitted in the understanding that it will not be used to interpret or limit the scope or meaning of the claims. Furthermore, as can be seen from the above detailed description, various features are combined in a single embodiment for the purpose of simplifying this disclosure. This method of disclosure should not be construed as reflecting an intention that the claimed embodiment requires more features than expressly listed in each claim. Rather, as reflected in the appended claims, the subject matter of the invention lies in fewer than all features of a single disclosed embodiment. Therefore, the appended claims are thus incorporated into the detailed description, wherein each claim exists independently as a separate embodiment.

[0091] In the description, mentioning an embodiment or embodiment means that a particular feature, structure, or characteristic described in connection with that embodiment is included in at least one embodiment of the circuit or method. The phrase "an embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment.

Claims

1. A method for manufacturing a semiconductor device, comprising: The substrate is divided into a first region and a second region; A customizable oxide-nitride-oxide ONO stack is formed in the first region, including: At least one of a first radical oxidation process step and a first oxide deposition process step is performed in an atomic layer deposition (ALD) tool to form a tunnel dielectric layer covering the substrate; Multiple silicon nitride deposition process steps are performed in the ALD tool to form a multilayer charge-trapping CT layer, including: The process parameters of the first silicon nitride deposition process step in the plurality of silicon nitride deposition process steps are determined to form the first CT sublayer; Modify at least one of the process parameters; Perform a second silicon nitride deposition process step to form a second CT sublayer covering the first CT sublayer; and At least one of a second radical oxidation process step and a second oxide deposition process step is performed in the ALD tool to form a barrier dielectric layer covering the multilayer CT layer in the first region, wherein the multilayer CT layer comprises at least three CT sublayers, and wherein the process parameters of the plurality of silicon nitride deposition process steps are modified such that the top CT sublayer adjacent to the barrier dielectric layer in the multilayer CT layer is the most oxygen-depleted, while the bottom CT sublayer adjacent to the tunnel dielectric layer is the most oxygen-rich.

2. The method according to claim 1, wherein, The silicon nitride includes oxygen-containing silicon oxynitride.

3. The method according to claim 1, wherein, The customizable ONO stacking process steps are performed in situ using the same ALD tool.

4. The method according to claim 1, wherein, The silicon, oxygen, and nitrogen film compositions of silicon nitride in the first CT sublayer and the second CT sublayer are different.

5. The method according to claim 1, wherein, The first CT sublayer is oxygen-rich silicon nitride, resulting in virtually no charge traps in the first CT sublayer, while the second CT sublayer is oxygen-depleted silicon nitride, resulting in a high density of charge traps in the second CT sublayer.

6. The method according to claim 5, further comprising: Multiple third silicon nitride deposition process steps are performed to form multiple third CT sublayers disposed between the first CT sublayer and the second CT sublayer, wherein the process parameters of the multiple third silicon nitride deposition process steps are adjusted such that the oxygen enrichment level of the multiple third CT sublayers is between the oxygen enrichment level of the first CT sublayer and the oxygen enrichment level of the second CT sublayer.

7. The method according to claim 5, further comprising: At least one of a third radical oxidation process step and a third oxide deposition process step is performed in the ALD tool to form a thin oxide film covering the first CT sublayer and below the second CT sublayer, wherein the thin oxide film is formed to reduce the tunneling of electron charge accumulated at the boundary of the second CT sublayer into the first CT sublayer.

8. The method according to claim 1, wherein, The process parameters for the first free radical oxidation process step and the second free radical oxidation process step include: Including the types of reacting gases in the O2 / H2 gas reaction; The flow rate of the reactive gas entering the ALD tool; The reaction time for each reactant gas; The order in which the reactive gases enter the ALD tool; and The number of repetitions and the repetition order, wherein the process parameters are configured to control at least one of the thickness, density, and mass of the oxide formed in the tunnel dielectric layer.

9. The method according to claim 1, wherein, The process parameters for the first oxide deposition process step and the second oxide deposition process step include: Including the types of silicon source precursor gases for hexachlorosilane HCD; Including the types of reacting gases in the O2 / H2 gas reaction; The flow rates of the reactant gas and the silicon source precursor gas; The reaction times of the reactant gas and the silicon source precursor gas, respectively; and The order in which the reactant gas and the silicon source precursor gas enter the ALD tool, wherein the process parameters are configured to control at least one of the thickness, density, and mass of the oxide formed in the barrier dielectric layer.

10. The method according to claim 1, wherein, The process parameters for the first silicon nitride deposition process step and the second silicon nitride deposition process step include: Including the types of silicon source precursor gases for hexachlorosilane HCD; Including the types of reacting gases in the NH3 / N2O reaction; The flow rates of the reactant gas and the silicon source precursor gas; and The reaction times of the reactant gas and the silicon source precursor gas are as follows; The order in which the reactive gas and the silicon source precursor gas enter the ALD tool; and Number of repetitions and order of repetition.

11. The method according to claim 1, wherein, At least one of the plurality of silicon nitride deposition process steps is plasma-enhanced.

12. The method according to claim 1, wherein: The first free radical oxidation process step and the first oxide deposition process step are repeated individually, alternately, or in combination of the above to form the tunnel dielectric layer; and The second free radical oxidation process step and the second oxide deposition process step are repeated individually, alternately, or in combination of both to form the barrier dielectric layer, wherein the process parameters of the first free radical oxidation process step and the second free radical oxidation process step, as well as the first oxide deposition process step and the second oxide deposition process step, are adjusted during the repeated process steps to customize the tunnel dielectric layer and the barrier dielectric layer.

13. The method according to claim 1, further comprising: A high-voltage HV gate oxide layer, an input / output (I / O) gate oxide layer, and a low-voltage LV gate oxide layer are formed in the second region of the substrate, wherein the barrier dielectric layer of the customizable ONO stack in the first region and at least one of the HV gate oxide layer, the I / O gate oxide layer, and the LV gate oxide layer are formed simultaneously by at least one of the second radical oxidation process step and the second oxide deposition process step.

14. A method for manufacturing a storage device, comprising: A tunnel oxide layer is formed in the storage and logic regions of the substrate; A customizable charge-trapping CT layer and capping layer are formed over the tunnel oxide layer, wherein the customizable CT layer comprises a plurality of CT sublayers, and wherein each of the CT sublayers is formed by one or more silicon nitride deposition process steps performed in an atomic layer deposition (ALD) chamber, the one or more silicon nitride deposition process steps having process parameters including the following: Including the types of silicon source precursor gases for hexachlorosilane HCD; Including the types of reacting gases in the NH3 / N2O reaction; The flow rates of the reactant gas and the silicon source precursor gas; The reaction times of the reactant gas and the silicon source precursor gas, respectively; and The order in which the reactant gas and the silicon source precursor gas enter the ALD chamber; The tunnel oxide layer, the customizable CT layer, and the capping layer are patterned to form a storage stack in the storage region, while the tunnel oxide layer, the customizable CT layer, and the capping layer are removed from the logic region; and At least one radical oxidation process step is performed simultaneously in the ALD chamber to: convert silicon nitride in at least the capping layer to form a barrier oxide layer covering the customizable CT layer, and convert silicon in the substrate to form a first gate oxide layer in the logic region.

15. The method of claim 14, further comprising: At least one oxide deposition process step is performed in the ALD chamber to simultaneously increase the thickness of the first gate oxide layer and the barrier oxide layer in the logic region.

16. The method of claim 14, wherein, Adjust the process parameters of the one or more silicon nitride deposition process steps to produce a CT sublayer with different thicknesses, densities, and at least one of the Si, O, and N film compositions of silicon nitride in the CT sublayer.

17. A method for manufacturing a memory device based on semiconductor-oxide-nitride-oxide-semiconductor (SONOS), comprising: A memory cell, including a SONOS transistor and a transport transistor, is formed in the memory region of the substrate, comprising: A tunnel oxide layer is formed in the storage region and logic region of the substrate; A customizable charge-trapping CT layer and capping layer are formed over the tunnel oxide layer, wherein the customizable CT layer comprises at least three CT sublayers, and wherein each of the CT sublayers is formed by one or more silicon nitride deposition process steps performed in an atomic layer deposition (ALD) chamber, wherein the process parameters of the one or more silicon nitride deposition process steps are modified such that the top CT sublayer of the at least three CT sublayers in the customizable CT layer is the most oxygen-deficient, while the bottom CT sublayer adjacent to the tunnel oxide layer is the most oxygen-rich; The tunnel oxide layer, the customizable CT layer, and the capping layer are patterned to form a storage stack in the storage region, while the tunnel oxide layer, the customizable CT layer, and the capping layer are removed from the logic region; and A barrier oxide layer covering the customizable CT layer and a first gate oxide layer of the transmission transistor are formed in the storage region; and An HV gate oxide layer for a high-voltage HV transistor, an I / O gate oxide layer for an input / output I / O transistor, and an LV gate oxide layer for a low-voltage LV transistor are formed in the logic region, wherein at least one of the HV gate oxide layer, the I / O gate oxide layer, and the LV gate oxide layer is formed by performing at least one radical oxidation process step in the ALD chamber to simultaneously perform the following operations: converting silicon nitride in at least the capping layer in the memory region to form the barrier oxide layer and converting silicon to form the first gate oxide layer, and converting silicon in the substrate in the logic region to at least partially form at least one of the HV gate oxide layer, the I / O gate oxide layer, and the LV gate oxide layer.

18. The method of claim 17, further comprising: At least one oxide deposition process step is performed in the ALD chamber to simultaneously increase the thickness of the barrier oxide layer and the first gate oxide layer in the storage region.

19. The method according to claim 17, wherein, The transmission transistor and the HV transistor are of the same type, and the first gate oxide layer and the HV gate oxide layer are formed simultaneously and have approximately the same thickness.

20. The method of claim 17, wherein, The process parameters of one or more silicon nitride deposition process steps are adjusted to produce the CT sublayer, wherein the Si, O and N film compositions of silicon nitride in the CT sublayer are different, and wherein, in the customizable CT layer, the top CT sublayer is the most oxygen-deficient, while the bottom CT sublayer is the most oxygen-rich.

21. The method according to claim 18, wherein, The oxide deposition process, the free radical oxidation process, and the silicon nitride deposition process are performed in situ in the ALD chamber, and the process temperature is controlled to be below 650°C.

22. The method of claim 17, further comprising: A barrier oxide layer covering the SONOS transistor and a high-K metal gate HKMG covering the first gate oxide layer of the transmission transistor are formed.

Citation Information

Patent Citations

  • Non volatile memory device possessing charge trapping layer and its manufacture method

    CN101170135A

  • Method of fabricating a charge-trapping gate stack using a CMOS process flow

    CN106062957A