High-temperature-resistant slow-release foamed material, preparation method and application thereof

By preparing a high-temperature resistant slow-release foaming material composed of mesoporous nanostructured inorganic silica gel and surfactant, the problem of rapid dissolution of slow-release materials at high temperatures was solved, and the effect of long-term stable release of foaming agent in high-temperature wells was achieved.

CN120059706BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202311602422.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-28
Publication Date
2026-11-24
Estimated Expiration
2043-11-28

AI Technical Summary

Technical Problem

Existing slow-release materials dissolve and decompose rapidly at high temperatures, resulting in the rapid release of surfactants and a short duration of sustained release, which is insufficient to meet the requirements of high-temperature downhole applications.

Method used

The high-temperature resistant slow-release foaming material with mesoporous nanostructure is mainly composed of inorganic silica gel and surfactant. It is prepared by hydrolysis and condensation to form porous nanoparticle aggregates, which are suitable for high-temperature downhole environments.

Benefits of technology

Achieving long-term stable release of foaming agents in high-temperature downhole environments extends the duration of sustained release and reduces the need for frequent well opening and chemical injection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120059706B_ABST
    Figure CN120059706B_ABST
Patent Text Reader

Abstract

This invention discloses a high-temperature resistant slow-release foaming material, its preparation method, and its application. The high-temperature resistant slow-release foaming material comprises inorganic silica gel and a surfactant. The foaming material of this invention has the advantages of good moldability and excellent temperature resistance, and can achieve stable and long-term release of the foaming agent. After release, the nano-agglomerates disintegrate, and the silicon nanoparticles can be carried out of the wellhead by the gas flow. It can be used in high-temperature oil and gas wells, reducing the need for frequent well opening and chemical injection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid composite materials technology, specifically to a high-temperature resistant slow-release foaming material, its preparation method, and its application. Background Technology

[0002] In natural gas extraction, as extraction time increases, downhole pressure decreases, and groundwater accumulates in the wellbore, reducing or even halting natural gas production. Adding foaming agents can produce low-density foam to remove the base fluid from the wellbore. These wellbore chemical foaming agents are typically in solid or liquid form. Solid foaming rods are usually made into fast-dissolving solid rods and are periodically injected into the wellbore through frequent well openings. However, the large single-use dosage of solid foaming agents results in a short effective duration. Using slow-release technology can reduce the number of operations, and the slow-release system can effectively improve the utilization rate of the active chemical components, reducing losses and volatilization due to environmental factors. Liquid foaming agents, on the other hand, are injected downhole via pumps, requiring investment in injection pipelines and pumps. Therefore, solid slow-release chemicals are an effective method to reduce investment in well opening and liquid injection equipment.

[0003] Slow-release technology has applications in agriculture, pharmaceuticals, and oilfield chemicals. In the pharmaceutical field, encapsulating drugs in slow-release capsules can reduce the frequency of application and extend the effective duration of action several times over. In the field of pesticide slow-release agents, there are many varieties, including microcapsules. The capsule shell can be a natural, semi-synthetic, or fully synthetic polymer compound, including proteins, high-molecular-weight carbohydrates, cellulose, fatty acids and their derivatives, inorganic polymers, vinyl polymers, polyamides, polyurethanes, and polyesters. In the field of slow-release fertilizers, modified polyvinyl alcohol is mixed with inorganic materials such as diatomaceous earth, zeolite powder, biochar, phosphate rock powder, and sulfur as coating materials to control nitrogen loss and improve nitrogen fertilizer utilization.

[0004] Slow-release technology has been widely applied in oilfields. For example, US20160009980A1 discloses a composite material containing a porous metal oxide such as alumina, zirconium oxide, or titanium oxide as a solid carrier and binder. This composite material, consisting of a well-formed compressible particle adsorbed onto calcined porous metal oxides or entering the gaps within the calcined porous metal oxides, can be introduced into oil or gas wells to slowly release the effective components adsorbed within the porous material. US20180134939A1 discloses a method of cross-linking scale inhibitors and slow-release active substances onto a carrier via chemical bonds, utilizing the cross-linking reaction of alcohols, amines, and acids. Downhole, the cross-linking bonds hydrolyze, slowly releasing the active substances. US20170058184A1 discloses a non-water-soluble carrier composed of corn cob sand, which is used in oil and gas field enhancement or production processes to adsorb liquid chemical reagents such as scale inhibitors and surfactants. The pressure resistance and liquid insolubility of the corn cob sand allow the active chemical substances to be slowly released into the oil and gas wells, achieving the purpose of slow release. US20120273197A1 discloses a composite material for well treatment operations such as hydraulic fracturing and sand control. This material allows one or more well treatment agents to be slowly released into the underground formation and / or into the wellbore penetrating the formation. It features a high specific surface area nanoscale calcined porous matrix (adsorbent) onto which the well treatment agent is coated. CN110157401A discloses a method for preparing a controllable long-lasting slow-release scale inhibitor capsule. The scale inhibitor and one of the slow-release components, an inorganic nanocarrier, are assembled into a homogeneous whole in the form of a solid solution. The capsule is then coated with a controllably dissolvable cross-linked polymer composed of carboxymethyl cellulose, polyvinyl alcohol, and porous zeolite. When the polymer dissolves in the environmental medium, the active substances are gradually released. Utilizing a dual controlled-release mechanism of polymer dissolution and desorption of the scale inhibitor from the inorganic nanocarrier, the capsule can be slowly released into the wellbore, thereby prolonging its protective effect. CN107304078A discloses an environmentally friendly slow-release polymer scale inhibitor, which uses a mixture of polyvinyl alcohol, sodium alginate and gelatin solution as a carrier material and boric acid as an additive to construct a slow-release wall material system to load the scale inhibitor, and performs slow release in a simulated oilfield water medium at 50°C.

[0005] Although sustained-release technology is increasingly used in oil and gas field development, the complex environmental characteristics of high-temperature wells lead to exceptionally stringent requirements for sustained-release materials. CN110564388A discloses a method for preparing a temperature-sensitive plugging colloid for oil and gas fields. This method involves multiphase physical adsorption and chemical pre-crosslinking of modified polyacrylamide, a trivalent crosslinking agent, a water-soluble sustained-release agent, and an aqueous phase, resulting in a temperature-sensitive, swollen, delayed-release colloid with sustained-release properties. However, its applicable temperature range is only 60-90℃. CN110003875A presents research on slow-release foaming agents, mixing surfactants and foaming agents with 5-20% casings to achieve an action time of 120 hours (5 days). However, this technology has drawbacks, including an operating temperature below 90℃ and a shelf life of less than 3 months for animal materials and inconsistent batch quality. In these studies, the selection of sustained-release materials for specific conditions (e.g., acid resistance, temperature resistance) remains a significant challenge.

[0006] In summary, most existing slow-release materials use slowly soluble materials to encapsulate surfactants to achieve a slow-release effect; however, the materials used dissolve and decompose rapidly at high temperatures, causing the surfactants to be released quickly, resulting in a short slow-release time.

[0007] Therefore, a new type of material is needed to solve the problems of short release time and low temperature resistance of existing slow-release materials for oil fields. Summary of the Invention

[0008] To address the problems existing in the prior art, this invention provides a high-temperature resistant slow-release foaming material, its preparation method, and its application. The high-temperature resistant slow-release foaming material of this invention has a mesoporous nanostructure, and its main components include a foaming agent (surfactant) and inorganic silica gel. The foaming material of this invention has the advantages of good moldability and excellent temperature resistance, and can achieve stable and long-term release of the foaming agent. After release, the nano-agglomerates disintegrate, and the silica nanoparticles can be carried out of the wellhead by the gas flow. It can be used in high-temperature oil and gas wells, reducing the need for frequent well opening and chemical injection.

[0009] One of the objectives of this invention is to provide a high-temperature resistant slow-release foaming material comprising inorganic silica gel and surfactant.

[0010] In a preferred embodiment of the present invention,

[0011] The high-temperature resistant slow-release foaming material is a porous aggregate of nanoparticles, wherein the particle size of the nanoparticles is preferably 20-100 nm, more preferably 20-50 nm; and / or, the porous aggregate of nanoparticles has a mesoporous structure.

[0012] In a preferred embodiment of the present invention,

[0013] The mass ratio of the inorganic silica gel to the surfactant is 1:(0.8-18), preferably 1:(2.7-14), and more preferably 1:(2.7-12.8).

[0014] In a preferred embodiment of the present invention,

[0015] The high-temperature resistant slow-release foam material also contains water, and the water content is 0.1 to 15 wt%, preferably 2 to 10 wt%, based on the total weight of the high-temperature resistant slow-release foam material.

[0016] In a preferred embodiment of the present invention,

[0017] The inorganic silica gel is obtained by hydrolysis and condensation of a silicon precursor. Preferably, the silicon precursor is at least one of silicate esters and silica sol, more preferably at least one of silicate esters, more preferably at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, and tetrabutyl silicate, and even more preferably tetraethyl silicate. The inorganic silica gel in this invention is a thermally stable inorganic silicon-containing polymer; and / or...

[0018] The surfactant is at least one of cationic surfactants, amphoteric surfactants, and anionic surfactants; preferably, the cationic surfactant is at least one of alkyl trimethylammonium salts; and / or, the amphoteric surfactant is at least one of alkyl betaines, preferably at least one of alkylamidopropyl betaines; and / or, the anionic surfactant is at least one of alkylbenzene sulfonates and alkyl sulfonates.

[0019] In a preferred embodiment of the present invention,

[0020] The alkyl chain lengths of the alkyltrimethylammonium salt, alkyl betaine, alkylbenzene sulfonate, and alkyl sulfonate are each independently 8 to 16; preferably,

[0021] The surfactant is at least one of dodecylamidopropyl betaine, cocamidopropyl betaine, and hexadecyltrimethylammonium salt.

[0022] In this invention, the alkyl chain length refers to the length of the alkyl backbone. It is understood that side chains may or may not be connected to the alkyl backbone. This invention does not limit the type of side chains; for example, they can be alkyl side chains. Those skilled in the art can freely choose, as long as it improves the temperature-resistant slow-release properties of the composite material.

[0023] Other commonly used additives in the art, such as inert inorganic salts, can also be added to the high-temperature resistant slow-release foaming material of the present invention. The inert inorganic salts are preferably Na2SO4 or NaCl, and their dosage is also conventional. Those skilled in the art can add them according to the actual situation.

[0024] In a preferred embodiment of the present invention,

[0025] The high-temperature resistant slow-release foaming material is prepared by a process including hydrolysis and polycondensation of components containing a silicon precursor and the surfactant; preferably, the mass ratio of the surfactant to the silicon precursor is (0.25-5):1, more preferably (0.8-4):1, and more preferably (0.8-3.7):1.

[0026] A second objective of this invention is to provide a method for preparing a high-temperature resistant slow-release foaming material, which is one of the objectives of this invention. The method includes mixing components, including a silicon precursor and the surfactant, and then hydrolyzing and polycondensing them. Preferably, the mass ratio of the surfactant to the silicon precursor is (0.25-5):1, more preferably (0.8-4):1, and even more preferably (0.8-3.7):1.

[0027] In a preferred embodiment of the present invention,

[0028] The method includes:

[0029] The surfactant is dissolved in water and the pH is adjusted to alkaline. Then, a silicon precursor is added and the pH is adjusted to acidic. After aging, the high-temperature resistant slow-release foaming material is obtained.

[0030] In a preferred embodiment of the present invention,

[0031] The mass ratio of the surfactant to water is 1:(1-10), preferably 1:(2-3); and / or,

[0032] After dissolving the surfactant in water, the pH is adjusted to 9-10, preferably using at least one of ammonia, sodium hydroxide, potassium hydroxide, sodium carbonate, and solutions thereof; and / or,

[0033] After adding the silicon precursor, adjust the pH to 2-3, preferably using at least one of hydrochloric acid, sulfuric acid, acetic acid, oxalic acid, and solutions thereof; and / or,

[0034] The aging conditions include: aging at 40–80°C for 48–96 hours, preferably aging in stages with increasing temperature, more preferably aging at 40–55°C for 1–12 hours, aging at 55–65°C for 1–3 days, and aging at 65–80°C for 0.5–1.5 days.

[0035] A third objective of this invention is to provide a high-temperature resistant slow-release foaming material obtained by one objective of this invention or by the preparation method of another objective of this invention as a foaming agent.

[0036] In a preferred embodiment of the present invention,

[0037] When the high-temperature resistant slow-release foaming material is used as a foaming agent, the application conditions include: wellbore temperature of 80-150℃; and / or pH of 4-5.

[0038] The temperature-resistant slow-release foaming material provided by this invention can slowly release active ingredients—surfactants—under high-temperature (e.g., 80-150℃) and acidic (e.g., pH 4-5) conditions in wellbore, and can be used as a foaming agent.

[0039] The foaming agent carried in the temperature-resistant slow-release foaming material of the present invention can solve the problem of frequent well opening and injection of foaming agent for high-temperature gas well drainage and gas production. Attached Figure Description

[0040] Figure 1 This is an appearance diagram of the high-temperature resistant slow-release foaming material of Example 1;

[0041] Figure 2 This is an appearance diagram of the high-temperature resistant slow-release foaming material of Example 2;

[0042] Figure 3 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 1 after one day of slow-release evaluation;

[0043] Figure 4 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 1 after 3 days of slow-release evaluation;

[0044] Figure 5 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 1 after 5 days of slow-release evaluation;

[0045] Figure 6 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 1 after 7 days of slow-release evaluation;

[0046] Figure 7 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 2 after 1 day of slow-release evaluation;

[0047] Figure 8 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 2 after 3 days of slow-release evaluation;

[0048] Figure 9 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 2 after 5 days of slow-release evaluation;

[0049] Figure 10 This is an image showing the appearance of the high-temperature resistant slow-release foam material of Example 2 after 7 days of slow-release evaluation;

[0050] Figure 11The image shows a microscopic SEM image of the high-temperature resistant slow-release foam material of Example 1 before it contains CTAB.

[0051] Figure 12 The image shows the CTAB-containing microstructure of the high-temperature resistant slow-release foam material from Example 1 after 3 days of slow-release evaluation.

[0052] Figure 13 The image shows a microscopic SEM image of the high-temperature resistant slow-release foam material containing CAB before slow release, as described in Example 2.

[0053] Figure 14 The image shows a microscopic SEM image of the high-temperature resistant slow-release foam material of Example 2 after 3 days of slow-release evaluation containing CAB.

[0054] Figure 15 This is a scanning electron microscope (SEM) image of the surface elemental analysis of the high-temperature resistant slow-release foam material in Example 1 before slow release.

[0055] Figure 16 This is a scanning electron microscope (SEM) image of the surface elemental analysis of the high-temperature resistant slow-release foam material in Example 2 before slow release.

[0056] Figure 17 This is a scanning electron microscope (SEM) image of the surface elemental analysis of the high-temperature resistant slow-release foaming material of Example 1 after 3 days of release.

[0057] Figure 18 The image shows the surface elemental analysis of the high-temperature resistant slow-release foam material of Example 2 after 3 days of release using a scanning electron microscope. Detailed Implementation

[0058] The present invention will now be described in detail with reference to specific embodiments and accompanying drawings. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.

[0059] Unless otherwise specified, the raw materials used in the examples are all publicly available in the prior art, such as those that can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0060] In this embodiment, the instrument used for thermogravimetric analysis was a Hitachi TG / DTA7200 thermogravimetric calorie analyzer.

[0061] Example 1

[0062] Mix 10g water and 4.0g hexadecyltrimethylammonium bromide (CTAB) at 25℃ and stir for 15min. Add NH4OH to adjust the pH to 9.5 and stir for 5min. Add 4.0g tetraethyl silicate (TEOS) and stir at 25℃ for 15min. Add 1mol / L HCl to adjust the pH to 2.5. Age at 50℃ for 4h, 60℃ for 2 days, and 75℃ for 1 day to form a gel solid block, which is the high-temperature resistant slow-release foaming material (e.g., Figure 1 As shown in the figure, the water content in the high-temperature resistant slow-release foam material was found to be 4.2 wt% by thermogravimetric analysis.

[0063] Example 2

[0064] 10g of water and 4.0g of dodecylamidopropyl betaine (CAB) were mixed and stirred at 25℃ for 15 minutes. NH4OH was added to adjust the pH to 9.5, and the mixture was stirred for 5 minutes. Then, 4.0g of tetraethyl orthosilicate (TEOS) was added and stirred at 25℃ for 15 minutes. The pH was adjusted to 2.5 with 1mol / L HCl. The mixture was aged at 50℃ for 4 hours, at 60℃ for 2 days, and at 75℃ for 1 day, forming a gel solid block, which is the high-temperature resistant slow-release foaming material (e.g., Figure 2 As shown in the figure, the water content in the high-temperature resistant slow-release foam material was found to be 8.5 wt% by thermogravimetric analysis.

[0065] Evaluation of surfactant release efficiency after release in Examples 1-2

[0066] The slow-release evaluation experiment was conducted as follows: 4.5g of the high-temperature resistant slow-release foaming material from Examples 1-2 was placed in a pressure-resistant bottle containing 60mL of simulated underground brine and sealed. The simulated underground brine contained the following components: calcium chloride 8.37g / L, magnesium chloride 0.42g / L, sodium sulfate 1.21g / L, and sodium chloride 60.74g / L. Carbon dioxide was bubbled into the simulated underground brine until saturation, simulating an acidic underground environment with a pH of 4. The experiment was conducted at a constant temperature of 130℃, with the carbon dioxide-saturated simulated underground brine replaced every 24 hours. The appearance of the sample after 1, 3, 5, and 7 days was observed. Figure 3-6 As shown, the appearance of the high-temperature resistant slow-release foam material of Example 2 after 1, 3, 5, and 7 days of slow-release evaluation is as follows. Figure 7-10 As shown, the high-temperature resistant slow-release foam material decomposes and gradually shrinks after 7 days in high-temperature salt water.

[0067] For the surfactants released in Examples 1-2, their release efficiency was evaluated by testing their foam volume and half-life performance: 40 mL of the solution released in 1-7 days was diluted with water to prepare 200 mL of standard solution and foamed by stirring. The foaming was carried out using a stirrer with a speed of 16000 rpm and a stirring time of 30 seconds. The foam volume was measured and the results are shown in Table 1.

[0068] Table 1

[0069] time Example 1 (ml) Example 2 (ml) Day 1 400 410 Day 2 345 310 Day 3 310 290 Day 4 285 260 Day 5 260 225 Day 6 255 218 Day 7 235 205

[0070] As can be seen from Table 1, the high-temperature resistant slow-release foaming materials of Examples 1-2 can maintain surfactant release for more than 72 hours, indicating that they have good slow-release performance.

[0071] Implement column 3

[0072] The series of high-temperature resistant slow-release foaming materials (including the high-temperature resistant slow-release foaming materials of Examples 1 and 2) were prepared by mixing surfactants and silicon precursors in different mass ratios, with the same preparation conditions as in Example 1.

[0073] Table 2

[0074]

[0075] As can be seen from Table 2, only when the mass ratio of surfactant to silicone precursor is preferably (0.8-4):1, more preferably (0.8-3.7):1, and even more preferably (1-3.7):1, can the high-temperature resistant slow-release foam material be formed into a relatively hard and complete solid. Outside this range, only soft wet gel or unformed fragments can be obtained. Wet gel is easy to stick to the well wall, and unformed fragments are not easy to inject into the well and are easily carried out of the well by the airflow, thus failing to achieve the slow-release effect.

[0076] Implement column 4

[0077] The microstructure of the high-temperature resistant slow-release foamed materials of Examples 1 and 2 was characterized after 3 days of initial and slow-release evaluation, such as... Figure 11-14 As shown: SEM microstructure reveals that the high-temperature resistant slow-release foam material contains porous aggregates of nanoparticles with a particle size of 20–100 nm, preferably 20–50 nm. These aggregates contain mesoporous structures, forming channels for the controlled release of surfactants. Surface elemental analysis (EDS) was performed on the high-temperature resistant slow-release foam materials of Examples 1 and 2 initially and after 3 days of release. Figure 15-18 As shown: Surface elemental analysis (EDS) reveals that the initial high-temperature resistant slow-release foam material contains the characteristic elements C, N, and Br of the corresponding surfactant, such as... Figure 15 and 16After 3 days of release, the porosity increases and the structure becomes looser, the content of surfactant characteristic elements decreases, and the silicon content increases, such as... Figure 17 and 18 .

[0078] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0079] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A high-temperature resistant slow-release foaming material, wherein the high-temperature resistant slow-release foaming material is a porous aggregate of nanoparticles, the porous aggregate of nanoparticles having a mesoporous structure, and the particle size of the nanoparticles being 20~100nm; the high-temperature resistant slow-release foaming material is prepared by mixing components including a silicon precursor and a surfactant through hydrolysis and condensation steps; the surfactant is at least one of cationic surfactant, amphoteric surfactant, and anionic surfactant; the cationic surfactant is at least one of alkyl trimethylammonium salt; the amphoteric surfactant is at least one of alkyl betaine; the anionic surfactant is at least one of alkylbenzene sulfonate and alkyl sulfonate; the mass ratio of the surfactant to the silicon precursor is (0.8~4):1; the silicon precursor is at least one of silicate ester and silica sol.

2. The high-temperature resistant slow-release foaming material as described in claim 1, characterized in that: The nanoparticles have a particle size of 20~50nm.

3. The high-temperature resistant slow-release foaming material as described in claim 1, characterized in that: The silicon precursor is at least one of silicate esters.

4. The high-temperature resistant slow-release foaming material as described in claim 1, characterized in that: The amphoteric surfactant is at least one of alkylamidopropyl betaine.

5. The high-temperature resistant slow-release foaming material as described in claim 3, characterized in that: The silicon precursor is at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, and tetrabutyl silicate.

6. The high-temperature resistant slow-release foaming material as described in claim 1, characterized in that: The alkyl chain lengths of the alkyltrimethylammonium salt, alkyl betaine, alkylbenzene sulfonate, and alkyl sulfonate are each independently 8 to 16.

7. The high-temperature resistant slow-release foaming material as described in claim 6, characterized in that: The surfactant is at least one of dodecylamidopropyl betaine, cocamidopropyl betaine, and hexadecyltrimethylammonium salt.

8. The high-temperature resistant slow-release foaming material according to any one of claims 1-7, characterized in that: The mass ratio of the surfactant to the silicon precursor is (0.8~3.7):

1.

9. A method for preparing a high-temperature resistant slow-release foaming material as described in any one of claims 1-7, comprising the steps of mixing components including a silicon precursor and the surfactant, followed by hydrolysis and polycondensation.

10. The preparation method according to claim 9, characterized in that: The mass ratio of the surfactant to the silicon precursor is (0.8~4):

1.

11. The preparation method according to claim 10, characterized in that: The mass ratio of the surfactant to the silicon precursor is (0.8~3.7):

1.

12. The preparation method according to claim 9, characterized in that... The method includes: The surfactant is dissolved in water and the pH is adjusted to alkaline. Then, a silicon precursor is added and the pH is adjusted to acidic. After aging, the high-temperature resistant slow-release foaming material is obtained.

13. The preparation method according to claim 12, characterized in that: The mass ratio of the surfactant to water is 1:(1~10); and / or, After dissolving the surfactant in water, adjust the pH to 9-10; and / or, After adding the silicon precursor, adjust the pH to 2-3; And / or, The aging conditions include aging at a temperature of 40~80℃ for 48~96 hours.

14. The preparation method according to claim 13, characterized in that: The mass ratio of the surfactant to water is 1:(2~3); and / or, After dissolving the surfactant in water, the pH is adjusted to 9-10 using at least one of ammonia, sodium hydroxide, potassium hydroxide, sodium carbonate, and their solutions; and / or, After adding the silicon precursor, the pH is adjusted to 2-3 using at least one of hydrochloric acid, sulfuric acid, acetic acid, oxalic acid, and their solutions; and / or, The aging conditions include: aging through staged temperature increases.

15. The preparation method according to claim 14, characterized in that: The aging conditions include: aging at 40~55℃ for 1~12 hours, aging at 55~65℃ for 1~3 days, and aging at 65~80℃ for 0.5~1.5 days.

16. The application of a high-temperature resistant slow-release foaming material as described in any one of claims 1-8 or a high-temperature resistant slow-release foaming material obtained by the preparation method described in any one of claims 9-15 as a foaming agent.

17. The application as described in claim 16, characterized in that: When the high-temperature resistant slow-release foaming material is used as a foaming agent, the application conditions include: wellbore temperature of 80~150℃; and / or pH of 4~5.

Citation Information

Patent Citations

  • Environment-friendly slow-release polymer scale inhibitor and preparation method thereof

    CN107304078A

  • Slow release type liquid-carrying and sand-carrying foam drainage agent and preparation method thereof

    CN110003875A

  • Preparation method of controllable long-acting slow-release scale inhibitor capsule

    CN110157401A

  • Temperature-sensitive plugging colloid for oil and gas fields, preparation method and use method thereof

    CN110564388A

  • Composites for controlled release of well treatment agents

    US20120273197A1