A production process for increasing the length dispersion of wool tops
By dividing the wool strip into three equal parts and performing specific stretching and breaking processes, the problems of fiber damage and low efficiency in existing technologies are solved, thereby improving the dispersion of wool strip length and increasing production efficiency.
Patent Information
- Application Number
- CN202510468143.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-15
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-04-15
AI Technical Summary
Existing technologies can easily lead to fiber damage when increasing the dispersion of wool strip length, affecting quality and performance, and resulting in low production efficiency.
The wool tops are divided into three equal parts and subjected to different stretching and breaking processes. By modifying the stretching device of the carding machine, intermittent punching is achieved to form wool tops of irregular lengths, which are then mixed with the finished wool tops in the carding machine.
It effectively improves the dispersion of wool strip length, reduces fiber damage, increases production efficiency, and reduces costs.
Abstract
Description
Technical Field
[0001] This invention relates to the field of wool processing technology, specifically to a production process method for improving the dispersion of wool strip length. Background Technology
[0002] Wool length dispersion refers to the difference or range of variation in fiber length within a wool top. This dispersion can be caused by a variety of factors, including different breeds of wool, feeding conditions, age, shearing season, and subsequent processing operations and parameters.
[0003] In wool textile processing, the length variation of wool tops has a certain impact on the quality and performance of the final product. Appropriate length variation can help enhance the softness, warmth, and breathability of wool fabrics. Wool fiber diameter is a major factor determining its value; it is closely related to its economic traits and has a significant impact on wool production, processing, and trade, determining 75% of the value of the wool top. Furthermore, variations in wool fiber fineness account for 61% of the total profit from wool processing, directly affecting the quality of yarn and fabrics.
[0004] To improve the length variation of wool tops, manufacturers can take a series of measures. First, in selecting wool raw materials, they can prioritize wool from the same breed, feeding conditions, and shearing season to reduce length differences caused by the raw materials themselves. Second, during wool processing, they can optimize process parameters such as combing and spinning to make the wool fiber length distribution more uniform. Furthermore, they can employ advanced spinning technologies and equipment, such as using ring spinning machines for precision spinning, to improve the fineness and uniformity of the wool tops.
[0005] While existing methods for increasing the dispersion of wool top length can achieve differentiation in wool length to some extent, they still have some drawbacks, such as the risk of wool damage: excessive stretching or breaking operations may damage wool fibers, affecting their quality and performance. This damage may manifest as fiber breakage, cuticle loss, or fiber twisting, thereby reducing the softness, warmth, and durability of the wool top; and low production efficiency: existing methods often require multiple operations or complex processes to achieve dispersion of wool length, which may lead to low production efficiency and increased production costs. Summary of the Invention
[0006] (a) Technical problems to be solved
[0007] To address the shortcomings of existing technologies, this invention provides a production process for improving the dispersion of wool sliver length. The process involves dividing the wool sliver into three equal parts. The first part is drafted to obtain a continuously drafted, broken wool sliver. By modifying the drafting device to intermittently interrupt the drafting at set times, the wool fibers in the second part are intermittently broken under external force, forming an irregularly long wool sliver, thus obtaining an intermittently broken wool sliver. The third part of the wool sliver is then fed into a carding machine along with the continuously drafted and intermittently broken wool sliver for mixing, resulting in the finished wool sliver. This method solves the problem that excessive drafting or breaking operations may damage the wool fibers, affecting their quality and performance.
[0008] (II) Technical Solution
[0009] To achieve the above objectives, the present invention provides the following technical solution: a production process method for improving the dispersion of wool strip length, comprising the following steps:
[0010] Step S001. Process the raw wool by washing, combing, pin combing and fine combing to produce wool strips of a certain weight and length;
[0011] Step S002. Divide the produced wool strips into three equal parts according to weight, and denoted as the first wool strip, the second wool strip and the third wool strip respectively. Feed the first wool strip into the modified carding machine, perform a 12-fold large drafting of the leather roller, and perform continuous tearing to form wool strips with large differences in length, thus obtaining a continuously drafted tearing wool strip.
[0012] Step S003. Feed the second wool strip into the modified carding machine. Modify the drafting device to achieve intermittent pauses at a set time. The set time range is 10 to 40 seconds. The carding machine feeds the roller, stops, and the drafting roller is synchronized to achieve over-pauses. The roller speed is increased to perform variable speed movement, which causes the wool strip to suddenly accelerate forward. Under the action of external force, some wool fibers are intermittently broken to form wool strips of irregular length, thus obtaining intermittently broken wool strips.
[0013] Step S004. The third wool top is fed into the carding machine and mixed with the continuous stretching and intermittent stretching wool tops to obtain the finished wool top.
[0014] Preferably, the raw wool is processed through washing, combing, pin combing, and fine combing to produce wool tops of a certain weight and length. The washing process removes dust, impurities, grass clippings, and grease contaminants from the wool, restoring its cleanliness and preparing it for subsequent combing. The raw wool is placed in a washing machine with an appropriate amount of detergent and water. Through mechanical stirring and rinsing, the wool is fully exposed to water and stains are removed. Excess water is then removed by centrifugation or pressing to obtain clean wool, completing the washing process. The combing process further loosens the cleaned wool, removing grass clippings and residual impurities, and straightens and parallels the wool fibers, arranging them into a web. The cleaned wool is then combed using a combing machine. The carding process involves the carding machine's needles combing the wool fibers, removing impurities, and creating a mesh-like structure to prepare for subsequent processes. This carding process straightens and parallels the wool fibers, further improving their orientation and uniformity. The carded wool is then fed into the carding machine for further combing, making the fibers even more uniform. The combing process further removes short fibers and impurities, increasing the length and uniformity of the wool fibers, preparing them for wool top production. Finally, the carded wool is fed into the combing machine, where a denser set of needles finely combs the wool, removing short fibers and residual impurities. After combing, the length and uniformity of the wool fibers are significantly improved.
[0015] Preferably, the carding machine includes a drafting unit and a feeding unit. The main function of the feeding unit is to feed the first wool sliver into the carding machine. The drafting unit drafts and combs the wool sliver to achieve the desired fineness and length. The drafting unit includes a front jaw gripping point and a rear jaw gripping point. There is relative movement between the two gripping points. The linear velocity at the output end is greater than the linear velocity at the feeding end. The gripping points have a certain gripping force. The wool fibers held by the jaws are straightened at the tail due to the resistance of the steel needles on the needle plate, and the wool sliver is also lengthened and thinned. Both the drafting unit and the feeding unit are equipped with a wool wrapping detection device. The wool wrapping detection device monitors the amount of wool wrapping. When the amount of wool wrapping exceeds the threshold, a carding machine stop command is issued.
[0016] Preferably, in step S002, the roller is an antistatic rubber pressure roller, the pressure range of the drafting roller is 150-300 kg, and the pressure of the feed roller is 3 / 4 of the pressure of the drafting roller.
[0017] Preferably, in step S002, the modification of the carding machine is as follows: adjust the feeding speed and angle to reduce clogging and breakage; adjust the carding components, such as the density and shape of the carding pins, to better meet the needs of the wool tops; select a leather roller with a high coefficient of friction and elasticity, such as an antistatic rubber pressure roller; precisely control the speed and tension relationship between the leather roller and the feeding system; and set the draft ratio to 12 times; design or modify the breaking mechanism to control the length of the wool top after breaking by adjusting the rotation speed and cutting force.
[0018] Preferably, the coefficient of variation (CV) is used to evaluate the dispersion of the wool sliver length, and to obtain the average length of the wool fibers in the continuously drawn wool sliver. And standard deviation σ, through the formula The coefficient of variation (CV) for continuous-stretch breakage of wool sliver was calculated, where the average length... This refers to the sum of the detected wool fiber lengths divided by the number of wool fibers detected. Let there be n wool fibers, i representing the fiber number, and the length of the i-th wool fiber be di. The formula is used to calculate... The average length was calculated. ; through formula The standard deviation σ of the wool strips was calculated.
[0019] Preferably, in step S003, a programmable logic controller (PLC) is used. By writing a program, it can control the pausing operation of the drafting device according to a set time interval, such as 10 seconds to 40 seconds. Sensors are installed at key parts of the drafting device to monitor the position, speed, or pressure status of the rollers and skin rollers. An actuator is installed so that it can accurately execute the pausing operation when it receives instructions from the PLC.
[0020] Preferably, step S003 includes feeding the wool strip, stopping the feeding roller, synchronizing the drafting roller, variable speed movement, and intermittent pausing operation, comprising the following steps:
[0021] Wool strip feeding: Feed the wool strips evenly into the modified carding machine;
[0022] Feed roller stop: When the wool strip enters the carding machine, the feed roller stops rotating at a set time point via the programmable controller;
[0023] Synchronization of the drafting rollers: The drafting rollers must also stop synchronously when the feeding rollers stop to ensure that the tension of the wool strip is consistent between the rollers;
[0024] Variable speed motion: Within a set time range (10 seconds to 40 seconds), simulate variable speed motion to rapidly increase the roller speed in a short period of time;
[0025] Intermittent buckling: When the roller speed increases to a certain level, the feed roller is suddenly released, causing it to start rotating again. At the same time, the drafting roller continues to run at a high speed. This sudden action will produce an intermittent buckling effect in the wool sliver. Due to the buckling effect, some wool fibers will be intermittently broken under the action of external force. This breaking process is irregular, so the final wool sliver length will also be irregular.
[0026] Preferably, the "overtaking" refers to: first, stopping the feeding roller, at which point the wool fibers at the feeding end stop advancing; subsequently, the drafting roller also stops, but due to the delay, the fibers in the drafting zone will still be subjected to a certain drafting force; when restarted, the drafting roller starts rotating first, "overtaking" the position of the feeding roller, thus distributing the fibers more evenly in the drafting zone; the feeding roller then starts and continues to feed new fibers; in this way, the fiber drafting process can be controlled more effectively, improving the uniformity and quality of the fibers.
[0027] Preferably, the coefficient of variation (CV) of the continuous-stretching wool strip is 36%-45%; the coefficient of variation (CV) of the intermittent-stretching wool strip is 32%-48%; and the coefficient of variation (CV) of the finished wool strip is 32%-41%.
[0028] Preferably, the following methods can be considered for real-time monitoring and control of wool strip length during the production process:
[0029] Laser scanning measurement: The wool tops are measured in real time using a laser scanning instrument. The scanning instrument can quickly and accurately obtain the length data of the wool tops and transmit the data to the quality control center for analysis and processing.
[0030] Visual imaging technology: This method uses a high-resolution camera or imaging system to image wool strips in real time and combines image processing algorithms to measure the length of the wool strips. This method can achieve non-contact measurement and has high accuracy and real-time performance.
[0031] Sensor monitoring: Length sensors are installed on the production line to monitor the length of wool strips in real time. The monitoring data is transmitted to the monitoring system for real-time feedback and control.
[0032] Data analysis and feedback control: The real-time collected wool top length data is input into the data analysis system of the quality control center. Through data analysis, the length during the production process is monitored and analyzed, and abnormalities are detected and feedback control is implemented in a timely manner.
[0033] Automated control system: Combining modern automated control systems with length monitoring and production equipment control, it enables automated monitoring and adjustment of the production process, timely detection and elimination of defective products, and ensures the stability and consistency of product quality.
[0034] (III) Beneficial Effects
[0035] This invention provides a production process for improving the dispersion of wool strip length, which has the following beneficial effects:
[0036] (1) The production process method for improving the dispersion of wool sliver length involves dividing the wool sliver into three equal parts, then drawing the first part of the wool sliver to obtain a continuously drawn and broken wool sliver; by modifying the drawing device to achieve intermittent interruption at a set time, the wool fibers of the second part of the wool sliver are intermittently broken under the action of external force to form an irregular length wool sliver, thus obtaining an intermittently broken wool sliver; the third part of the wool sliver is fed into a carding machine and mixed with the continuously drawn and broken wool sliver to obtain the finished wool sliver, thereby solving the problem that the drawing or breaking operation may damage the wool fibers and affect their quality and performance.
[0037] (2) The production process method for improving the dispersion of wool strip length can achieve the dispersion of wool length through a simple process flow, which can improve production efficiency and reduce production costs. Detailed Implementation
[0038] Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0039] Example 1
[0040] To achieve the above objectives, embodiments of the present invention provide the following technical solution: a production process method for improving the dispersion of wool strip length, comprising the following steps:
[0041] Step S001. Process the raw wool by washing, combing, pin combing and fine combing to produce wool strips of a certain weight and length;
[0042] Step S002. Divide the produced wool strips into three equal parts according to weight, and denoted as the first wool strip, the second wool strip and the third wool strip respectively. Feed the first wool strip into the modified carding machine, perform a 12-fold large drafting of the leather roller, and perform continuous tearing to form wool strips with large differences in length, thus obtaining a continuously drafted tearing wool strip.
[0043] Step S003. Feed the second wool strip into the modified carding machine. Modify the drafting device to achieve intermittent pauses at a set time. The set time range is 10 seconds. The carding machine feeds the roller, stops, and the drafting roller is synchronized to achieve over-pauses. Increase the roller speed and perform variable speed movement, so that the wool strip suddenly accelerates forward. Under the action of external force, some wool fibers are intermittently broken to form wool strips of irregular length, thus obtaining intermittently broken wool strips.
[0044] Step S004. The third wool top is fed into the carding machine and mixed with the continuous stretching and intermittent stretching wool tops to obtain the finished wool top.
[0045] Further processing involves washing, combing, pin combing, and fine combing to produce wool tops of a certain weight and length. The washing process removes dust, impurities, grass clippings, and grease contaminants from the wool, restoring its cleanliness and preparing it for subsequent combing. The raw wool is placed in a washing machine with appropriate amounts of detergent and water. Mechanical agitation and rinsing ensure the wool is fully in contact with water and removes stains. Excess water is then removed by centrifugation or pressing, resulting in clean wool, completing the washing process. The combing process further loosens the cleaned wool, removing grass clippings and residual impurities, and straightens and parallels the wool fibers, arranging them into a web-like structure. The cleaned wool is then combed using a combing machine. The wool is combed, where the pins of the combing machine open up the wool fibers and remove impurities. The combed wool forms a web-like structure, preparing it for subsequent processes. The pin combing process makes the wool fibers straighter and more parallel, further improving their orientation and uniformity. The combed wool is then fed into the pin combing machine for further combing, making the fibers even more uniform. The fine combing process is used to further remove short fibers and impurities, improving the length and uniformity of the wool fibers, preparing them for making wool tops. The combed wool is then fed into the fine combing machine, where a denser pin line is used to finely comb the wool, removing short fibers and residual impurities. After fine combing, the length and uniformity of the wool fibers are significantly improved.
[0046] Furthermore, the carding machine includes a drafting unit and a feeding unit. The main function of the feeding unit is to feed the first wool sliver into the carding machine. The drafting unit drafts and combs the wool sliver to achieve the desired fineness and length. The drafting unit includes a front jaw gripping point and a rear jaw gripping point. There is relative movement between the two gripping points. The linear velocity at the output end is greater than the linear velocity at the feeding end. The gripping points have a certain gripping force. The wool fibers held by the jaws are straightened at the tail due to the resistance of the steel needles on the needle plate, and the wool sliver is also lengthened and thinned. Both the drafting unit and the feeding unit are equipped with a wool wrapping detection device. The wool wrapping detection device monitors the amount of wool wrapping. When the amount of wool wrapping exceeds the threshold, a carding machine stop command is issued.
[0047] Furthermore, in step S002, the modification of the carding machine is as follows: adjust the feeding speed and angle to reduce clogging and breakage; adjust the carding components, such as the density and shape of the carding pins, to better meet the needs of the wool tops; select a leather roller with a high coefficient of friction and elasticity, such as an antistatic rubber pressure roller; precisely control the speed and tension relationship between the leather roller and the feeding system; and set the draft ratio to 12 times; design or modify the breaking mechanism to control the length of the wool top after breaking by adjusting the rotation speed and cutting force.
[0048] Furthermore, the coefficient of variation (CV) is used to evaluate the dispersion of wool sliver length, and the average length of wool fibers in the continuously drawn wool sliver is obtained. And standard deviation σ, through the formula The coefficient of variation (CV) for continuous-stretch breakage of wool sliver was calculated, where the average length... This refers to the sum of the detected wool fiber lengths divided by the number of wool fibers detected. Let there be n wool fibers, i representing the fiber number, and the length of the i-th wool fiber be di. The formula is used to calculate... The average length was calculated. ; through formula The standard deviation σ of the wool strips was calculated.
[0049] Example 2
[0050] To achieve the above objectives, embodiments of the present invention provide the following technical solution: a production process method for improving the dispersion of wool strip length, comprising the following steps:
[0051] Step S001. Process the raw wool by washing, combing, pin combing and fine combing to produce wool strips of a certain weight and length;
[0052] Step S002. Divide the produced wool strips into three equal parts according to weight, and denoted as the first wool strip, the second wool strip and the third wool strip respectively. Feed the first wool strip into the modified carding machine, perform a 12-fold large drafting of the leather roller, and perform continuous tearing to form wool strips with large differences in length, thus obtaining a continuously drafted tearing wool strip.
[0053] Step S003. Feed the second wool strip into the modified carding machine. Modify the drafting device to achieve intermittent pauses at a set time. The set time range is 40 seconds. The carding machine feeds the roller, stops, and the drafting roller is synchronized to achieve over-pauses. Increase the roller speed and perform variable speed movement, so that the wool strip suddenly accelerates forward. Under the action of external force, some wool fibers are intermittently broken to form wool strips of irregular length, thus obtaining intermittently broken wool strips.
[0054] Step S004. The third wool top is fed into the carding machine and mixed with the continuous stretching and intermittent stretching wool tops to obtain the finished wool top.
[0055] Furthermore, in step S002, the roller is an antistatic rubber pressure roller, the pressure range of the drafting roller is 150-300 kg, and the pressure of the feed roller is 3 / 4 of the ratio of the feed roller to the drafting roller.
[0056] Furthermore, in step S003, a programmable logic controller (PLC) is used to control the pausing operation of the drafting device according to a set time interval, such as 10 to 40 seconds. Sensors are installed at key parts of the drafting device to monitor the position, speed, or pressure status of the rollers and skin rollers. Actuators are installed so that the pausing operation can be accurately executed when the PLC is received.
[0057] Furthermore, step S003 includes feeding the wool strip, stopping the feeding roller, synchronizing the drafting roller, variable speed motion, and intermittent pausing operation, comprising the following steps:
[0058] Wool strip feeding: Feed the wool strips evenly into the modified carding machine;
[0059] Feed roller stop: When the wool strip enters the carding machine, the feed roller stops rotating at a set time point via the programmable controller;
[0060] Synchronization of the drafting rollers: The drafting rollers must also stop synchronously when the feeding rollers stop to ensure that the tension of the wool strip is consistent between the rollers;
[0061] Variable speed motion: Within a set time range (10 seconds to 40 seconds), simulate variable speed motion to rapidly increase the roller speed in a short period of time;
[0062] Intermittent buckling: When the roller speed increases to a certain level, the feed roller is suddenly released, causing it to start rotating again. At the same time, the drafting roller continues to run at a high speed. This sudden action will produce an intermittent buckling effect in the wool sliver. Due to the buckling effect, some wool fibers will be intermittently broken under the action of external force. This breaking process is irregular, so the final wool sliver length will also be irregular.
[0063] Furthermore, the "overtaking" refers to the following: First, the feeding roller stops, at which point the wool fibers at the feeding end cease to advance; subsequently, the drafting roller also stops, but due to the delay, the fibers in the drafting zone will still be subjected to a certain drafting force; when restarted, the drafting roller begins to rotate first, "overtaking" the position of the feeding roller, thus distributing the fibers more evenly in the drafting zone; the feeding roller then restarts, continuing to feed in new fibers; in this way, the fiber drafting process can be controlled more effectively, improving fiber uniformity and quality.
[0064] Furthermore, the coefficient of variation (CV) of the continuous stretching and breaking wool strip is 36%-45%; the coefficient of variation (CV) of the intermittent stretching and breaking wool strip is 32%-48%; and the coefficient of variation (CV) of the finished wool strip is 32%-41%.
[0065] Furthermore, preferably, the following methods can be considered for real-time monitoring and control of wool strip length during the production process:
[0066] Laser scanning measurement: The wool tops are measured in real time using a laser scanning instrument. The scanning instrument can quickly and accurately obtain the length data of the wool tops and transmit the data to the quality control center for analysis and processing.
[0067] Visual imaging technology: This method uses a high-resolution camera or imaging system to image wool strips in real time and combines image processing algorithms to measure the length of the wool strips. This method can achieve non-contact measurement and has high accuracy and real-time performance.
[0068] Sensor monitoring: Length sensors are installed on the production line to monitor the length of wool strips in real time. The monitoring data is transmitted to the monitoring system for real-time feedback and control.
[0069] Data analysis and feedback control: The real-time collected wool top length data is input into the data analysis system of the quality control center. Through data analysis, the length during the production process is monitored and analyzed, and abnormalities are detected and feedback control is implemented in a timely manner.
[0070] Automated control system: Combining modern automated control systems with length monitoring and production equipment control, it enables automated monitoring and adjustment of the production process, timely detection and elimination of defective products, and ensures the stability and consistency of product quality.
[0071] In summary, this production process for improving the length dispersion of wool sliver involves dividing the wool sliver into three equal parts. The first part is drafted to obtain a continuously drafted, broken wool sliver. By modifying the drafting device to intermittently pause at set times, the wool fibers in the second part are intermittently broken under external force, forming an irregularly long wool sliver, thus obtaining an intermittently broken wool sliver. The third part of the wool sliver is then fed into a carding machine along with the continuously drafted and intermittently broken wool sliver for mixing, resulting in the finished wool sliver. This process addresses the problem that excessive drafting or breaking operations may damage the wool fibers, affecting their quality and performance.
[0072] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A production process for improving the dispersion of wool strip length, characterized in that, Includes the following steps: Step S001. Process the raw wool by washing, combing, pin combing and fine combing to produce wool strips of a certain weight and length; Step S002. Divide the wool strips made in step S001 into three equal parts according to weight, which are respectively called the first wool strip, the second wool strip and the third wool strip. Feed the first wool strip into the modified combing machine, perform a 12-fold large stretch, and perform continuous tearing to obtain a continuously stretched and torn wool strip. The modification of the carding machine is as follows: adjust the feeding speed and angle to reduce clogging and sliver breakage; adjust the needle density and shape of the carding components to better meet the needs of wool slivers; select a leather roller with a high coefficient of friction and elasticity, i.e., an antistatic rubber pressure roller, with the pressure range of the drafting roller being 150-300 kg, and the pressure of the feeding roller being 3 / 4 of the pressure of the drafting roller; set the drafting ratio to 12 times. Step S003. Feed the second wool strip into the modified carding machine. Modify the drafting device to achieve intermittent pausing at a set time to form wool strips of irregular length, resulting in intermittently broken wool strips. Use a programmable logic controller (PLC) to control the pausing operation of the drafting device at set time intervals, with the set time range being 10 to 40 seconds. Install sensors at key parts of the drafting device to monitor the position, speed, or pressure status of the feeding roller, drafting roller, and leather roller components. Install actuators to accurately execute the pausing operation upon receiving instructions from the PLC. Step S003 includes wool strip feeding, feeding roller stopping, drafting roller synchronization, variable speed motion, and intermittent pausing operation, comprising the following steps: Wool sliver feeding: The wool sliver is fed evenly into the modified carding machine; Feed roller stop: After the wool sliver enters the carding machine, the feed roller stops rotating at a set time point via the programmable logic controller (PLC); Drafting roller synchronization: The drafting roller also needs to stop synchronously at the same time as the feed roller stops to ensure that the tension of the wool sliver remains consistent between the feed roller and the drafting roller; Variable speed motion: Within a set time range, variable speed motion is simulated to rapidly increase the speed of the drafting roller in a short period of time; Intermittent pause: When the speed of the drafting roller increases to a certain level, the feed roller is suddenly released to restart its rotation, while the drafting roller continues to run at a higher speed. Step S004. The third wool top is fed into the carding machine and mixed with the continuous stretching and intermittent stretching wool tops to obtain the finished wool tops. The coefficient of variation (CV) of the continuous-stretching type of wool strip is 36%-45%; the coefficient of variation (CV) of the intermittent-stretching type of wool strip is 32%-48%; and the coefficient of variation (CV) of the finished wool strip is 32%-41%.
2. The production process method for improving the dispersion of wool strip length according to claim 1, characterized in that, In step S001: the wool washing process is used to remove dust, grass clippings and oil contaminants from the wool, making the wool clean and laying a good foundation for the subsequent wool combing process; The raw wool is placed in a wool washing machine with an appropriate amount of detergent and water. Through mechanical stirring and rinsing, the wool is fully in contact with water to remove stains. Excess water is then removed by centrifugation or pressing to obtain clean wool, completing the wool washing process. The carding process further loosens the clean wool, removing grass clippings and residual impurities, and straightens the wool fibers to form a relatively straight and parallel web. A carding machine is used to comb the clean wool; the carding machine's pins open the wool fibers and remove impurities. The combed wool forms a web structure, preparing for subsequent processes. The pin combing process makes the wool fibers straighter and parallel, further improving fiber orientation and uniformity. The combed wool is then fed into a pin combing machine for further combing, making the fibers more uniform. The fine combing process further removes short fibers and impurities, increasing the length and uniformity of the wool fibers, preparing for the production of wool tops. The combed wool is then fed into a fine combing machine, where a denser pin line is used to finely comb the wool, removing short fibers and residual impurities.
3. The production process method for improving the dispersion of wool strip length according to claim 1, characterized in that, The combing machine in step S002 includes a drafting unit and a feeding unit. Both the drafting unit and the feeding unit are equipped with a hair wrapping detection device. The hair wrapping amount is monitored by the hair wrapping detection device. When the hair wrapping amount exceeds the threshold, a stop command for the combing machine is issued.
4. The production process method for improving the dispersion of wool strip length according to claim 1, characterized in that, The coefficient of variation (CV) is used to evaluate the dispersion of wool sliver length and to obtain the average length of wool fibers in a continuously drawn, broken wool sliver. And standard deviation σ, through the formula The coefficient of variation (CV) for continuous-stretch breakage of wool sliver was calculated, where the average length... This refers to the sum of the detected wool fiber lengths divided by the number of wool fibers detected. Let there be n wool fibers, i representing the fiber number, and the length of the i-th wool fiber be di. The formula is used to calculate... The average length was calculated. ; through formula The standard deviation σ of the wool strips was calculated.
Citation Information
Patent Citations
Production process of worsted three-component wool fancy yarn
CN113502581A
Stretch break method and product
WO2000077283A2