Solar cell

By using silver electrodes and AgSi regions in crystalline silicon solar cells, combined with appropriate passivation film retention and lead-free glass frit, the problem of electrode-substrate contact damage was solved, resulting in a high-efficiency improvement in cell performance.

CN120092512BActive Publication Date: 2026-11-20NAMICS CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380077093.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-06-13
Filing Date
2023-08-09
Publication Date
2026-11-20
Estimated Expiration
2043-08-09

AI Technical Summary

Technical Problem

In existing crystalline silicon solar cells, it is difficult to simultaneously improve the open-circuit voltage (Voc) and fill factor (FF) during the electrode formation process, and contact damage between the electrode and the substrate leads to performance degradation.

Method used

A silver (Ag) electrode is used, and an AgSi region is formed between the electrode and the substrate. By combining an appropriate passivation film retention rate and glass composition, the passivation film is not completely burned through, and an AgSi region with a depth of more than 100 nm is formed. Lead-free glass is used to reduce contact resistance.

Benefits of technology

High-efficiency crystalline silicon solar cells with high open-circuit voltage (Voc) and high fill factor (FF) have been achieved, reducing carrier recombination and surface defects and improving cell performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120092512B_ABST
    Figure CN120092512B_ABST
Patent Text Reader

Abstract

Provided is a crystalline silicon solar cell having high efficiency with a high open-circuit voltage (Voc) and a fill factor (FF). The solar cell of the present invention includes a crystalline silicon substrate (1) including an impurity diffusion layer; a passivation film (2) disposed on at least a portion of the impurity diffusion layer of the substrate (1); and an electrode (20) including silver (Ag) and disposed on at least a portion of the passivation film (2), the solar cell further including at least one AgSi region (30) disposed between at least a portion of the electrode (20) and the substrate (1), the AgSi region (30) including at least one AgSi region (30) having a depth of 100 nm or more, and in a scanning electron microscope photograph of a 5.7 μm x 3.9 μm cross section of the solar cell including the AgSi region (30), the proportion of the length of the passivation film (2) remaining, i.e., the remaining rate of the passivation film (2), is 10 to 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a crystalline silicon solar cell using a crystalline silicon substrate. Background Technology

[0002] In semiconductor devices such as crystalline silicon solar cells, which use crystalline silicon substrates formed by processing monocrystalline or polycrystalline silicon into a flat plate shape, electrodes are typically formed on the surface of the silicon substrate using a conductive paste for electrode formation to facilitate electrical contact between the device and the outside. In recent years, the production volume of crystalline silicon solar cells has increased significantly in semiconductor devices with electrodes formed in this way. These solar cells have an impurity diffusion layer, an anti-reflection film (passivation film), and a light-incident side surface electrode on one surface of the crystalline silicon substrate, and a back electrode on the other surface. Using the light-incident side surface electrode and the back electrode, the electricity generated by the crystalline silicon solar cell can be extracted to the outside.

[0003] In the electrode formation of conventional crystalline silicon solar cells, a conductive paste containing conductive powder, glass frit, organic binder, solvent, and other additives is used. Silver particles (silver powder) are primarily used as the conductive powder.

[0004] Patent Document 1 describes a method for manufacturing a crystalline silicon solar cell. Patent Document 1 describes the use of a conductive paste for electrode formation comprising inorganic materials to form the electrodes of the crystalline silicon solar cell. Patent Document 1 describes the inorganic materials as including conductive particles and glass frit.

[0005] Patent Document 2 describes a process for improving the ohmic contact behavior between the contact grid and the emitter layer in a silicon solar cell. Specifically, the process described in Patent Document 2 involves applying a given voltage in the direction opposite to the positive direction of the silicon solar cell, directing a point light source to the solar side of the silicon solar cell, and thereby irradiating a cross-section of a sub-section on the solar side.

[0006] Patent Document 3 discloses a conductive composition comprising silver powder, PbO-containing glass powder, and an organic carrier for forming electrodes of solar cells. Patent Document 3 also discloses a conductive composition used to form an electrode that penetrates a silicon nitride layer and is conductive to an n-type semiconductor layer formed beneath the silicon nitride layer. Furthermore, Patent Document 3 discloses that the basicity of the glass powder contained in the conductive composition is 0.6 or more and 0.8 or less, and the glass transition temperature is 300°C to 450°C.

[0007] Existing technical documents

[0008] Patent documents

[0009] Patent Document 1: Japanese Patent Application Publication No. 2011-86754

[0010] Patent Document 2: Japanese Patent Publication No. 2021-513218

[0011] Patent Document 3: Japanese Patent Application Publication No. 2009-231826 Summary of the Invention

[0012] Figure 5 The image shows an example of a typical cross-sectional schematic diagram of a crystalline silicon solar cell. For example... Figure 5 As shown, in a typical crystalline silicon solar cell, the electrode pattern of the light-incident side surface electrode 20 (surface electrode) is printed onto the passivation film 2, which functions as a passivation film 2, using a conductive paste or similar method via screen printing. The conductive paste is then dried and fired at a given temperature to form the light-incident side surface electrode 20. In a typical crystalline silicon solar cell, during firing at this given temperature, the conductive paste burns through the passivation film 2. This burn-through allows the light-incident side surface electrode 20 to form in contact with the impurity diffusion layer 4. It should be noted that burn-through refers to the etching of the passivation film 2, which serves as an insulating film, using glass frit or similar materials contained in the conductive paste, thereby making the light-incident side surface electrode 20 conductive with the impurity diffusion layer 4. Figure 5 In the example shown, during the firing of the electrode pattern, the electrode pattern burns through the passivation film 2, causing the passivation film 2 to disappear and the light-incident surface electrode 20 to contact the impurity diffusion layer 4. A pn ​​junction is formed at the interface between the n-type crystalline silicon substrate 1 and the impurity diffusion layer 4. Most of the incident light incident on the crystalline silicon solar cell passes through the passivation film 2 and the impurity diffusion layer 4 before entering the n-type crystalline silicon substrate 1. During this process, the light is absorbed in the n-type crystalline silicon substrate 1, generating electron-hole pairs. Due to the electric field caused by the pn junction, electrons are separated from the n-type crystalline silicon substrate 1 to the back electrode 15, and holes are separated from the p-type impurity diffusion layer 4 to the light-incident surface electrode 20. Electrons and holes (charge carriers) are extracted to the outside in the form of current through these electrodes.

[0013] Figure 2 This is an example of a schematic diagram showing the light-incident side surface of a crystalline silicon solar cell. For example... Figure 2 As shown, on the light-incident side surface of a crystalline silicon solar cell, a main grid electrode (light-incident side main grid electrode 20a) and a light-incident side sub-grid electrode 20b (sometimes simply referred to as "sub-grid electrode 20b") are disposed as the light-incident side surface electrode 20. Figure 5 and Figure 2In the example shown, electrons from the electron-hole pairs generated by incident light on the crystalline silicon solar cell converge at the sub-gate electrode 20b, and then converge at the light-incident main gate electrode 20a. At the light-incident main gate electrode 20a, interconnecting metal solder strips covered with solder are welded to it, and current is extracted to the outside using these metal solder strips.

[0014] The photoelectric conversion efficiency (sometimes simply called "conversion efficiency") of a solar cell is expressed as the product of the fill factor (FF), open circuit voltage (Voc), and short circuit current (Jsc). Essentially, the fill factor (FF) and open circuit voltage (Voc) are inversely related; it is difficult to simultaneously increase both.

[0015] To obtain crystalline silicon solar cells with high conversion efficiency, especially high fill factor (FF), low contact resistance is required between the light incident side surface electrode 20 and the impurity diffusion layer 4.

[0016] Furthermore, in conventional crystalline silicon solar cells, during the formation of the light-incident side surface electrode 20, the conductive paste electrode pattern is burned through, thereby burning through the passivation film 2 and coming into contact with the impurity diffusion layer 4. This burn-through causes damage to the impurity diffusion layer 4, resulting in a decrease in the performance of the crystalline silicon solar cell (especially the open-circuit voltage (Voc)).

[0017] As mentioned above, it is generally difficult to improve both the fill factor and the open-circuit voltage simultaneously. On the other hand, if the structure between the electrode and the substrate necessary to obtain a high-efficiency crystalline silicon solar cell with high open-circuit voltage (Voc) and fill factor (FF) is understood, guidelines for manufacturing high-efficiency crystalline silicon solar cells can be obtained.

[0018] Therefore, the object of the present invention is to provide a high-efficiency crystalline silicon solar cell with high open-circuit voltage (Voc) and fill factor (FF). In particular, in order to obtain a high-efficiency crystalline silicon solar cell with high open-circuit voltage (Voc) and fill factor (FF), the object of the present invention is to provide a crystalline silicon solar cell with a given structure between the electrode and the substrate.

[0019] To address the aforementioned issues, the present invention has the following configuration.

[0020] (Component 1)

[0021] Component 1 is a solar cell that comprises:

[0022] A substrate comprising crystalline silicon and having an impurity diffusion layer on at least one surface;

[0023] A passivation film disposed on at least a portion of the impurity diffusion layer of the substrate; and

[0024] An electrode comprising silver (Ag) is disposed on at least a portion of the passivation film described above.

[0025] The aforementioned solar cell further includes at least one AgSi region disposed at least a portion between the electrode and the substrate.

[0026] The aforementioned AgSi region includes at least one AgSi region with a depth of 100 nm or more.

[0027] In the scanning electron microscope image of the 5.7 μm × 3.9 μm cross section of the solar cell containing the AgSi region, the proportion of the length of the passivation film remaining, i.e. the passivation film retention rate, is 10 to 90%.

[0028] (Component 2)

[0029] Configuration 2 is a solar cell of Configuration 1, wherein the ratio of the thickness Da of the passivation film immediately after its formation to the thickness Db of the passivation film in a scanning electron microscope image of the solar cell containing the AgSi region (5.7 μm × 3.9 μm) formed on the surface of the solar cell is 15% to 85%.

[0030] (Component 3)

[0031] Configuration 3 is a solar cell of configuration 1 or 2, wherein the electrode further comprises 0.1 to 5.0 parts by weight of glass material relative to 100 parts by weight of silver (Ag) contained in the electrode.

[0032] (Component 4)

[0033] Configuration 4 is a solar cell of Configuration 3, wherein the glass transition temperature of the glass material is 250 to 600°C.

[0034] (Component 5)

[0035] Configuration 5 is a solar cell of configuration 3 or 4 as follows, that is, the glass material mentioned above contains at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O and ZnO.

[0036] (Composition 6)

[0037] Configuration 6 is a solar cell of any one of Configurations 3 to 5 below, that is, the glass material described above does not substantially contain PbO.

[0038] (Component 7)

[0039] Configuration 7 is a solar cell of any one of Configurations 1 to 6 below, that is, the above electrodes do not substantially contain lead (Pb).

[0040] (Composition 8)

[0041] Configuration 8 is a solar cell of any one of Configurations 1 to 7 below, that is, the electrode described above does not substantially contain aluminum particles.

[0042] (Composition 9)

[0043] Configuration 9 is a solar cell of any one of configurations 1 to 8, wherein the substrate is a crystalline silicon substrate of the first conductivity type.

[0044] The aforementioned impurity diffusion layer is an impurity diffusion layer of the second conductivity type.

[0045] The aforementioned electrode is a light incident side surface electrode disposed on the light incident side surface.

[0046] The aforementioned solar cell further includes a back electrode configured to be electrically connected to a surface of the crystalline silicon substrate opposite to the light-incident surface.

[0047] The light incident side surface electrode is a light incident side surface electrode that has been treated as follows: while applying a voltage between the back electrode and the light incident side surface electrode to allow a current to flow in the opposite direction between the impurity diffusion layer of the second conductivity type and the crystalline silicon substrate of the first conductivity type, light from a point source is irradiated onto the light incident side surface of the solar cell.

[0048] According to the present invention, a high-efficiency crystalline silicon solar cell with high open-circuit voltage (Voc) and fill factor (FF) can be provided. In particular, according to the present invention, in order to obtain a high-efficiency crystalline silicon solar cell with high open-circuit voltage (Voc) and fill factor (FF), a crystalline silicon solar cell with a given structure between the electrode and the substrate can be provided. Attached Figure Description

[0049] Figure 1 This is an example of a cross-sectional schematic diagram of a crystalline silicon solar cell according to this embodiment.

[0050] Figure 2 This is an example of a schematic diagram of the light-incident side surface of a crystalline silicon solar cell.

[0051] Figure 3 This is an example of a schematic diagram of the back side of a crystalline silicon solar cell.

[0052] Figure 4 This is an example of a cross-sectional schematic diagram of a bifacial light-receiving crystalline silicon solar cell according to this embodiment.

[0053] Figure 5 This is an example of a cross-sectional schematic diagram of the area near the light-incident surface electrode (sub-gate electrode) of a typical crystalline silicon solar cell, and it is a cross-sectional schematic diagram showing the state in which the anti-reflection film (passivation film) between the electrode and the impurity diffusion layer disappears due to burn-through.

[0054] Figure 6 This is a cross-sectional SEM (scanning electron microscope) image (magnification: 20,000x) of the passivation film on the light-incident side surface of the crystalline silicon solar cell of Example 3, which is a diagram used to illustrate the depth d of the AgSi region.

[0055] Figure 7 This is a cross-sectional SEM (scanning electron microscope) image (magnification: 20,000x) of the passivation film near the light-incident surface of the crystalline silicon solar cell of Example 3, and is a graph used to illustrate the passivation film retention rate Lp / (Lp+Le).

[0056] Figure 8 This is a cross-sectional SEM (scanning electron microscope) image (magnification: 20,000x) of the passivation film on the light-incident side surface of the crystalline silicon solar cell of Comparative Example 1. Detailed Implementation

[0057] The embodiments of the present invention will now be described in detail. It should be noted that the following embodiments are merely illustrative of the present invention and do not limit the scope of the invention.

[0058] Solar cells

[0059] Figure 1 The diagram shows an example of a cross-sectional schematic of a solar cell according to this embodiment. The solar cell of this embodiment includes: a substrate comprising crystalline silicon (crystalline silicon substrate 1), a passivation film 2, and an electrode (e.g., a light-incident side surface electrode 20). Furthermore, the solar cell of this embodiment further includes at least one AgSi region 30 disposed at least a portion between the electrode and the substrate.

[0060] <<Substrate>>

[0061] The solar cell of this embodiment includes a substrate. The substrate of the solar cell of this embodiment is a crystalline silicon substrate 1. Therefore, the solar cell of this embodiment is a crystalline silicon solar cell.

[0062] In this specification, "crystalline silicon" includes both monocrystalline and polycrystalline silicon. Furthermore, the term "crystalline silicon substrate" refers to a material in which crystalline silicon is shaped into a planar or other shape suitable for forming semiconductor devices such as electrical or electronic components. Any method can be used to manufacture crystalline silicon. For example, the Chuklaski method can be used for monocrystalline silicon, and the casting method can be used for polycrystalline silicon. Additionally, polycrystalline silicon ribbons manufactured using other methods, such as those produced by the Czochralski method, or polycrystalline silicon formed on dissimilar substrates such as glass, can also be used as the crystalline silicon substrate 1. Furthermore, the term "crystalline silicon solar cell" refers to a solar cell manufactured using the crystalline silicon substrate 1. In this specification, the crystalline silicon substrate 1 is sometimes simply referred to as "substrate."

[0063] In conventional solar cells, materials used as the semiconductor substrate include crystalline silicon, silicon carbide, germanium, and gallium arsenide. From the perspectives of safety and cost, crystalline silicon (monocrystalline silicon and polycrystalline silicon, etc.) is preferred as the semiconductor substrate material for solar cells.

[0064] The crystalline silicon substrate 1 of the solar cell in this embodiment is either an n-type crystalline silicon substrate 1 or a p-type crystalline silicon substrate 1 containing n-type or p-type impurities. Examples of n-type impurities in the n-type crystalline silicon substrate 1 include group 13 elements such as boron (B), aluminum (Al), and gallium (Ga). Examples of p-type impurities in the p-type crystalline silicon substrate 1 include group 15 elements such as phosphorus (P), arsenic (As), and antimony (Sb).

[0065] like Figure 1 As shown, the solar cell of this embodiment includes an impurity diffusion layer 4 on at least a portion of at least one surface of the crystalline silicon substrate 1. In the case of the solar cell of this embodiment, the impurity diffusion layer 4 formed on the light incident side surface is a p-type or n-type impurity diffusion layer 4. It should be noted that, in this specification, as... Figure 1 As shown, the portion of the substrate in which the impurity diffusion layer 4 is not formed is sometimes referred to as the "substrate body 6".

[0066] In this specification, in crystalline silicon containing n-type or p-type impurities, one conductivity type (n-type or p-type) is referred to as the first conductivity type, and the other conductivity type (p-type or n-type) that is not the first conductivity type is referred to as the second conductivity type. When the crystalline silicon substrate 1 is of the first conductivity type, the impurity diffusion layer 4 is an impurity diffusion layer of the second conductivity type. Specifically, when the crystalline silicon substrate 1 is an n-type crystalline silicon substrate 1 containing n-type impurities, the impurity diffusion layer 4 formed on at least one surface of the crystalline silicon substrate 1 is a p-type impurity diffusion layer 4. Conversely, when the crystalline silicon substrate 1 is a p-type crystalline silicon substrate 1 containing p-type impurities, the impurity diffusion layer 4 formed on at least one surface of the crystalline silicon substrate 1 is an n-type impurity diffusion layer 4. By selecting the first and second conductivity types in this way, a pn junction can be formed near the surface of the crystalline silicon substrate 1 on which the impurity diffusion layer 4 is formed.

[0067] In this embodiment, the first conductivity type of the solar cell is preferably an n-type crystalline silicon substrate 1. Furthermore, the second conductivity type of the solar cell in this embodiment is preferably a p-type impurity diffusion layer 4. Generally, the electron mobility as a charge carrier in the n-type crystalline silicon substrate 1 is higher than the hole mobility as a charge carrier in the p-type crystalline silicon substrate 1. Therefore, using an n-type crystalline silicon substrate 1 is advantageous for obtaining a solar cell with high conversion efficiency.

[0068] The sheet resistance of the impurity diffusion layer 4 is preferably 30–300 Ω / □ (square), 40–160 Ω / □ (square), and more preferably 45–120 Ω / □. Furthermore, the depth of the impurity diffusion layer 4 can be 0.3 μm to 1.0 μm. It should be noted that the depth of the impurity diffusion layer 4 refers to the depth from the surface of the impurity diffusion layer 4 to the pn junction. The depth of the pn junction can be set to the depth from the surface of the impurity diffusion layer 4 to a depth where the impurity concentration in the impurity diffusion layer 4 is the same as the impurity concentration in the substrate body 6.

[0069] It should be noted that in this specification, the impurity diffusion layer 4 of the crystalline silicon solar cell of this embodiment is sometimes referred to as the "silicon emitter layer".

[0070] <<Passivation Film 2>>

[0071] The solar cell of this embodiment includes a passivation film 2. The passivation film 2 is disposed on at least a portion of the impurity diffusion layer 4 of the substrate.

[0072] The passivation film 2 can function as an anti-reflective film. In this specification, the passivation film 2 formed on the light incident side surface of the crystalline silicon substrate 1 is sometimes referred to as an anti-reflective film.

[0073] The passivation film 2 can be a single layer or multiple layers. When the passivation film 2 is a single layer, from the perspective of effectively passivating the surface of the silicon substrate, a thin film (SiN film) using silicon nitride (SiN) as the material is preferred. Alternatively, when the passivation film 2 is multiple layers, it can be a laminate of a thin film using silicon nitride as the material and a thin film using silicon oxide as the material (SiN / SiO). x (Membranes). It should be noted that in SiN / SiO... x When the film is passivation film 2, from the perspective of being able to more effectively passivate the surface of the silicon substrate, it is preferable to make SiO x SiO is formed by contacting the film with the silicon substrate 1. x Membrane, in SiO x A SiN film is formed on the membrane. SiO x The film can be the natural oxide film of the silicon substrate.

[0074] Figure 5 The image shows an example of a typical cross-sectional schematic diagram of a crystalline silicon solar cell. For example... Figure 5 As shown, in a typical crystalline silicon solar cell, a passivation film 2 (anti-reflection film) is formed on the impurity diffusion layer 4. Furthermore, an electrode pattern for the light-incident side surface electrode 20 (surface electrode) is printed onto the passivation film 2 using a conductive paste, such as through screen printing. The conductive paste is then dried and fired at a given temperature to form the light-incident side surface electrode 20. In a typical crystalline silicon solar cell, during firing at this given temperature, the conductive paste burns through the passivation film 2. This burn-through allows the light-incident side surface electrode 20 to form in electrical contact with the impurity diffusion layer 4 in a typical crystalline silicon solar cell. It should be noted that burn-through refers to the etching of the passivation film 2, which serves as an insulating film, by a glass frit or similar material contained in the conductive paste, thereby making the light-incident side surface electrode 20 conductive with the impurity diffusion layer 4. Figure 5 In the typical example of a crystalline silicon solar cell shown, during the firing of the electrode pattern, the electrode pattern burns through the passivation film 2, thereby the passivation film 2 disappears, and the light incident side surface electrode 20 comes into contact with the impurity diffusion layer 4.

[0075] On the other hand, such as Figure 1As shown, in the case of the crystalline silicon solar cell of this embodiment, a passivation film 2 (anti-reflection film) is present in most of the space between the surface electrode 20 on the light incident side and the impurity diffusion layer 4. Therefore, in the case of the crystalline silicon solar cell of this embodiment, most of the passivation film 2 in the portion of the passivation film 2 that contacts the impurity diffusion layer 4 of the crystalline silicon substrate 1, excluding the AgSi region 30 described later, can remain unchanged. Due to the presence of the passivation film 2, the increase in surface defect density, which is a cause of carrier recombination, can be prevented. As a result, the crystalline silicon solar cell of this embodiment can obtain a high open-circuit voltage (Voc).

[0076] In the case of the crystalline silicon solar cell of this embodiment, after firing for forming the electrode, a large portion of the passivation film 2 between the electrode and the impurity diffusion layer 4 remains. In this specification, the degree to which the passivation film 2 remains between the electrode and the crystalline silicon substrate 1 after firing for forming the electrode is expressed as the passivation film 2 retention rate. The passivation film 2 retention rate will be described later.

[0077] <<Electrode>>

[0078] The solar cell of this embodiment includes electrodes. The electrodes of the solar cell of this embodiment are disposed on at least a portion of the passivation film 2. Furthermore, the electrodes of the solar cell of this embodiment contain silver (Ag).

[0079] like Figure 1 As shown, a sub-gate electrode 20b is disposed on the light-incident side surface of a crystalline silicon solar cell as a light-incident side surface electrode 20. Figure 1 In the example shown, holes in electron-hole pairs generated by incident light onto a crystalline silicon solar cell are collected at the sub-gate electrode 20b via an impurity diffusion layer 4 (e.g., a p-type impurity diffusion layer 4). Therefore, a low contact resistance between the sub-gate electrode 20b and the impurity diffusion layer 4 is required.

[0080] It should be noted that, in Figure 1 The back side of the crystalline silicon solar cell shown is provided with a back electrode 15 on the side opposite to the light incident side surface. In this specification, the light incident side surface electrode 20 and the back electrode 15, which serve as electrodes for extracting current from the crystalline silicon solar cell to the outside, are sometimes simply referred to as "electrodes".

[0081] Figure 4 The diagram shows an example of a cross-sectional schematic of a bifacial light-receiving crystalline silicon solar cell (bifacial power-generating crystalline silicon solar cell) according to this embodiment. Figure 4 The crystalline silicon solar cell shown can generate electricity by receiving light from two surfaces (the first and second light-incident surfaces).

[0082] Generally, the electrodes of crystalline silicon solar cells can be formed by printing a conductive paste using methods such as screen printing and then firing it. In this specification, the conductive paste used to form the electrodes of the crystalline silicon solar cell of this embodiment is sometimes referred to as a given conductive paste. Generally, the conductive paste contains conductive particles and an organic carrier. Furthermore, the conductive paste may further contain glass frit in addition to the conductive particles and organic carrier. The electrodes of the solar cell of this embodiment contain silver (Ag). Therefore, the conductive particles contained in the given conductive paste need to contain silver (Ag). The organic carrier contained in the conductive paste is burned off during firing to form the electrode. Therefore, the fired electrode contains components contained in the conductive paste other than the organic carrier. Specifically, the fired electrode contains conductive components originating from the conductive particles of the conductive paste. Furthermore, if the conductive paste contains glass frit, the fired electrode further contains components originating from the glass frit of the conductive paste.

[0083] From the perspective of obtaining low resistance and high reliability, the conductive component in a given electrode of the crystalline silicon solar cell of this embodiment is preferably composed only of silver. It should be noted that the conductive component composed only of silver may contain other metallic elements as unavoidable impurities.

[0084] In this specification, the term "glass frit" refers to a substance primarily composed of various oxides, such as metal oxides, typically used in the form of glassy particles. During the firing process used to form electrodes, the glass frit softens, and the particles bond together. In this specification, the component (oxides) of the glass frit contained in the electrode is also simply referred to as "glass frit."

[0085] In the solar cell of this embodiment, the content of glass frit in the electrode is preferably 0.1 to 5.0 parts by weight relative to the content of silver (Ag) in the electrode per 100 parts by weight, more preferably 0.2 to 4.0 parts by weight, even more preferably 0.3 to 3.0 parts by weight, and particularly preferably 0.4 to 2.7 parts by weight. By keeping the content of glass frit within an appropriate range, the reactivity of the glass frit to the passivation film 2 can be made appropriate during the firing process used to form the electrode.

[0086] In the solar cell of this embodiment, the glass transition temperature of the glass frit contained in the electrode is preferably 250–600°C, more preferably 270–500°C, and even more preferably 300–400°C. By setting the glass transition temperature (Tg) of the glass frit to 250°C or higher, the reactivity to the passivation film 2 can be suppressed. In addition, by setting the glass transition temperature (Tg) to 600°C or lower, the contact resistance between the resulting electrode (e.g., the light incident side surface electrode 20) and the impurity diffusion layer 4 can be reduced.

[0087] In the solar cell of this embodiment, the glass frit contained in the electrode preferably comprises at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, BaO, CuO, Li2O, and ZnO. More preferably, the glass frit contained in the electrode comprises at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O, and ZnO. By including at least one of these oxides in the glass frit, the basicity of the glass frit can be adjusted to an appropriate range. By adjusting the basicity of the glass frit to an appropriate range, the reactivity of the glass frit to the passivation film 2 can be appropriately ensured during firing to form the electrode.

[0088] Although not specifically limited, the glass frit contained in the electrodes of the solar cell of this embodiment may substantially not contain PbO. Furthermore, the electrodes of the solar cell of this embodiment may substantially not contain lead (Pb). In this specification, "lead-free glass frit" means glass frit that substantially does not contain lead (Pb). Since the glass frit is manufactured using metal oxides as raw materials, lead-free glass frit means glass frit that substantially does not contain lead oxide (PbO). When manufacturing lead-free glass frit, materials containing lead (PbO) are not intentionally used. However, lead-free glass frit may contain trace amounts of lead that are unavoidably mixed in as impurities. Specifically, the lead-free glass frit of this embodiment may contain less than 0.1% by weight of lead as an impurity per 100% by weight of the glass frit.

[0089] In the manufacture of conventional crystalline silicon solar cells, the glass frit contained in the conductive paste used for electrode formation is lead-containing glass frit (PbO). This is because, in the case of conventional crystalline silicon solar cells, by including lead-containing glass frit in the conductive paste for electrode formation, the contact resistance between the light-incident surface electrode 20 and the impurity diffusion layer 4 can be reduced. However, lead can have adverse effects on human health. When products are manufactured using lead-containing materials, lead may pollute the environment upon product disposal. Therefore, it is desirable to use lead-free materials that do not contain lead when manufacturing products. Therefore, it is preferable to use lead-free glass frit in the solar cell manufacturing process. By using lead-free glass frit, it is possible to manufacture solar cells with electrodes that are substantially free of lead (Pb). Therefore, lead pollution to the environment can be suppressed.

[0090] Furthermore, in this embodiment, the materials other than the electrodes of the crystalline silicon solar cell may also be substantially lead-free. To prevent lead pollution of the environment, the crystalline silicon solar cell of this embodiment is preferably a lead-free solar cell.

[0091] The electrode of the solar cell in this embodiment may further contain an aluminum component derived from aluminum particles. The aluminum particles may be included as particles different from the conductive particles in (A). If the conductive paste used to form the electrode contains aluminum, the electrode also contains aluminum.

[0092] In the crystalline silicon substrate 1, aluminum has the property of being a p-type impurity. During the firing of the conductive paste printed on the crystalline silicon, aluminum in the conductive paste diffuses into the crystalline silicon, becoming a p-type impurity. Therefore, when an electrode is formed on the surface of the p-type semiconductor layer of the crystalline silicon substrate 1, by including aluminum particles in the conductive paste, a low contact resistance can be obtained between the electrode and the p-type semiconductor layer. Therefore, when an electrode is formed on the surface of the p-type semiconductor layer of the crystalline silicon substrate 1, the conductive paste can include aluminum particles.

[0093] On the other hand, because the conductive paste contains aluminum particles, the adhesion of the electrode to the p-type semiconductor layer is reduced, resulting in the problem that the electrode can easily peel off from the p-type semiconductor layer of the solar cell. In other words, because the conductive paste contains aluminum particles, the reliability of the electrode to the p-type semiconductor layer is significantly compromised.

[0094] Furthermore, in order to electrically connect multiple solar cell units, metal solder strips are used to interconnect the electrodes of the solar cells. When the conductive paste used for electrode formation contains aluminum particles, there is a problem of reduced welding strength between the metal solder strips and the electrodes.

[0095] Based on the above description, the conductive paste of this embodiment preferably contains aluminum particles in a given amount or less, or does not contain aluminum particles.

[0096] Specifically, the aluminum particles are as follows. The conductive paste of this embodiment further contains 0.5 parts by weight or less of aluminum particles relative to 100 parts by weight of silver particles (A), or does not contain aluminum particles. Furthermore, the upper limit of the aluminum particle content in the conductive paste of this embodiment is preferably 0.3 parts by weight or less relative to 100 parts by weight of silver particles (A), more preferably less than 0.3 parts by weight, and even more preferably 0.25 parts by weight or less. The conductive paste of this embodiment can be a conductive paste that does not contain aluminum particles. It should be noted that "does not contain aluminum particles" means excluding the intentional addition of "aluminum particles," but does not exclude the inclusion of aluminum components as unavoidable impurities.

[0097] Furthermore, in this invention, at least one AgSi region is formed in at least a portion between the electrode and the substrate. Thus, when the electrode is formed on the surface of the p-type semiconductor layer of the crystalline silicon substrate 1, even if the electrode does not substantially contain aluminum, a low contact resistance can be obtained between the electrode and the p-type semiconductor layer.

[0098] On the other hand, if the conductive paste used to form the electrode contains aluminum, it has an impact from a reliability point of view.

[0099] like Figure 2 and 3 As shown, the electrodes of a crystalline silicon solar cell can include a light-incident side main grid electrode 20a and / or a back TAB electrode 15a. The light-incident side main grid electrode 20a has the function of electrically connecting the sub-grid electrode 20b, which is used to collect the current generated by the solar cell, to an interconnecting metal solder strip. Similarly, the back TAB electrode 15a has the function of electrically connecting the back full-face electrode 15b, which is used to collect the current generated by the solar cell, to an interconnecting metal solder strip. If the sub-grid electrode 20b contacts the crystalline silicon substrate 1, the surface defect density of the surface (interface) of the crystalline silicon substrate 1 at the contact point of the sub-grid electrode 20b increases, and the performance of the solar cell decreases. In the crystalline silicon solar cell of this embodiment, the passivation film 2 (anti-reflection film) is not completely burned through when the sub-grid electrode 20b is formed. Therefore, most of the passivation film 2 at the contact point with the crystalline silicon substrate 1 can remain unchanged, preventing the increase in surface defect density that is a cause of carrier recombination. As a result, a crystalline silicon solar cell with a high open-circuit voltage (Voc) can be obtained.

[0100] Figure 1 The crystalline silicon solar cell shown can have Figure 3 The back electrode 15 of the structure shown is configured to be electrically connected to another surface of the semiconductor substrate of the first conductivity type. Figure 3 As shown, the back electrode 15 may typically include a back full electrode 15b and a back TAB electrode 15a electrically connected to the back full electrode 15b.

[0101] Figure 1 The main grid electrode of the crystalline silicon solar cell shown contains Figure 2 The light incident side main gate electrode 20a and shown Figure 3 The back TAB electrode 15a is shown. Interconnect metal solder strips, covered with solder, are bonded to the light-incident side main grid electrode 20a and the back TAB electrode 15a. These solder strips are used to extract the current generated by the solar cell to the outside of the crystalline silicon solar cell unit. Figure 4 The bifacial light-receiving crystalline silicon solar cell shown can also have a light-incident side main grid electrode 20a and a back TAB electrode 15a with the same shape as the light-incident side main grid electrode 20a.

[0102] The width of the main grid electrodes (light-incident side main grid electrode 20a and back TAB electrode 15a) can be the same as the width of the interconnect metal solder strips. To ensure low resistance of the main grid electrodes, a large width is preferred. On the other hand, to increase the incident area of ​​light relative to the light-incident side surface, a small width of the light-incident side main grid electrode 20a is preferable. Therefore, the width of the main grid electrodes can be set to 0.05–5 mm, preferably 0.08–3 mm, more preferably 0.1–2 mm, and even more preferably 0.15–1 mm. Furthermore, the number of main grid electrodes can be determined according to the size of the crystalline silicon solar cell. The number of main grid electrodes is optional. Specifically, the number of main grid electrodes can be 3 or 4, or more. The optimal number of main grid electrodes can be determined by simulating the operation of the solar cell to maximize the conversion efficiency of the crystalline silicon solar cell. It should be noted that since the crystalline silicon solar cells are interconnected in series using interconnect metal solder strips, the number of light-incident side main grid electrodes 20a and back TAB electrodes 15a is preferably the same. For the same reason, the widths of the light incident side main gate electrode 20a and the back TAB electrode 15a are preferably the same.

[0103] To increase the incident area of ​​light on the crystalline silicon solar cell, the area occupied by the light-incident surface electrode 20 on the light-incident side surface is preferably as small as possible. Therefore, the sub-gate electrode 20b on the light-incident side surface is preferably as narrow as possible and preferably has as few electrodes as possible. On the other hand, from the perspective of reducing electrical losses (ohmic losses), it is preferable that the sub-gate electrode 20b has a large width and a large number of electrodes. In addition, from the perspective of reducing the contact resistance between the sub-gate electrode 20b and the crystalline silicon substrate 1 (impurity diffusion layer 4), it is also preferable that the sub-gate electrode 20b has a large width. According to the above explanation, the number of main grid electrodes can also be determined according to the size of the crystalline silicon solar cell and the width of the main grid electrode. The optimal width and number of sub-gate electrodes 20b (the spacing of the sub-gate electrodes 20b) can be determined by simulating the operation of the solar cell to maximize the conversion efficiency of the crystalline silicon solar cell. It should be noted that, regarding Figure 4 The width and number of the back sub-gate electrodes 15c of the back electrode 15 of the bifacial light-receiving crystalline silicon solar cell shown can also be determined in the same way.

[0104] <<AgSi Region 30>>

[0105] The solar cell of this embodiment includes at least one AgSi region 30. The AgSi region 30 is disposed in at least a portion between the electrode and the substrate. Figure 6 An example of AgSi region 30 is shown in the SEM image. AgSi region 30 only needs to be disposed in at least a portion between the electrode and the substrate; for example, it can also be... Figure 6The area indicated by symbol 30 surrounded by a dashed line in the SEM image is designated as AgSi region 30.

[0106] In manufacturing the solar cell of this embodiment, silver (Ag) contained in the electrode diffuses into the silicon (Si) of the substrate, thereby forming an alloy of silver (Ag) and silicon (Si) in at least a portion between the electrode and the substrate. In this specification, the region of the silver (Ag) and silicon (Si) alloy formed during the manufacturing of the solar cell of this embodiment is referred to as "AgSi region 30". AgSi region 30 can be determined as a region where both Ag and Si are detected when the cross-section of the solar cell of this embodiment is measured using an energy dispersive X-ray fluorescence spectrometer (hereinafter sometimes referred to as EDX).

[0107] The term "one AgSi region 30" refers to an AgSi region 30 that is separate from other AgSi regions 30. Figure 6 The SEM image shows one AgSi region 30. The solar cell of this embodiment preferably has multiple spot-like AgSi regions 30 in at least a portion between the electrode and the substrate. The AgSi regions 30 participate in electrical conduction between the electrode and the impurity diffusion layer 4 as local conductive portions.

[0108] In the crystalline silicon solar cell of this embodiment, for example, when a cross-section of 1 mm in length, which is part of the sub-gate electrode, is observed by SEM, approximately 1 to 3 spot-like AgSi regions 30 are present. Therefore, the portion containing AgSi regions 30 can be considered an extremely small portion of the region where the electrode is formed.

[0109] The crystalline silicon solar cell of this embodiment includes at least one AgSi region 30 with a depth d of 100 nm or more.

[0110] In this specification, the depth d of the so-called AgSi region 30 refers to... Figure 6 The SEM image obtained by SEM observation of the cross-section of AgSi region 30 shown refers to any one point at the interface between the electrode and AgSi region 30. Figure 6 B1) is connected to any one point at the interface between the substrate and the AgSi region 30. Figure 6 The length of the longest line segment among the line segments (B2) (connecting) Figure 6The length d of the line segment between B1 and B2. Specifically, in the AgSi region 30 determined by SEM image superimposed with EDX measurement obtained by SEM observation of the cross section near the passivation film 2 at a magnification of 20,000, the given line segment is determined and the length of the given line segment is measured, thereby obtaining the depth d of the AgSi region 30.

[0111] The depth d of the AgSi region 30 is preferably 100–4000 nm, more preferably 120–3000 nm, even more preferably 130–2500 nm, and particularly preferably 150–2000 nm. By setting the depth d of the AgSi region 30 to this range, the contact resistance is reduced, and a high-efficiency crystalline silicon solar cell with a high fill factor (FF) can be obtained.

[0112] In this embodiment, the AgSi region 30 of the solar cell is preferably formed by a laser processing process. The laser processing process refers to treating the light-incident side surface electrode 20 by applying a voltage between the back electrode 15b and the light-incident side surface electrode 20 to allow a current flowing in the opposite direction between the second conductivity type impurity diffusion layer 4 and the first conductivity type crystalline silicon substrate 1, while irradiating the light-incident side surface of the solar cell with light from a point source. In this case, the solar cell further includes a back electrode 15b arranged in a manner electrically connected to the surface of the crystalline silicon substrate 1 opposite to the light-incident side surface. Using the laser processing process, a suitable AgSi region 30 can be formed.

[0113] Details about the laser processing technology will be described later.

[0114] Figure 4 The diagram shows an example of a cross-sectional schematic of a bifacial crystalline silicon solar cell. Figure 4 The illustrated double-sided light-receiving crystalline silicon solar cell has an impurity diffusion layer 4, a passivation film 2 (anti-reflection film), and a back passivation film 14. The given structure of the electrode containing the AgSi region 30 is as follows... Figure 4 As shown, this structure can also be suitably applied as the back electrode 15 (back sub-gate electrode 15c) of a bifacial light-receiving crystalline silicon solar cell. Therefore, in a bifacial light-receiving crystalline silicon solar cell, when forming the light-incident side surface electrode 20 (especially the sub-gate electrode 20b) and the back electrode 15 (back sub-gate electrode 15c) on the light-incident side surface, a given AgSi region 30 can be formed near both the light-incident side surface and the back surface.

[0115] <<Residual rate of passivation film 2>>

[0116] In this specification, the degree to which the passivation film 2 exists between the electrode and the impurity diffusion layer 4 of the crystalline silicon substrate 1 after firing for forming the electrode in the solar cell of this embodiment is expressed as the retention rate of the passivation film 2. It should be noted that the passivation film 2 disappears in the regions where the AgSi region 30 is formed. Since the AgSi region 30 is not formed in the regions where the passivation film 2 exists, the so-called retention rate of the passivation film 2 can be considered as the proportion of the region near the AgSi region 30 where the AgSi region 30 is not formed.

[0117] use Figure 7 The example of a SEM image of a cross-section of a solar cell illustrates the method for determining the retention rate of the passivation film 2. First, to obtain the retention rate of the passivation film 2, a cross-section containing the passivation film 2 and the AgSi region 30 is observed using SEM at a magnification of 20,000, thereby obtaining an SEM image. It should be noted that the transverse (horizontal direction) length of this SEM image is 5.7 μm, and the longitudinal (perpendicular direction) length is 3.9 μm. Then, the total length Lp of the cross-section of the passivation film 2 in this SEM image is measured. Figure 7 In the example shown, the total length Lp of the cross-section of the passivation film 2 in the SEM image is the sum of the lengths of Lp1, Lp2, Lp3, and Lp4. Then, in this SEM image, the total length Le of the cross-section of the interface between the AgSi region 30 and the electrode in the portion where the AgSi region 30 is formed is measured. Length Le corresponds to the length by which the passivation film 2 disappears during the solar cell manufacturing process. Figure 7 In the example shown, the total length Le of the cross-section of the interface between the AgSi region 30 and the electrode in the portion where the AgSi region 30 is formed is the total length of Le1 and Le2. The retention rate of the passivation film 2 can be obtained as Lp / (Lp+Le). It should be noted that the portion of the passivation film 2 that disappears during the solar cell manufacturing process can be determined using EDX-based measurements. Furthermore, the lengths of Le1, etc., can be measured by approximating the passivation film 2, etc., as a straight line.

[0118] In the crystalline silicon solar cell of this embodiment, the residual rate of the passivation film 2 is 10% to 90%, preferably 30% or more and less than 90%, more preferably 50% or more and less than 90%, and even more preferably 70% to 89%. By making the residual rate of the passivation film 2 within an appropriate range, a high-efficiency crystalline silicon solar cell with high open-circuit voltage (Voc) and fill factor (FF) can be obtained.

[0119] <<Thickness ratio of passivation film 2 before and after firing>>

[0120] In this specification, the film thickness ratio before and after firing of the passivation film 2 is the ratio (Db / Da) of the film thickness Da of the passivation film 2 before firing for forming the electrode to the film thickness Db of the passivation film 2 after firing for forming the electrode (after the solar cell is completed). In this specification, the film thickness ratio before and after firing is sometimes simply referred to as "film thickness ratio (Db / Da)".

[0121] In the solar cell of this embodiment, the film thickness ratio (Db / Da) is preferably 15% to 85%, more preferably 20% to 70%, and even more preferably 30% to 60%. By setting the film thickness ratio (Db / Da) of the passivation film 2 to a given range, it is possible to prevent the increase in surface defect density, which is a cause of carrier recombination, during power generation in the solar cell of this embodiment.

[0122] In this specification, the pre-firing thickness Da of the passivation film 2 refers to the thickness of the passivation film 2 when it is formed on a given substrate. The thickness Da immediately after film formation can be measured by SEM observation of a cross-section near the passivation film 2 before electrode formation.

[0123] In this specification, the so-called film thickness Db after the solar cell is completed refers to the thickness of the passivation film 2 in a scanning electron microscope image of a 5.7 μm × 3.9 μm cross section containing the AgSi region 30 of the solar cell after the electrode is formed by firing on the surface of the solar cell.

[0124] In this specification, the thickness Db of the passivation film 2 in a 5.7 μm × 3.9 μm cross-section of the solar cell containing the AgSi region 30, as seen in a scanning electron microscope image of the completed solar cell after electrodes are formed on the surface of the solar cell, refers to the thickness of the passivation film 2 near the AgSi region 30 in the completed solar cell after forming electrodes and the AgSi region 30 by forming an electrode pattern on the passivation film 2 formed on a given substrate using a given conductive paste, performing a given firing process, etc. Sometimes, the film thickness Db is referred to as "the film thickness Db after the solar cell is completed". The film thickness Db after the solar cell is completed can be determined by observing a 5.7 μm × 3.9 μm image area of ​​the cross-section containing the passivation film 2 and the AgSi region 30 in the completed solar cell after the electrodes and the AgSi region 30 are formed using SEM. That is, the final film thickness Db of the completed solar cell is the film thickness Db of the passivation film 2 in a scanning electron microscope image of a 5.7 μm × 3.9 μm cross-section containing the AgSi region 30 of the completed solar cell. Specifically, the cross-section containing the passivation film 2 and the AgSi region 30 is observed by SEM at a magnification of 20,000, thereby obtaining an SEM image (SEM image range: 5.7 μm × 3.9 μm). The SEM image is divided into 6 equal parts along the longitudinal direction, and the film thickness of the passivation film 2 at the 5 intersections of the 6-part image is measured (5 locations). The average of the film thicknesses at the 5 locations can be used to obtain the final film thickness Db of the passivation film 2 of the completed solar cell.

[0125] <Methods for Manufacturing Solar Cells>

[0126] The manufacturing method of the crystalline silicon solar cell of this embodiment will now be described.

[0127] The method for manufacturing a solar cell according to this embodiment includes a step of forming an electrode (light incident side surface electrode 20) by printing a given conductive paste onto the surface of a passivation film 2 (anti-reflection film) on a semiconductor layer (impurity diffusion layer 4) of the second conductivity type, followed by drying and firing. The given conductive paste will be described later.

[0128] The method for manufacturing a solar cell according to this embodiment includes a step of preparing a first conductivity type (p-type or n-type) crystalline silicon substrate 1. As the semiconductor substrate of the first conductivity type, either an n-type crystalline silicon substrate 1 or a p-type crystalline silicon substrate 1 can be used. In the solar cell of this embodiment, since it is possible to obtain a solar cell with higher efficiency, it is preferable to use an n-type crystalline silicon substrate 1.

[0129] It should be noted that, from the viewpoint of obtaining high conversion efficiency, the surface of the light incident side of the crystalline silicon substrate 1 preferably has a pyramid-shaped texture structure.

[0130] Subsequently, the method for manufacturing a solar cell according to this embodiment includes a step of forming a second conductivity type impurity diffusion layer 4 on one surface of a first conductivity type semiconductor substrate.

[0131] When using an n-type crystalline silicon substrate 1 as the crystalline silicon substrate 1, the impurity diffusion layer 4 can be, for example, a p-type impurity diffusion layer 4 formed by diffusing elements such as boron (B), which are p-type impurities. It should be noted that a p-type crystalline silicon substrate 1 can also be used to manufacture crystalline silicon solar cells. In this case, the impurity diffusion layer 4 is an n-type impurity diffusion layer 4 formed by diffusing elements such as phosphorus (P), which are n-type impurities.

[0132] When forming the impurity diffusion layer 4, it can be formed in such a way that the sheet resistance of the impurity diffusion layer 4 is 30 to 300 Ω / □ (square), preferably 40 to 150 Ω / □, and more preferably 45 to 120 Ω / □. Furthermore, in the manufacturing method of the crystalline silicon solar cell of this embodiment, the depth of the impurity diffusion layer 4 can be set to 0.3 μm to 1.0 μm. The sheet resistance and depth of the impurity diffusion layer 4 can be controlled by adjusting the concentration of the dopant coated on the crystalline silicon substrate 1 and conditions such as the temperature and / or time for the diffusion of impurity elements.

[0133] The method for manufacturing a solar cell according to this embodiment includes a step of forming a back electrode 15 in a manner electrically connected to another surface of a semiconductor substrate of the first conductivity type (n-type crystalline silicon substrate 1). It should be noted that the back electrode 15 can be formed either before or after the formation of the light-incident side surface electrode 20. Furthermore, the firing for forming the back electrode 15 can be performed simultaneously with or separately from the firing for forming the light-incident side surface electrode 20.

[0134] Specifically, in the manufacturing method of the crystalline silicon solar cell of this embodiment, a back electrode 15 is formed by printing a conductive paste on another surface (back side) of the crystalline silicon substrate 1 and firing it.

[0135] It should be noted that in manufacturing such as Figure 4 In the case of the bifacial light-receiving crystalline solar cell shown, a second impurity diffusion layer 16 can be formed. Alternatively, a back electrode 15 can be formed using a given conductive paste (conductive composition), and the aforementioned AgSi region 30 is formed between the back electrode 15 and the crystalline silicon substrate 1. Therefore, in the case of the bifacial light-receiving crystalline solar cell, it is preferable to use a given conductive paste to form the back electrode 15. In this case, the back electrode 15 is a sintered body of the given conductive paste.

[0136] Subsequently, the method for manufacturing a solar cell according to this embodiment includes forming a passivation film 2 in a manner that brings it into contact with the surface of a semiconductor layer (impurity diffusion layer 4) of the second conductivity type. The passivation film 2 can function as an anti-reflective film.

[0137] Specifically, in the manufacturing method of the crystalline silicon solar cell of this embodiment, an anti-reflective film that also functions as a passivation film 2 is formed on the surface of the impurity diffusion layer 4 formed in the above-described process. The passivation film 2 (anti-reflective film) can be a silicon nitride film (SiN film). When using a silicon nitride film as the passivation film 2, the silicon nitride film layer also functions as the passivation film 2 on the light incident side surface. Therefore, when using a silicon nitride film as the passivation film 2, a high-performance crystalline silicon solar cell can be obtained. Furthermore, by making the passivation film 2 a silicon nitride film, it is possible to provide anti-reflective properties against incident light. The silicon nitride film can be formed using methods such as PECVD (Plasma Enhanced Chemical Vapor Deposition).

[0138] The method for manufacturing a solar cell according to this embodiment includes a step of forming a light-incident side surface electrode 20 on at least a portion of the surface of a passivation film 2 (anti-reflection film). In the manufacturing method of this embodiment, a given conductive paste, described later, is used to form the light-incident side surface electrode 20. Therefore, the light-incident side surface electrode 20 is a sintered body of the given conductive paste.

[0139] In the manufacturing method of the crystalline silicon solar cell of this embodiment, the light incident side surface electrode 20 is formed by printing a given conductive paste onto the surface of a passivation film 2 (anti-reflection film) and then firing it. It should be noted that the firing for forming the light incident side surface electrode 20 can be performed simultaneously with the firing for forming the back electrode 15.

[0140] Specifically, firstly, the pattern of the light-incident side surface electrode 20 printed using the given conductive paste is dried at a temperature of approximately 100–150°C for several minutes (e.g., 0.5–5 minutes). It should be noted that, at this time, the given conductive paste can be used to form the light-incident side main gate electrode 20a and the light-incident side sub-gate electrode 20b of the light-incident side surface electrode 20.

[0141] After the pattern of the light-incident side surface electrode 20 is printed and dried, a conductive paste for forming the back electrode 15 is then printed and dried. A given conductive paste is preferably used to form the electrodes (light-incident side surface electrode 20 and, depending on the situation, back electrode 15) of a solar cell such as a crystalline silicon solar cell.

[0142] Subsequently, the material obtained by drying the printed conductive paste is fired in an atmosphere under given firing conditions using a firing furnace such as a tubular furnace. The firing atmosphere is atmospheric, and the firing temperature is 500–1000°C, more preferably 600–1000°C, even more preferably 500–900°C, and particularly preferably 700–900°C. Firing is preferably performed within a short time, and the temperature distribution (temperature-time curve) during firing is preferably peak-shaped. For example, it is preferable to use the above-mentioned temperature as the peak temperature, and the furnace entry / exit time is 10–100 seconds, more preferably 20–80 seconds, and even more preferably 40–60 seconds.

[0143] During firing, it is preferable to fire the conductive paste used to form the light-incident side surface electrode 20 and the back electrode 15 simultaneously, thus forming both electrodes at the same time. By printing a given conductive paste onto the light-incident side surface and the back surface in this way and firing it simultaneously, the firing process for electrode formation can be completed in only one step. Therefore, crystalline silicon solar cells can be manufactured at a lower cost.

[0144] The method for manufacturing a solar cell according to this embodiment includes a step of forming the AgSi region 30 described above. In order to form the AgSi region 30, a laser processing process may be performed, for example, in the method for manufacturing a solar cell according to this embodiment.

[0145] The laser processing technology refers to the following process: Between the second conductivity type semiconductor layer and the first conductivity type semiconductor substrate, a voltage is applied to the back electrode 15 and the light-incident side surface electrode 20 to allow current to flow in the pn junction in the opposite direction to the forward direction, while light from a point source is irradiated onto the light-incident side surface of the solar cell. Due to the effect of the light from the point source, charge carriers (electron-hole pairs) are generated inside the semiconductor substrate. The applied voltage enables the movement of these charge carriers, i.e., the flow of current. The voltage is applied in such a way that the direction of current flow in the pn junction is opposite to the forward direction. Therefore, when the semiconductor substrate is an n-type semiconductor substrate and the semiconductor layer is a p-type semiconductor layer, a voltage is applied to the back electrode 15 and the light-incident side surface electrode 20 in such a way that current flows from the n-type semiconductor substrate to the p-type semiconductor layer. Conversely, when the semiconductor substrate is a p-type semiconductor substrate and the semiconductor layer is an n-type semiconductor layer, a voltage is applied to the back electrode 15 and the light-incident side surface electrode 20 in such a way that current flows from the n-type semiconductor layer to the p-type semiconductor substrate.

[0146] In the following description, a solar cell with an n-type crystalline silicon substrate 1 as the semiconductor substrate of the first conductivity type and a p-type impurity diffusion layer 4 (sometimes simply referred to as "impurity diffusion layer 4") as the semiconductor layer of the second conductivity type will be used as an example.

[0147] like Figure 1 As shown, when a laser processing technique is used, a passivation film 2 (anti-reflection film) exists in most of the area between the light-incident surface electrode 20 and the impurity diffusion layer 4. In the laser processing technique, a given voltage is applied in such a way that a current flows in the pn junction in the opposite direction to the forward direction, and light from a point source (e.g., a laser) is irradiated. This causes a current to flow in a small region between the light-incident surface electrode 20 and the impurity diffusion layer 4, resulting in localized heating. As a result, as... Figure 6 and 7 As shown, a region of silver and silicon alloy is formed between the light-incident side surface electrode 20 and the impurity diffusion layer 4, serving as a locally electrically conductive portion (locally conductive section). In this specification, the region of silver (Ag) and silicon (Si) alloy formed by laser processing processes, etc., is referred to as "AgSi region 30". AgSi region 30 can be determined as a region where both Ag and Si are detected by measurement using an energy dispersive X-ray fluorescence spectrometer (hereinafter sometimes referred to as EDX). Furthermore, the passivation film 2 is not present in the region where AgSi region 30 is formed. That is, in the region where AgSi region 30 is formed, the impurity diffusion layer 4 (the silicon emitter layer of the second conductivity type) is electrically conductive to the light-incident side surface electrode 20 via AgSi region 30. Since the locally formed AgSi region 30 is an electrically conductive portion (locally conductive part), good electrical conductivity can be achieved between the light incident side surface electrode 20 and the impurity diffusion layer 4.

[0148] Generally, by performing laser processing, the fill factor (FF) can be increased without reducing the open circuit voltage (Voc), a characteristic of solar cells. By forming a given AgSi region 30, both a higher open circuit voltage (Voc) and a higher fill factor (FF) can be obtained.

[0149] The crystalline silicon solar cell of this embodiment can be manufactured as described above.

[0150] The crystalline silicon solar cell of this embodiment, obtained as described above, is electrically connected using interconnecting metal solder strips. A solar cell module is then manufactured by laminating a glass plate, a sealing material, and a protective sheet. The interconnecting metal solder strips can be metal solder strips covered with solder (e.g., copper-based strips). The solder can be tin-based, specifically commercially available leaded solder or lead-free solder. To obtain lead-free solar cells, lead-free solder is preferred.

[0151] <Conductive paste>

[0152] A given conductive paste that can be used to form the electrodes of the crystalline silicon solar cell of this embodiment will be described. This given conductive paste is suitable for forming the AgSi region 30 described above. Hereinafter, the given conductive paste will sometimes be referred to as the conductive paste of this embodiment.

[0153] The conductive paste of this embodiment exhibits lower reactivity to the passivation film 2 (anti-reflection film) compared to conventional conductive pastes, and thus possesses reactivity with the passivation film 2 (anti-reflection film) suitable for laser processing. Therefore, the conductive paste of this embodiment is preferably used for forming the light-incident side surface electrode 20 of a crystalline silicon solar cell using a laser processing process.

[0154] The inventors have discovered that when a laser processing process is applied to a solar cell with a light-incident side surface electrode 20 formed using a conventional conductive paste, it adversely affects the passivation film 2 (anti-reflective film) and the impurity diffusion layer 4 (and the substrate), resulting in a decrease in the conversion efficiency of the solar cell. Furthermore, the inventors have found that this is because the conventional conductive paste has excessively high burn-through (reactivity) properties towards the passivation film 2 (anti-reflective film).

[0155] The conductive paste that can be used to form the light incident side surface electrode 20 based on laser processing technology needs to have properties different from conventional conductive pastes (conductive pastes that can burn through the passivation film 2).

[0156] Furthermore, the inventors have discovered that by adjusting the alkalinity and content of the lead-free glass frit to an appropriate range, the reactivity of the glass frit to the passivation film 2 (anti-reflective film) can be appropriately adjusted. Since lead-free glass frit is used, lead pollution caused by lead release into the environment can be prevented. Moreover, even when using lead-free glass frit, contact resistance can be reduced to the same extent as with lead-containing glass frit. Based on the above findings, the inventors have discovered a conductive paste that is preferably used in the manufacture of crystalline silicon using laser processing technology.

[0157] By forming the electrodes of a crystalline silicon solar cell using the conductive paste of this embodiment and performing a laser processing process to form a given AgSi region 30, a low contact resistance can be obtained between the electrode and the impurity diffusion layer 4 of the solar cell without compromising the function of the passivation film 2. Therefore, by using the conductive paste of this embodiment to perform a laser processing process to form a given AgSi region 30, a crystalline silicon solar cell with high conversion efficiency can be obtained. When manufacturing a crystalline silicon solar cell, the conductive paste of this embodiment is preferably used to form the given AgSi region 30 using a laser processing process.

[0158] The components contained in the conductive paste of this embodiment will be specifically described.

[0159] <<(A) Conductive particles>>

[0160] The conductive paste of this embodiment contains (A) conductive particles.

[0161] In the conductive paste of this embodiment, metal particles or alloy particles can be used as conductive particles. Examples of metals included in the metal or alloy particles include silver, gold, copper, nickel, zinc, and tin. Silver particles (Ag particles) can be used as the metal particles. It should be noted that the conductive paste of this embodiment may contain metals other than silver, such as gold, copper, nickel, zinc, and tin. From the perspective of obtaining low resistance and high reliability, the conductive particles are preferably silver particles composed of silver. It should be noted that silver particles composed of silver may contain other metallic elements as unavoidable impurities. Furthermore, a large quantity of silver particles (Ag particles) is sometimes referred to as silver powder (Ag powder). The same applies to other particles.

[0162] The shape and size (also called particle diameter) of the conductive particles are not particularly limited. For example, spherical and flake-like shapes can be used. The particle size can be defined using the cumulative size of 50% of all particles (D50). In this specification, D50 is also referred to as the average particle size. It should be noted that the average particle size (D50) can be determined by measuring particle size distribution using the Microtrac method (laser diffraction scattering method) and based on the results of the particle size distribution measurement.

[0163] The average particle size (D50) of the conductive particles is preferably 0.5 to 2.5 μm, more preferably 0.8 to 2.2 μm. By keeping the average particle size (D50) of the conductive particles within a given range, the reactivity of the conductive paste to the passivation film 2 can be suppressed during the firing of the conductive paste. It should be noted that if the average particle size (D50) is greater than the above range, problems such as clogging may occur during screen printing.

[0164] Alternatively, the size of silver particles can be expressed as their BET specific surface area (also simply referred to as "specific surface area"). The preferred BET specific surface area of ​​silver particles is 0.1–1.5 m². 2 / g, more preferably 0.2 to 1.2m 2 / g. BET specific surface area can be measured, for example, using a fully automated specific surface area measuring device such as Macsoeb (manufactured by MOUNTEC).

[0165] <<(B) Organic Carrier>>

[0166] The conductive paste of this embodiment includes (B) an organic carrier.

[0167] As an organic carrier, it can contain organic binders and solvents. The organic binders and solvents serve functions such as adjusting the viscosity of the conductive paste, and there are no particular limitations. Alternatively, the organic binder can be dissolved in a solvent before use.

[0168] In the conductive paste of this embodiment, (B) the organic carrier preferably comprises at least one selected from ethyl cellulose, rosin ester, acrylic resin, and organic solvent. By including at least one selected from ethyl cellulose, rosin ester, acrylic resin, and organic solvent in the (B) organic carrier, the conductive paste can be screen printed appropriately, and the shape of the printed pattern can be made into a suitable shape.

[0169] As an organic binder, cellulose-based resins (e.g., ethyl cellulose, nitrocellulose, etc.) and (meth)acrylic resins (e.g., polymethyl acrylate, polymethyl methacrylate, etc.) can be selected. The organic carrier contained in the conductive paste of this embodiment preferably includes at least one selected from ethyl cellulose, rosin ester, butyral, acrylic resins, and organic solvents. The amount of organic binder added relative to 100 parts by weight of silver particles is typically 0.1 to 30 parts by weight, preferably 0.2 to 5 parts by weight.

[0170] As an organic solvent, one or more can be selected from alcohols (e.g., terpineol, α-terpineol, β-terpineol, etc.) and esters (e.g., hydroxyl-containing esters, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, diethylene glycol monobutyl ether acetate (butyl carbitol acetate), etc.). The amount of solvent added is typically 0.5 to 30 parts by weight relative to 100 parts by weight of silver particles, preferably 2 to 25 parts by weight. A specific example of an organic solvent is diethylene glycol monobutyl ether acetate (butyl carbitol acetate).

[0171] <<(C) Glass Material>>

[0172] The conductive paste of this embodiment includes (C) glass frit.

[0173] In the conductive paste of this embodiment, (C) the alkalinity of the glass frit B GF B is the product of (A) the content of conductive particles in the conductive paste (set to 100 parts by weight) and (C) the content of glass frit in the conductive paste (in parts by weight). GF The basicity B of the glass frit is in the range of 0.25 to 1.45, preferably in the range of 0.3 to 1.4, and more preferably in the range of 0.3 to 1.2. GF The product of B and the content G GF • G is within an appropriate range, which allows the glass frit to have appropriate reactivity to the passivation film 2 (anti-reflective film). Therefore, when manufacturing crystalline silicon using a laser processing process, the conductive paste of the embodiment can be preferably used.

[0174] The basicity of the glass powder can be calculated using the method described in Patent Document 3 (Japanese Patent Application Publication No. 2009-231826). Specifically, regarding "basicity," the basicity of the glass powder can be defined using the formula shown in "K. Morinaga, H. Yoshida And H. Takebe: J. AmCerm. Soc., 77, 3113 (1994)". Specifically, it is as follows.

[0175] Oxide M i O of M i The bonding force between -O ions, as the attraction Ai between cations and oxygen ions, is given by the following equation.

[0176] A i =Z i ·Z 02- / (r i +r 02- ) 2 =Zi·2 / (r) i +1.40) 2

[0177] Z i The valence of the cation is 2, and the oxygen ion is 2.

[0178] r i : Ionic radius of cation ( )

[0179] The ionic radius r of oxygen ions i It is 1.40 nm. The A in the above formula... i The reciprocal of B i (=1 / A) i Let M be a single-component oxide. i Oxygen supply capacity.

[0180] B i ≡1 / A i

[0181] If this B i Standardized as B CaO =1, B SiO2 =0, then give the B of each single-component oxide. i -Indicators. If the B of each component... i - By extending the index to multi-component systems using the percentage of cations, the basicity (=B) of a melt of glass oxide (glass frit) with any composition can be calculated. GF ).

[0182] B GF =Σn i ·B i

[0183] n i : Cation percentage

[0184] Alkalinity (B) specified like this GF As mentioned above, alkalinity indicates oxygen supply capacity; a higher value indicates easier oxygen supply and easier oxygen exchange with other metal oxides. In other words, "alkalinity" can represent the degree of dissolution in the glass melt.

[0185] Since the content G of glass frit (C) is a ratio relative to the content of conductive particles (A), it is a dimensionless number. Furthermore, as mentioned above, since B... i It is standardized as B CaO =1, B SiO2 =0, therefore (C) the alkalinity of the glass frit B GF (=Σn) i ·B i ( ) is a dimensionless number. Therefore, (C) the basicity of the glass material B GF The product of B and the content G GF G is also a dimensionless number.

[0186] The alkalinity (B) of the glass frit in this embodiment GF The preferred alkalinity is 0.10–1.5, more preferably 0.15–1.3, and even more preferably 0.20–1.1. At alkalinity (B... GF Within such a range, by adjusting the amount of glass frit added to the conductive paste, the reactivity of the glass frit to the passivation film 2 can be made appropriate.

[0187] The glass frit content G in the conductive paste of this embodiment is preferably 0.1 to 5.0 parts by weight relative to 100 parts by weight of conductive particles, more preferably 0.2 to 4.0 parts by weight, even more preferably 0.3 to 3.0 parts by weight, and particularly preferably 0.4 to 2.7 parts by weight. The glass frit content G in the conductive paste is related to the alkalinity (B). GF By appropriately adjusting the glass frit, the reactivity of the glass frit to the passivation film 2 can be made appropriate. More specifically, in order to prepare a conductive paste suitable for forming electrodes using laser processing, the glass frit content is reduced compared to the past, and the basicity of the glass frit is made to an appropriate range, thereby suppressing the reactivity to the passivation film 2 and increasing Voc.

[0188] The glass transition temperature (Tg) of the (C) glass frit in this embodiment is preferably 250–600°C, more preferably 270–500°C, and even more preferably 300–400°C. By setting the glass transition temperature (Tg) of the (C) glass frit to 250°C or higher, the reactivity to the passivation film 2 can be suppressed. In addition, by setting the glass transition temperature (Tg) to 600°C or lower, the contact resistance between the resulting electrode (e.g., the light incident side surface electrode 20) and the impurity diffusion layer 4 can be reduced.

[0189] The glass transition temperature (Tg) can be determined as follows. Using a differential calorimeter (MACScience Co., Ltd. TG-DTA2000S), the glass powder (as sample) and a reference material are set up. The temperature is increased from room temperature to 900°C at a rate of 10°C / min. A curve (DTA curve) is obtained by plotting the temperature difference between the glass powder and the reference material relative to the temperature. The first inflection point of the DTA curve obtained in this way can be defined as the glass transition temperature Tg.

[0190] The shape of the glass frit particles is not particularly limited; for example, spherical or amorphous shapes can be used. Furthermore, the particle size is not particularly limited. From a workability perspective, the average particle size (D50) is preferably in the range of 0.1 to 10 μm, more preferably in the range of 0.5 to 5 μm.

[0191] The glass frit contained in the conductive paste of this embodiment can be composed of different types of glass frit (first glass frit and second glass frit) independently.

[0192] First, let's explain the first glass material.

[0193] The first glass frit contained in the conductive paste of this embodiment preferably comprises one or more selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, BaO, CuO, Li2O, and ZnO. More preferably, the first glass frit contained in the conductive paste of this embodiment comprises one or more selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O, and ZnO. By including at least one of these oxides in the first glass frit, the basicity of the first glass frit can be adjusted to an appropriate range.

[0194] The first glass frit preferably contains Bi2O3. The content of Bi2O3 in the first glass frit (100 mol%) is preferably 10 to 80 mol%, more preferably 15 to 75 mol%, and even more preferably 20 to 70 mol%. By including Bi2O3 in the first glass frit, the contact resistance can be reduced while adjusting the reactivity to the passivation film 2 to an appropriate range.

[0195] The conductive paste of this embodiment contains, in mol% (C) Bi₂O₃ content (C) in the first glass frit. Bi2O3 The product of C and the content G of the first glass frit Bi2O3 • G is preferably in the range of 10 to 200, more preferably in the range of 13 to 170, and even more preferably in the range of 15 to 150. This is achieved by increasing the product C with the glass content G. Bi2O3 • G is the range mentioned above, which can reduce contact resistance while adjusting the reactivity of the passivation film to an appropriate range.

[0196] The first glass frit may contain SiO2 within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains SiO2, the SiO2 content in the first glass frit (100 mol%) is preferably 10 to 60 mol%, more preferably 15 to 40 mol%. By including an appropriate amount of SiO2 in the first glass frit, the reactivity with the passivation film 2 can be controlled.

[0197] The first glass frit may contain B2O3 within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains B2O3, the content of B2O3 in the first glass frit (100 mol%) is preferably 3 to 60 mol%, more preferably 4 to 50 mol%. By including an appropriate amount of B2O3 in the first glass frit, the reactivity with the passivation film 2 can be controlled.

[0198] The first glass frit may contain V2O5 within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains V2O5, the V2O5 content in the first glass frit (100 mol%) is preferably less than 8 mol%, more preferably less than 5 mol%. By including V2O5 in the first glass frit, the basicity of the first glass frit can be reduced. Therefore, when the basicity of the first glass frit is high, by including an appropriate amount of V2O5, the basicity of the first glass frit can be adjusted to an appropriate range.

[0199] The first glass frit may contain TeO2 within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains TeO2, the TeO2 content in the first glass frit (100 mol%) is preferably less than 80 mol%, more preferably less than 50 mol%. By including TeO2 in the first glass frit, the basicity of the first glass frit can be reduced. Therefore, when the basicity of the first glass frit is high, by including an appropriate amount of TeO2, the basicity of the first glass frit can be adjusted to an appropriate range.

[0200] The first glass frit may contain BaO within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains BaO, the BaO content in the first glass frit (100 mol%) is preferably 3 to 20 mol%, more preferably 5 to 10 mol%. By including an appropriate amount of BaO in the first glass frit, the reactivity to the passivation film 2 can be adjusted to an appropriate range.

[0201] The first glass frit may contain CuO within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains CuO, the CuO content in the first glass frit (100 mol%) is preferably 10 to 40 mol%, more preferably 20 to 30 mol%. By including an appropriate amount of CuO in the first glass frit, the reactivity to the passivation film 2 can be adjusted to an appropriate range.

[0202] The first glass frit may contain Li2O within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains Li2O, the content of Li2O in the first glass frit (100 mol%) is preferably 3 to 40 mol%, more preferably 5 to 30 mol%. By including an appropriate amount of Li2O in the first glass frit, the reactivity to the passivation film 2 can be adjusted to an appropriate range.

[0203] The first glass frit may contain ZnO within a range that does not adversely affect the conductive paste of this embodiment. When the first glass frit contains ZnO, the ZnO content in the first glass frit (100 mol%) is preferably 5 to 70 mol%, more preferably 15 to 60 mol%. By including ZnO in the first glass frit, the basicity of the first glass frit can be adjusted to an appropriate range.

[0204] The first glass frit contained in the conductive paste of this embodiment is preferably lead-free glass frit. In this case, the first glass frit contained in the conductive paste of this embodiment does not substantially contain lead (Pb). However, the lead-free first glass frit used in this embodiment may contain trace amounts of lead as an impurity, which is unavoidable. Specifically, the lead-free first glass frit used in this embodiment may contain less than 0.1% by weight of lead as an impurity. By manufacturing solar cells using a conductive paste containing lead-free first glass frit, lead pollution to the environment can be prevented when discarding solar cells.

[0205] The second glass material will now be described. The second glass material is a glass material containing PbO.

[0206] The second glass frit contained in the conductive paste of this embodiment preferably comprises one or more selected from PbO, SiO2, Al2O3, B2O3, ZnO, V2O5, WO3, and Nb2O3. More preferably, the second glass frit contained in the conductive paste of this embodiment comprises PbO, SiO2, Al2O3, B2O3, and ZnO.

[0207] In the conductive paste of this embodiment, the second glass frit preferably contains at least one selected from ZnO, V2O5, WO3, and Nb2O3. By including at least one of these oxides in the second glass frit, the basicity of the second glass frit can be adjusted to an appropriate range.

[0208] The second glass frit preferably contains PbO. The PbO content in the second glass frit (100 mol%) is preferably 25 to 60 mol%, more preferably 30 to 55 mol%, and even more preferably 40 to 55 mol%. By including PbO in the second glass frit, the contact resistance can be reduced while suppressing the reactivity to the passivation film 2.

[0209] The second glass frit preferably contains SiO2. The SiO2 content in the second glass frit (100 mol%) is preferably 20 to 65 mol%, more preferably 25 to 60 mol%. By including SiO2 in the second glass frit, the reactivity to the passivation film 2 can be suppressed.

[0210] The second glass frit preferably contains Al2O3. The content of Al2O3 in the second glass frit (100 mol%) is preferably 3.0 to 6.8 mol%, more preferably 3.5 to 6 mol%. By including Al2O3 in the second glass frit, the reactivity to the passivation film 2 can be suppressed.

[0211] The second glass frit preferably contains B2O3. The B2O3 content in the second glass frit (100 mol%) is preferably 3.0–15 mol%, more preferably 3.5–12 mol%.

[0212] The second glass frit preferably contains ZnO. The ZnO content in the second glass frit (100 mol%) is preferably 5 to 20 mol%, more preferably 8 to 15 mol%. By including ZnO in the second glass frit, the basicity of the second glass frit can be adjusted to an appropriate range.

[0213] In this embodiment, the conductive paste preferably contains C, expressed in mol% of PbO in the second glass frit. PbO The product C with the content G of the second glass frit PbO G is in the range of 20 to 139, more preferably in the range of 22 to 130, and even more preferably in the range of 26 to 105. In the product C... PbO When G is greater than 139, the reactivity of the second glass frit with the passivation film 2 is too high. Additionally, in the case of accumulated C... PbO When G is less than 20, the contact resistance between the obtained electrode and the impurity diffusion layer 4 is too high.

[0214] In the first and second glass frits, the glass frit particles can be a single type of particle containing a given amount of each of the required multiple oxides. Alternatively, particles composed of a single oxide can be used as particles that differ for each of the required multiple oxides. Furthermore, multiple particles with different compositions of the required multiple oxides can be used in combination. To synergistically obtain the effects of different types of oxides, the particles of the first and second glass frits are preferably a single type of particle containing a given amount of each of the required multiple oxides.

[0215] <Other Ingredients>

[0216] The conductive paste of this embodiment may include additives and additives other than those mentioned above, within a range that does not adversely affect the solar cell characteristics of the resulting solar cell.

[0217] In the conductive paste of this embodiment, as an additive, substances selected from plasticizers, defoamers, dispersants, leveling agents, stabilizers, and adhesion promoters may be further incorporated as needed. Among these, at least one plasticizer selected from phthalates, glycolates, phosphate esters, sebacic acid esters, adipates, and citrate esters may be used.

[0218] The conductive paste of this embodiment may include additives other than those described above within a range that does not adversely affect the characteristics of the resulting solar cell. For example, the conductive paste of this embodiment may further include at least one additive selected from titanium resin, titanium oxide, cobalt oxide, cerium oxide, silicon nitride, copper manganese tin, aluminosilicate, and aluminum silicate. By including these additives, the adhesion strength of the electrode to the passivation film 2 can be improved. These additives may be in the form of particles (additive particles). The amount of additive added relative to 100 parts by weight of silver particles is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 2 parts by weight. To obtain higher adhesion strength, the additive is preferably copper manganese tin, aluminosilicate, or aluminum silicate. The additive may include both aluminosilicate and aluminum silicate.

[0219] <Method for manufacturing conductive paste>

[0220] The method for manufacturing the conductive paste according to this embodiment will now be described. The conductive paste according to this embodiment can be manufactured by adding silver particles, glass frit, and other additives and / or additives as needed to an organic binder and solvent, and then mixing and dispersing them.

[0221] Mixing can be performed, for example, using a planetary mixer. Dispersion can be performed using a three-roll mill. Mixing and dispersion are not limited to these methods; various known methods can be used.

[0222] Example

[0223] The following examples will be used to specifically describe this embodiment; however, the present invention is not limited to these examples.

[0224] <Solar cells of Examples 1-7 and Comparative Examples 1 and 2>

[0225] In the examples and comparative examples, monocrystalline silicon solar cells were fabricated, and the electrical characteristics of the monocrystalline silicon solar cells were measured, thereby evaluating the performance of the solar cells in the examples and comparative examples.

[0226] <<Materials and Preparation Ratios of Conductive Paste>>

[0227] Tables 1 and 2 show the proportions of (A) conductive particles and (C) glass frit in the conductive pastes of the Examples and Comparative Examples. The proportions shown in Tables 1 and 2, as well as the proportions of each component below, are expressed as parts by weight of each component when (A) conductive particles are set to 100 parts by weight. The components contained in the conductive paste are shown below.

[0228] (A) Silver particles

[0229] Table 3 shows the type, manufacturer, shape, average particle size (D50), TAP density, and BET specific surface area of ​​the silver particles A1 and A2 used in the conductive pastes of the examples and comparative examples. Tables 1 and 2 show the proportions of silver particles A1 and A2 in the conductive pastes of the examples and comparative examples. It should be noted that the average particle size (D50) was determined by measuring the particle size distribution using the Microtrac method (laser diffraction scattering method) and obtaining the median diameter (D50) based on the particle size distribution measurement results. The same applies to the average particle size (D50) of other components. Furthermore, the BET specific surface area was measured using a fully automated specific surface area measuring device, Macsoeb (manufactured by MOUNTEC). Regarding the BET specific surface area, it was measured using the BET 1-point method based on nitrogen adsorption after pre-drying at 100°C and passing nitrogen gas through it for 10 minutes.

[0230] (B) Organic carrier

[0231] Organic carriers and solvents are used. As the organic binder, 0.4 parts by weight of ethyl cellulose with an ethoxylated content of 48–49.5% by weight is used. As the solvent, 3 parts by weight of diethylene glycol monobutyl ether acetate (butyl carbitol acetate) is used.

[0232] (C) Glass material

[0233] Table 4 shows the composition, basicity, and glass transition temperature of the glass frits GF1 to GF6 used in the conductive pastes of the examples and comparative examples. It should be noted that the average particle size (D50) of the glass frits GF1 to GF6 is set to 2 μm. Tables 1 and 2 show the type and content (parts by weight) of the (C) glass frits in the conductive pastes of the examples and comparative examples.

[0234] The glass transition temperatures (DTAs) of glass frits GF1 to GF6 were determined. Table 4 shows the measured DTA values ​​for glass frits GF1 to GF6. The determination of the glass transition temperatures of the glass frits was performed as follows: Approximately 50 mg of glass frits GF1 to GF6 were added as samples to a platinum bath, and alumina powder was used as a standard sample. Under atmospheric conditions, a differential thermal analysis (DTA) apparatus (RIGAKU Corporation, TG-8120) was used to heat the glass frits from room temperature to 800°C at a heating rate of 20°C / min to obtain the DTA curve. The first endothermic start point (extrapolation point) of the DTA curve was set as the glass transition temperature.

[0235] Glass frits GF1 to GF6 are manufactured as follows: First, powdered oxides used as raw materials are measured, mixed, and added to a crucible. The crucible is placed in a heated oven, and the contents are heated to the melt temperature. The raw materials are maintained at the melt temperature until fully melted. Then, the crucible is removed from the oven, and the molten contents are stirred evenly. Next, the contents of the crucible are rapidly cooled at room temperature using a stainless steel double roller to obtain plate-shaped glass. Finally, the plate-shaped glass is pulverized and evenly dispersed in a mortar, and sieved using a mesh sieve to obtain glass frit with the desired particle size. Glass frit that passes through a 100-mesh sieve but remains on a 200-mesh sieve is sieved, resulting in a glass frit with an average particle size (D50) of 149 μm. This glass frit is further pulverized to obtain a glass frit with an average particle size (D50) of 2 μm.

[0236] Then, the above-mentioned types and proportions of (A) conductive particles, (B) organic carrier and (C) glass frit are mixed using a planetary mixer and further dispersed using a three-roll mill to paste them, thereby producing the conductive pastes of the Examples and Comparative Examples.

[0237] <<Manufacturing of Monocrystalline Silicon Solar Cells>>

[0238] Manufacturing such as Figure 4 The example shown is a bifacial light-receiving monocrystalline silicon solar cell. The substrate used is a phosphorus-doped n-type monocrystalline silicon substrate (substrate thickness 200 μm).

[0239] First, after forming a silicon oxide layer of approximately 20 μm on the substrate using dry oxidation, etching is performed using a solution containing hydrogen fluoride, pure water, and ammonium fluoride to remove damage to the substrate surface. Furthermore, heavy metals are removed using an aqueous solution containing hydrochloric acid and hydrogen peroxide.

[0240] Then, a texture (convex-concave shape) is formed on both sides of the substrate using wet etching. Specifically, a pyramid-shaped texture structure is formed on both sides (the main light-incident side surface and the back side) using wet etching (sodium hydroxide aqueous solution). Subsequently, it is cleaned with an aqueous solution containing hydrochloric acid and hydrogen peroxide.

[0241] Then, boron is implanted into one surface (the light incident side surface) of the substrate with the textured structure to form a p-type diffusion layer to a depth of about 0.5 μm. The sheet resistance of the p-type diffusion layer is 150 Ω / □.

[0242] In addition, phosphorus was implanted into another textured surface (back side) of the aforementioned substrate to form an n-type diffusion layer to a depth of approximately 0.5 μm. The sheet resistance of the n-type diffusion layer was 20 Ω / □. Boron and phosphorus were implanted simultaneously using a thermal diffusion method.

[0243] Then, passivation films 2 are formed on the surface of the substrate with the p-type diffusion layer (light incident side surface) and the surface of the substrate with the n-type diffusion layer (back side). Specifically, firstly, after forming a thin oxide film layer of 1-2 nm on the light incident side surface and the back side, a silicon nitride film with a thickness of about 60 nm is formed using plasma CVD with silane gas and ammonia gas. Specifically, glow discharge decomposition is performed on a mixed gas of NH3 / SiH4 = 0.5 at 1 Torr (133 Pa), thereby forming a silicon nitride film (anti-reflective film) with a thickness of about 70 nm using plasma CVD.

[0244] The conductive paste used for electrode formation on the surface (light incident side surface) of the substrate on which the p-type diffusion layer is formed in the monocrystalline silicon solar cells of the embodiments and comparative examples uses the conductive paste in the amounts shown in Tables 1 and 2.

[0245] The conductive paste was printed using screen printing. On the passivation film 2 of the substrate described above, a pattern consisting of a 1.5 mm wide light-incident side main gate electrode 20a and a 60 μm wide light-incident side sub-gate electrode 20b was printed to a thickness of approximately 20 μm. After that, it was dried at 150°C for about 1 minute.

[0246] As the back electrode 15 (the electrode on the surface where the n-type diffusion layer is formed), the same Ag paste was printed using screen printing. It should be noted that the electrode pattern of the back electrode 15 is the same as that of the light-incident side surface electrode 20. It was then dried at 150°C for approximately 60 seconds. The thickness of the conductive paste used on the dried back electrode 15b was approximately 20 μm. Subsequently, it was simultaneously fired on both sides using a belt furnace (firing furnace) CDF7210 manufactured by Despatch Industries, Inc., at a peak temperature of 720°C and a furnace in-and-out time of 50 seconds. A monocrystalline silicon solar cell was fabricated as shown above.

[0247] <<Laser Processing Technology>>

[0248] The light-incident surface of the monocrystalline silicon solar cells in the above embodiments and comparative examples is subjected to a laser processing process to form the AgSi region 30. That is, while applying a negative voltage to the back electrode 15, the light-incident surface of the solar cells is processed using a laser. Figure 2 A positive voltage is applied to the light-incident surface electrode 20 of the pattern shown, causing a current flowing in the opposite direction between the p-type impurity diffusion layer 4 and the n-type crystalline silicon substrate 1 of the solar cell, while irradiating the light-incident surface of the solar cell with laser light. The applied voltage during the laser processing is 20V, and the intensity of the irradiated laser is 100W / cm². 2 The voltage application and laser irradiation time were set to 2 seconds.

[0249] The solar cells of the embodiments and comparative examples were fabricated as shown above.

[0250] <Determination of the electrical properties of solar cells after laser processing>

[0251] The electrical characteristics of the monocrystalline silicon solar cells after laser processing were measured as follows. Specifically, the current-voltage characteristics of the prototype solar cells were measured using a solar simulator SS-150XIL manufactured by Eiko Seiki Co., Ltd., under simulated sunlight conditions of 25°C and AM 1.5 (energy density 100 mW / cm²). 2 The measurements were performed under laser irradiation, and the fill factor (FF), open circuit voltage (Voc), and conversion efficiency (%) were calculated based on the results. It should be noted that two monocrystalline silicon solar cells manufactured under identical conditions were fabricated, and the average value of the two was used to calculate the measured values. The electrical characteristics (fill factor (FF), open circuit voltage (Voc), and conversion efficiency (%)) of the solar cells after laser treatment were measured. The measurement results are shown in Tables 1 and 2.

[0252] As can be clearly seen from Table 1, the solar cells of Examples 1-7, fabricated using the given conductive paste, exhibit high electrical characteristics after laser processing, for example, a conversion efficiency ranging from 21.3% to 24.4%. In contrast, the solar cells fabricated using the conductive paste of Comparative Example 1 exhibit low electrical characteristics after laser processing, for example, a conversion efficiency ranging from 7.3% to 20.2%. Therefore, it is evident that the solar cells of Examples 1-7 of this embodiment, having the given AgSi region 30, exhibit superior electrical characteristics after laser processing compared to the solar cells of Comparative Examples 1 and 2.

[0253] <SEM Photos>

[0254] The cross-section near the passivation film 2 (anti-reflective film) of the solar cells of the embodiments and comparative examples was observed using a scanning electron microscope (SEM). Figure 6 and 7 This is a cross-sectional SEM image of the solar cell from Example 3. Additionally, Figure 8 This is a cross-sectional SEM image of the solar cell in Comparative Example 1.

[0255] When a laser processing technique is used, a passivation film 2 (anti-reflection film) exists in most of the area between the light-incident surface electrode 20 and the impurity diffusion layer 4. In the laser processing technique, a given voltage is applied such that a current flows through the pn junction in the opposite direction to the forward direction, and light from a point source (e.g., a laser) is irradiated. This causes a current to flow through a small region between the light-incident surface electrode 20 and the impurity diffusion layer 4, resulting in localized heating. As a result, as... Figure 6 and 7 As shown, an AgSi region 30 (an alloy of silver and silicon) is formed between the light-incident side surface electrode 20 and the impurity diffusion layer 4 as a locally electrically conductive portion (locally conductive portion). That is, the locally conductive portion contains an alloy of silver and silicon. In addition, in the locally conductive portion, the impurity diffusion layer 4 (the silicon emitter layer of the second conductivity type) is in direct contact with the light-incident side surface electrode 20 without being separated by the passivation film 2 (anti-reflection film). By utilizing this locally formed electrically conductive portion (locally conductive portion), good electrical conductivity between the light-incident side surface electrode 20 and the impurity diffusion layer 4 can be achieved. The given conductive paste used to manufacture the solar cell of this embodiment has low reactivity with the passivation film 2 (anti-reflection film) and has reactivity with the passivation film 2 (anti-reflection film) suitable for laser processing. Therefore, the conductive paste of this embodiment can be preferably used for forming the light-incident side surface electrode 20 of a crystalline silicon solar cell using a laser processing process.

[0256] <Depth d of AgSi region 30>

[0257] The depth d of the AgSi region 30 in Examples 1-7 and Comparative Examples 1 and 2 was measured as shown below. The measurement results are shown in Tables 1 and 2.

[0258] Figure 6 The depth d of the AgSi region 30 is illustrated in the figure. The depth d of the AgSi region 30 is determined as follows: in an SEM image obtained by observing the cross-section of the AgSi region 30, any one point (d) is taken as the interface between the electrode and the AgSi region 30. Figure 6 Any point from B1 to the interface between the substrate and the AgSi region 30 ( Figure 6 The length of the line segment with the longest length (B2) is ( Figure 6 The length d) of the line segment connecting B1 and B2 was measured. The cross-section of the completed solar cell, including the passivation film 2 and the AgSi region 30, was observed using SEM at a magnification of 20,000 times, thereby obtaining... Figure 6 The SEM image shown.

[0259] <Residual rate of passivation film 2>

[0260] The retention rates of passivation film 2 in Examples 1-7 and Comparative Examples 1 and 2 were measured as shown below. The measurement results are presented in Tables 1 and 2.

[0261] Specifically, firstly, the cross-section of the completed solar cell, including the passivation film 2 and the AgSi region 30, was observed using SEM at a magnification of 20,000x, resulting in an SEM image (SEM image range: 5.7 μm × 3.9 μm). It should be noted that the transverse (horizontal direction) length of this SEM image is 5.7 μm, and the longitudinal (perpendicular direction) length is 3.9 μm. Then, as... Figure 7 As illustrated, the total length Lp of the cross-section of the passivation film 2 in the SEM image was measured. Figure 7 In the example shown, the total length Lp of the cross-section of the passivation film 2 in the SEM image is the sum of the lengths of Lp1, Lp2, Lp3, and Lp4. Then, in this SEM image, the total length Le of the cross-section of the interface between the AgSi region 30 and the electrode in the portion where the AgSi region 30 is formed is measured. Length Le corresponds to the length by which the passivation film 2 disappears during the solar cell manufacturing process. Figure 7 In the example shown, the total length Le of the cross-section of the interface between the AgSi region 30 and the electrode in the portion where the passivation film 2 disappears is the total length of Le1 and Le2. The retention rate of the passivation film 2 can be obtained as Lp / (Lp+Le). It should be noted that the lengths Lp1, etc., are determined by approximating the passivation film 2 as a straight line.

[0262] <Thickness and thickness ratio of passivation film 2 before and after firing>

[0263] The thickness Da of the passivation film 2 before firing and the thickness Db of the completed solar cells of Examples 1-7 and Comparative Examples 1 and 2 were measured. The measurement results are shown in Tables 1 and 2. Tables 1 and 2 show the film thickness ratio of the passivation film 2 before and after firing.

[0264] The thickness Da of the passivation film 2 before firing was determined by SEM observation of the cross-section of the passivation film 2 immediately after its formation. That is, the passivation film 2 was formed on the surface of a given crystalline silicon substrate 1 under the same conditions as in the examples and comparative examples, and the cross-section of the passivation film 2 was observed by SEM to obtain the thickness Da of the passivation film 2 before firing in the examples and comparative examples.

[0265] The final film thickness Db of the solar cell refers to the passivation film 2 of the completed solar cell after electrodes are formed on its surface and a given laser processing technology is applied. Specifically, firstly, a cross-section of the completed solar cell, including the passivation film 2 and the AgSi region 30, is observed using SEM at a magnification of 20,000, resulting in an SEM image (SEM image range: 5.7 μm × 3.9 μm). Then, the SEM image is divided into 6 equal parts along its longitudinal direction, and the film thickness of the passivation film 2 at the 5 junctions of the 6-part image is measured (5 locations). The final film thickness Db of the solar cell is set as the average of the 5 film thicknesses of the passivation film 2.

[0266] The so-called film thickness ratio before and after firing of passivation film 2 is the ratio of the film thickness Da of passivation film 2 before firing to the film thickness Db of solar cell after completion (Db / Da), as measured as above.

[0267] <Evaluation>

[0268] As shown in Tables 1 and 2, in the solar cells of Examples 1 to 7, the depth d of the AgSi region 30, determined from the cross-sectional SEM images, ranges from 200 to 1800 nm. Furthermore, it can be confirmed that the given AgSi region 30 is formed in the solar cells of Examples 1 to 7. Additionally, the film thickness ratio of the passivation film 2 before and after firing in the solar cells of Examples 1 to 7 ranges from 17% to 78%, and the retention rate of the passivation film 2 ranges from 10% to 90%. Therefore, it can be confirmed that the given passivation film 2 also remains after the manufacturing of the solar cells of Examples 1 to 7, which are manufactured by performing the given firing and laser processing processes. As a result, the solar cells of Examples 1 to 7, manufactured using a conductive paste containing glass frits of GF1 to 3, GF5, and GF6, exhibit high electrical characteristics after the laser processing process, for example, a conversion efficiency ranging from 21.3% to 24.4%. Furthermore, in the solar cells of Examples 1-7, due to the presence of a passivation film 2 with a given passivation function, the open-circuit voltage (Voc) is high, ranging from 0.69 to 0.72 V. It should be noted that the fill factor (FF) of the solar cells of Examples 1-7 is in the range of 72.7% to 82.6%, which is a desirable value.

[0269] It should be noted that the residual rate of the passivation film 2 in the solar cells of Examples 1-5 ranges from 76% to 88%, and the conversion efficiency ranges from 23.4% to 24.4%. That is, the conversion efficiency of the solar cells of Examples 1-5 is higher than that of the solar cell of Example 6 (with a residual rate of 10% for the passivation film 2) and the solar cell of Example 7 (with a residual rate of 90% for the passivation film 2). Therefore, it can be said that a solar cell with a higher conversion efficiency can be obtained when the residual rate of the passivation film 2 is 30% or more and less than 90%.

[0270] Furthermore, the passivation film 2 of the solar cells in Examples 1-5 has a film thickness ratio of 36% to 51% before and after firing, and a conversion efficiency of 23.4% to 24.4%. That is, the conversion efficiency of the solar cells in Examples 1-5 is higher than that of the solar cell in Example 6 (film thickness ratio of 78%) and the solar cell in Example 7 (film thickness ratio of 17%). Therefore, it can be said that a solar cell with a higher conversion efficiency can be obtained when the film thickness ratio of the passivation film 2 before and after firing is 20% to 70%.

[0271] On the other hand, as shown in Table 2, in the solar cell of Comparative Example 1, the AgSi region 30 was not observed in the cross-sectional SEM image. Furthermore, the passivation film 2 of the solar cell of Comparative Example 1 had a film thickness ratio of 91% before and after firing, and the retention rate of the passivation film 2 was 100%. Therefore, in the solar cell of Comparative Example 1 manufactured by performing the given firing and laser processing process, it can be confirmed that the given passivation film 2 remains essentially unchanged after its formation, and no AgSi region is formed. Thus, the electrical characteristics of the solar cell made using a conductive paste containing GF4 glass frit after the laser processing process are low, for example, the conversion efficiency is 7.3%. In particular, in the solar cell of Comparative Example 1, since the passivation film 2, which serves as an insulating film, remains, the fill factor (FF) is as low as 35.7%.

[0272] In the solar cell of Comparative Example 2, an AgSi region 30 was observed in the cross-sectional SEM image. As shown in Table 2, the depth d of the AgSi region 30 in the solar cell of Comparative Example 2, determined from the cross-sectional SEM image, is 1200 nm. It should be noted that the thickness ratio of the passivation film 2 before and after firing in the solar cell of Comparative Example 2 is 5%, and the retention rate of the passivation film 2 is 5%. Therefore, it is evident that the solar cell of Comparative Example 2, manufactured by performing the given firing and laser processing process, has less passivation film 2 compared to the solar cells of Examples 1-7. As a result, the conversion efficiency of the solar cell of Comparative Example 2, made using a conductive paste containing GF3 glass frit after laser processing, is 20.2%, lower than that of the solar cells of Examples 1-7. Furthermore, in the solar cell of Comparative Example 2, due to the reduced presence of passivation film 2, the passivation function is lower, resulting in a low open-circuit voltage (Voc) of 0.64 V. It can be assumed that in the solar cell of Comparative Example 2, the passivation film 2 was burned through when the electrode formed using a conductive paste containing GF3 glass frit was fired.

[0273] In addition, since the solar cells of Examples 1, 2 and 4 to 7 are made using a conductive paste containing lead-free glass frit (GF1 to 5 glass frit), lead pollution to the environment can be prevented when the solar cells are discarded.

[0274]

[0275]

[0276]

[0277]

[0278] Explanation of reference numerals in the attached figures

[0279] 1 Crystalline silicon substrate, 2 Passivation film, 4 Impurity diffusion layer, 6 Substrate body, 14 Back passivation film, 15 Back electrode, 15a Back TAB electrode (back main gate electrode), 15b Back full electrode, 15c Back sub-gate electrode, 16 Second impurity diffusion layer, 20 Light incident side surface electrode (surface electrode), 20a Light incident side main gate electrode, 20b Light incident side sub-gate electrode, 30 AgSi region.

Claims

1. A solar cell comprising: A substrate comprising crystalline silicon and having an impurity diffusion layer on at least one surface; A passivation film disposed on at least a portion of the impurity diffusion layer of the substrate; and An electrode comprising silver (Ag) and disposed on at least a portion of the passivation film. The solar cell further includes at least one AgSi region disposed at least a portion between the electrode and the substrate. The AgSi region includes at least one AgSi region with a depth of more than 100 nm. In a scanning electron microscope image of a 5.7 μm × 3.9 μm cross-section of the solar cell containing the AgSi region, the proportion of the length of the passivation film remaining, i.e., the passivation film retention rate, is 10% to 90%. The substrate containing crystalline silicon is a crystalline silicon substrate of the first conductivity type. The impurity diffusion layer is a second conductivity type impurity diffusion layer. The electrode is a light incident side surface electrode disposed on the light incident side surface. The solar cell further includes a back electrode configured to be electrically connected to a surface of the crystalline silicon substrate opposite to the light-incident surface. The light-incident side surface electrode is a light-incident side surface electrode that has been treated such that, while applying a voltage between the back electrode and the light-incident side surface electrode to allow a current to flow in the opposite direction between the impurity diffusion layer of the second conductivity type and the crystalline silicon substrate of the first conductivity type, light from a point source is irradiated onto the light-incident side surface of the solar cell.

2. The solar cell according to claim 1, wherein, The ratio of the passivation film thickness Da immediately after its formation to the passivation film thickness Db in a scanning electron microscope image of a 5.7 μm × 3.9 μm cross-section of the solar cell containing the AgSi region, formed by forming the electrode on the surface of the solar cell, is 15% to 85%.

3. The solar cell according to claim 1 or 2, wherein, The electrode further comprises 0.1 to 5.0 parts by weight of glass frit relative to 100 parts by weight of the silver (Ag) contained in the electrode.

4. The solar cell according to claim 3, wherein, The glass transition temperature of the glass material is 250℃~600℃.

5. The solar cell according to claim 3, wherein, The glass material comprises at least one selected from SiO2, B2O3, V2O5, Bi2O3, TeO2, Li2O and ZnO.

6. The solar cell according to claim 3, wherein, The glass material does not actually contain PbO.

7. The solar cell according to claim 1 or 2, wherein, The electrode does not actually contain lead (Pb).

8. The solar cell according to claim 1 or 2, wherein, The electrode does not actually contain aluminum particles.

Citation Information

Patent Citations

  • Conductive composition, solar cell using the same, manufacturing method thereof, and solar cell module formed using the solar cell

    JP2009231826A

  • Solar cell and method of manufacturing the same

    JP2011086754A

  • Method for improving ohmic contact behavior between contact grid and emitter layer of silicon solar cells

    JP2021513218A

  • Special Ag paste for grid line electrode at front surface of crystalline silicon solar battery

    CN102157220A