Preparation method and application of high-hiding power pigment red P.R170

By using a combination of EDTA, other additives, ultrasonic treatment, and magnetic field treatment at low temperatures, the problem of insufficient hiding power of Pigment Red P.R170 was solved, and Pigment Red P.R170 with high hiding power, tinting strength, and weather resistance was prepared, reducing production costs and energy consumption.

CN120173429BActive Publication Date: 2026-11-20NINGXIA CAIYAN TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510262921.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-06
Publication Date
2026-11-20
Estimated Expiration
2045-03-06

AI Technical Summary

Technical Problem

The existing pigment red P.R170 has insufficient hiding power, which requires multiple coatings, increases production costs and affects the uniformity and appearance quality of the coating. At the same time, the traditional synthesis process is energy-intensive and the product has poor stability and weather resistance.

Method used

By using a combination of EDTA, other additives, ultrasonic treatment, and magnetic field treatment under low-temperature conditions, naphthol AS-PH was completely dissolved, avoiding hydrolysis. Combined with nonionic surfactants and low-temperature coupling reaction, the reaction conditions were optimized to prepare high-coverage pigment red P.R170.

Benefits of technology

It significantly improves the hiding power and tinting strength of Pigment Red P.R170, enhances weather resistance, reduces preparation costs and energy consumption, is suitable for continuous large-scale production, and reduces waste gas and wastewater emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005300383110000091
    Figure BDA0005300383110000091
Patent Text Reader

Abstract

The application discloses a preparation method of high-hiding-power pigment red P.R170 and application thereof, relates to the technical field of organic pigments, and comprises the following steps: step S1, preparation of a diazonium component; step S2, low-temperature preparation of a coupling component; step S3, a coupling reaction; and step S4, pigmentization treatment. The preparation method of the high-hiding-power pigment red P.R170 is characterized by optimizing a process and preparing the coupling component under low-temperature conditions, so that the prepared high-hiding-power pigment red P.R170 has high hiding power and tinting strength and excellent weather resistance, and can be widely applied in the fields of coatings, inks, plastics and rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organic pigment technology, and in particular to a method for preparing a high-coverage pigment red P.R170 and its application. Background Technology

[0002] Organic pigments possess advantages such as vibrant colors, high tinting strength, a wide range of color spectra, and low toxicity, and are currently widely used in coatings, printing inks, plastics, and rubber. However, most organic pigments on the market suffer from drawbacks such as low lightfastness, poor heat resistance, and poor weather resistance. Pigment Red P.R170 is an important high-performance pigment, holding a crucial position in high-end industrial coatings and automotive painting due to its excellent lightfastness, heat resistance, and solvent resistance.

[0003] Traditional Pigment Red P.R170 has some limitations in practical applications, the most prominent being insufficient hiding power. Hiding power is a crucial performance indicator for pigments, directly affecting their coverage on the substrate and overall cost. Insufficient hiding power necessitates multiple coats to achieve the desired coverage, increasing production costs and reducing efficiency. Furthermore, insufficient hiding power also affects coating uniformity and appearance quality, particularly noticeable on dark substrates.

[0004] The preparation of Pigment Red P.R170 typically uses the diazo component DB-70 and the coupling component naphthol AS-PH as raw materials. Naphthol AS-PH is a non-water-soluble substance and must be dissolved to effectively participate in chemical reactions. Currently, the widely used synthesis process for Pigment Red P.R170 both domestically and internationally involves dissolving naphthol AS-PH in a high-temperature (around 85℃) alkaline medium. Under these conditions, the hydroxyl groups (-OH) on the naphthol AS-PH molecule form water-soluble sodium hydroxide (-ONa), which disperses in an aqueous system and undergoes a coupling reaction. However, naphthol AS-PH is formed by the condensation of 2-hydroxy-3-naphthyl carboxylic acid and ethoxynaphthylamine, linked by an amide group. Under high-temperature and alkaline conditions, while naphthol AS-PH dissolves, the amide group on its molecular structure hydrolyzes to generate ethoxyaniline and 2-hydroxy-3-naphthyl carboxylic acid. This results in poor quality Pigment Red P.R170 produced using this synthesis process, with its stability, weather resistance, and hiding power requiring further improvement. In addition, this synthesis process also suffers from the drawback of high energy consumption for utilities.

[0005] For example, Chinese invention patent CN106046844B discloses a production method for an environmentally friendly organic pigment, Red 170, including the following steps: 1. Add water, hydrochloric acid, acetic acid, and p-aminobenzamide to a diazotization tank and dissolve them at room temperature; 2. Cool the diazotization tank by blowing ice and add sodium nitrite for diazotization to obtain a diazo liquid; 3. Add water, liquid alkali, ethanol, naphthol AS-PH, and naphthol AS-OL to a chemical tank in sequence and heat to 80°C to obtain a coupling solution; 4. Add ice water and emulsifier OP-10 to the coupling tank, and put the diazo liquid into the coupling tank; 5. Add dicumyl peroxide, triethanolamine oleate, titanium dioxide, and ethanol, and heat to a certain temperature, then wash with water, filter, and dry; The organic pigment Red 170 produced by this invention does not use aromatic amines prohibited by the EU REACH regulation as intermediates for synthesizing organic pigments, has sufficient raw material supply, has the advantage of low cost, and reduces the emission of waste. However, naphthol AS-PH is easily hydrolyzed in alkaline solution at 80°C, resulting in poor product quality and insufficient covering power; moreover, this production method consumes a lot of energy for utilities, which is not conducive to energy conservation and emission reduction.

[0006] It is evident that developing a preparation method and application of Pigment Red P.R170 with excellent hiding power, tinting strength and weather resistance meets market demand, has broad market and social value, and is of great significance to promoting the development of the field of high hiding power organic pigments. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art by providing a method for preparing a high-coverage pigment red P.R170 and its application. This method not only improves the applicability of the pigment itself, but also greatly reduces the preparation cost and energy consumption, resulting in significant economic and social benefits. The pigment red P.R170 prepared by this method has high covering power and tinting strength, and excellent weather resistance.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is: a method for preparing a high-coverage pigment red P.R170, comprising the following steps:

[0009] Step S1, Preparation of diazo component: Add water, p-aminobenzamide and hydrochloric acid to the diazotization kettle in sequence, stir until completely dissolved and clear, add ice to cool to 0-5℃, add sodium nitrite to carry out diazotization reaction, after the reaction is completed, add aqueous solution of aminosulfonic acid or aqueous solution of urea dropwise until starch-potassium iodide test paper no longer shows color, and obtain diazo component solution;

[0010] Step S2, preparation of coupling components: Water, terpineol, EDTA and other additives are added sequentially to a dissolving tank, the temperature is raised to 35-38℃, naphthol AS-PH is added, and the mixture is stirred for 18-25 min. Then, alkaline solution is added, and the mixture is stirred for another 20-30 min. After ultrasonic treatment and magnetic field treatment, the coupling component solution is obtained.

[0011] Step S3, Coupling reaction: Place the diazo component solution into the coupling reaction vessel, add the nonionic surfactant while stirring, and then add the coupling component solution dropwise over a period of 20-30 minutes. After the addition is complete, continue stirring for 50-70 minutes to obtain the coupling product.

[0012] Step S4, Pigmentation treatment: Add sulfuric acid to the coupling product to adjust the pH to 6.5-7.5, then heat to 70-90℃ and keep warm for 1-2 hours. Then cool to below 40℃, filter, wash with water until neutral, dry, and pulverize to obtain high hiding power pigment red P.R170.

[0013] Preferably, the mass ratio of water, p-aminobenzamide, hydrochloric acid, and sodium nitrite in step S1 is 500:35:69:18.2.

[0014] Preferably, the mass percentage concentration of hydrochloric acid in step S1 is 30%-31.5%.

[0015] Preferably, the diazotization reaction in step S1 takes 1-2 hours.

[0016] Preferably, the mass percentage concentration of the aqueous solution of aminosulfonic acid in step S1 is 10%-15%; and the mass percentage concentration of the aqueous solution of urea is 10-20%.

[0017] Preferably, the mass ratio of water, terroir oil, EDTA, other additives, naphthol AS-PH, and alkali solution in step S2 is 800:30:3:(2-4):79:770.

[0018] Preferably, the other additives in step S2 include the following components in parts by weight: 4-6 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 2-4 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 1-3 parts of pyridine hydroxypropanesulfonate.

[0019] Preferably, the mass percentage concentration of the alkaline solution in step S2 is 25%-35%.

[0020] Preferably, the alkaline solution in step S2 is at least one of sodium hydroxide aqueous solution, pyridine aqueous solution, and ethylenediamine aqueous solution.

[0021] Preferably, in step S2, the ultrasonic frequency of the ultrasonic treatment is 50-100kHz, the power is 300-500W, and the treatment time is 3-6min; the magnetic field strength of the magnetic field treatment is 5000-12000Gs, and the treatment time is 3-5min.

[0022] Preferably, the mass ratio of the nonionic surfactant to the naphthol AS-PH in the diazo component solution in step S3 is 79:50.

[0023] Preferably, the nonionic surfactant in step S3 is fatty alcohol polyoxyethylene ether AEO-9.

[0024] Preferably, the mass percentage concentration of sulfuric acid in step S3 is 5%-8%.

[0025] Another object of the present invention is to provide an application of the aforementioned high-coverage pigment red P.R170 in the fields of coatings, inks, plastics, and rubber.

[0026] Due to the application of the above technical solution, the present invention has the following beneficial effects:

[0027] (1) The preparation method of high hiding power pigment red P.R170 disclosed in this invention is simple in preparation process, convenient in operation and control, high in preparation efficiency and finished product qualification rate, low in dependence on equipment, suitable for continuous large-scale production, and has high promotion and application value.

[0028] (2) The preparation method of high hiding power pigment red P.R170 disclosed in this invention can completely dissolve naphthophenol AS-PH under low temperature conditions (35℃-38℃) with the synergistic solubilizing effect of styrax oil, EDTA and other additives. This greatly reduces the degree of hydrolysis of naphthophenol AS-PH during the dissolution process, thereby synthesizing high quality, good stability, strong weather resistance, high hiding power and low manufacturing cost pigment red P.R170; the preparation process has low energy consumption of public utilities, which is conducive to energy conservation and emission reduction.

[0029] (3) The preparation method of high-coverage pigment red P.R170 disclosed in this invention includes the following components in parts by weight: 4-6 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 2-4 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 1-3 parts of pyridinium hydroxypropanesulfonate; the alkaline solution is at least one of sodium hydroxide aqueous solution, pyridine aqueous solution, and ethylenediamine aqueous solution. Through the rational selection of the specific composition of other additives and alkaline solution, especially the first introduction of the amphoteric organic ionic salt pyridinium hydroxypropanesulfonate, organic alkaline solution, and energy field treatment, the low-temperature dissolution of the coupling component chromophore AS-PH can be effectively improved, avoiding hydrolysis during dissolution under high-temperature alkaline conditions, increasing the rate of coupling reaction, and thus improving the quality of pigment red P.R170, resulting in sufficient covering power, excellent tinting strength, and excellent weather resistance.

[0030] (4) The preparation method of high hiding power Pigment Red P.R170 disclosed in this invention significantly improves the hiding power and overall performance of Pigment Red P.R170 through the combination of process optimization and pigment treatment, solves the problem of insufficient hiding power of Pigment Red P.R170 prepared by traditional process, and expands its application range; water is used as the main solvent, reducing the use of organic solvents, and by optimizing the reaction conditions, the emission of waste gas and wastewater is reduced, making the preparation method relatively more environmentally friendly. Detailed Implementation

[0031] The following description is intended to disclose the invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art.

[0032] Example 1

[0033] A method for preparing a high-coverage pigment red P.R170 includes the following steps:

[0034] Step S1, Preparation of diazo component: Add water, p-aminobenzamide and hydrochloric acid to the diazotization kettle in sequence, stir until completely dissolved and clear, add ice to cool to 5°C, add sodium nitrite to carry out diazotization reaction, after the reaction is completed, add aminosulfonic acid aqueous solution dropwise until starch-potassium iodide test paper no longer shows color, and obtain diazo component solution;

[0035] Step S2, Preparation of coupling components: Water, terpineol, EDTA and other additives are added sequentially to a dissolving tank, the temperature is raised to 35°C, naphthol AS-PH is added, and the mixture is stirred for 18 min. Then, alkaline solution is added, and the mixture is stirred for another 20 min. After ultrasonic treatment and magnetic field treatment, the coupling component solution is obtained.

[0036] Step S3, Coupling reaction: Place the diazo component solution into the coupling reaction vessel, add the nonionic surfactant while stirring, and then add the coupling component solution dropwise over a period of 20 minutes. After the addition is complete, continue stirring for 50 minutes to obtain the coupling product.

[0037] Step S4, Pigmentation treatment: Add sulfuric acid to the coupling product to adjust the pH to 6.5, then heat to 70°C and keep warm for 1 hour. Then cool to below 40°C, filter, wash with water until neutral, dry, and pulverize to obtain high-coverage pigment red P.R170.

[0038] In step S1, the mass ratio of water, p-aminobenzamide, hydrochloric acid, and sodium nitrite is 500:35:69:18.2; the mass percentage concentration of hydrochloric acid in step S1 is 30%; the diazotization reaction time in step S1 is 1 hour; and the mass percentage concentration of the aqueous solution of aminosulfonic acid in step S1 is 10%.

[0039] In step S2, the mass ratio of water, terephthalic acid oil, EDTA, other additives, naphthol AS-PH, and alkali solution is 800:30:3:2:79:770. The other additives in step S2 include the following components by weight: 4 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 2 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 1 part of pyridinium hydroxypropanesulfonate. The alkali solution in step S2 has a mass percentage concentration of 25%. The alkali solution in step S2 is an aqueous sodium hydroxide solution. The ultrasonic frequency for the ultrasonic treatment in step S2 is 50 kHz, the power is 300 W, and the treatment time is 3 min. The magnetic field strength for the magnetic field treatment is 5000 Gs, and the treatment time is 3 min.

[0040] The mass ratio of the nonionic surfactant to the naphthol AS-PH in the diazo component solution in step S3 is 79:50; the nonionic surfactant in step S3 is fatty alcohol polyoxyethylene ether AEO-9; and the mass percentage concentration of sulfuric acid in step S3 is 5%.

[0041] Example 2

[0042] A method for preparing a high-coverage pigment red P.R170 includes the following steps:

[0043] Step S1, Preparation of diazo component: Add water, p-aminobenzamide and hydrochloric acid to the diazotization kettle in sequence, stir until completely dissolved and clear, add ice to cool to 4°C, add sodium nitrite to carry out diazotization reaction, after the reaction is completed, add urea aqueous solution dropwise until starch-potassium iodide test paper no longer shows color, and obtain diazo component solution;

[0044] Step S2, Preparation of Coupling Components: Water, Taikoo Oil, EDTA and other additives are added sequentially to a dissolving tank, the temperature is raised to 36°C, naphthol AS-PH is added, and the mixture is stirred for 20 min. Then, alkaline solution is added, and the mixture is stirred for another 22 min. After ultrasonic and magnetic field treatment, the coupling component solution is obtained.

[0045] Step S3, Coupling reaction: Place the diazo component solution into the coupling reaction vessel, add the nonionic surfactant while stirring, and then add the coupling component solution dropwise over a period of 23 minutes. After the addition is complete, continue stirring for 55 minutes to obtain the coupling product.

[0046] Step S4, Pigmentation treatment: Add sulfuric acid to the coupling product to adjust the pH to 6.7, then heat to 75°C and keep warm for 1.2 hours. Then cool to below 40°C, filter, wash with water until neutral, dry, and pulverize to obtain high-coverage pigment red P.R170.

[0047] The mass ratio of water, p-aminobenzamide, hydrochloric acid, and sodium nitrite in step S1 is 500:35:69:18.2; the mass percentage concentration of hydrochloric acid in step S1 is 30.5%; the diazotization reaction time in step S1 is 1.2 h; and the mass percentage concentration of the aqueous urea solution in step S1 is 13%.

[0048] In step S2, the mass ratio of water, terpineol, EDTA, other additives, naphthol AS-PH, and alkali solution is 800:30:3:2.5:79:770. The other additives in step S2 include the following components by weight: 4.5 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 2.5 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 1.5 parts of pyridine hydroxypropanesulfonate. The alkali solution in step S2 has a mass percentage concentration of 27%. The alkali solution in step S2 is an aqueous pyridine solution. The ultrasonic frequency for the ultrasonic treatment in step S2 is 70 kHz, the power is 350 W, and the treatment time is 4 min. The magnetic field strength for the magnetic field treatment is 7000 Gs, and the treatment time is 3.5 min.

[0049] The mass ratio of the nonionic surfactant to the naphthol AS-PH in the diazo component solution in step S3 is 79:50; the nonionic surfactant in step S3 is fatty alcohol polyoxyethylene ether AEO-9; and the mass percentage concentration of sulfuric acid in step S3 is 6%.

[0050] Example 3

[0051] A method for preparing a high-coverage pigment red P.R170 includes the following steps:

[0052] Step S1, Preparation of diazo component: Add water, p-aminobenzamide and hydrochloric acid to the diazotization kettle in sequence, stir until completely dissolved and clear, add ice to cool to 3°C, add sodium nitrite to carry out diazotization reaction, after the reaction is completed, add aminosulfonic acid aqueous solution dropwise until starch-potassium iodide test paper no longer shows color, and obtain diazo component solution;

[0053] Step S2, Preparation of coupling components: Water, terpineol, EDTA and other additives are added sequentially to a dissolving tank, the temperature is raised to 36.5℃, naphthol AS-PH is added, and the mixture is stirred for 22 min. Then, alkaline solution is added, and the mixture is stirred for another 25 min. After ultrasonic treatment and magnetic field treatment, the coupling component solution is obtained.

[0054] Step S3, Coupling reaction: Place the diazo component solution into the coupling reaction vessel, add the nonionic surfactant while stirring, and then add the coupling component solution dropwise over a period of 25 minutes. After the addition is complete, continue stirring for 60 minutes to obtain the coupling product.

[0055] Step S4, Pigmentation treatment: Add sulfuric acid to the coupling product to adjust the pH to 7, then heat to 80℃ and keep warm for 1.5h, then cool to below 40℃, filter, wash with water until neutral, dry, and pulverize to obtain high hiding power pigment red P.R170.

[0056] The mass ratio of water, p-aminobenzamide, hydrochloric acid, and sodium nitrite in step S1 is 500:35:69:18.2; the mass percentage concentration of hydrochloric acid in step S1 is 31%; and the diazotization reaction time in step S1 is 1.5 h.

[0057] The aqueous solution of aminosulfonic acid in step S1 has a mass percentage concentration of 13%; the mass ratio of water, terephthalic acid oil, EDTA, other additives, naphthol AS-PH, and alkali solution in step S2 is 800:30:3:3:79:770; the other additives in step S2 include the following components by weight: 5 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 3 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 2 parts of pyridinium hydroxypropanesulfonate.

[0058] The mass percentage concentration of the alkaline solution in step S2 is 30%; the alkaline solution in step S2 is an aqueous solution of ethylenediamine; the ultrasonic frequency of the ultrasonic treatment in step S2 is 75 kHz, the power is 400 W, and the treatment time is 4.5 min; the magnetic field strength of the magnetic field treatment is 9000 Gs, and the treatment time is 4 min; the mass ratio of the nonionic surfactant to the naphthol AS-PH in the diazo component solution in step S3 is 79:50; the nonionic surfactant in step S3 is fatty alcohol polyoxyethylene ether AEO-9; the mass percentage concentration of the sulfuric acid in step S3 is 7.5%.

[0059] Example 4

[0060] A method for preparing a high-coverage pigment red P.R170 includes the following steps:

[0061] Step S1, Preparation of diazo component: Add water, p-aminobenzamide and hydrochloric acid to the diazotization kettle in sequence, stir until completely dissolved and clear, add ice to cool to 2°C, add sodium nitrite to carry out diazotization reaction, after the reaction is completed, add urea aqueous solution dropwise until starch-potassium iodide test paper no longer shows color, and obtain diazo component solution;

[0062] Step S2, preparation of coupling components: Water, Taikoo oil, EDTA and other additives are added sequentially to a dissolving tank, the temperature is raised to 37°C, naphthol AS-PH is added, and the mixture is stirred for 23 min. Then, alkaline solution is added, and the mixture is stirred for another 28 min. After ultrasonic treatment and magnetic field treatment, the coupling component solution is obtained.

[0063] Step S3, Coupling reaction: Place the diazo component solution into the coupling reaction vessel, add the nonionic surfactant while stirring, and then add the coupling component solution dropwise over a period of 28 minutes. After the addition is complete, continue stirring for 67 minutes to obtain the coupling product.

[0064] Step S4, Pigmentation treatment: Add sulfuric acid to the coupling product to adjust the pH to 7.3, then heat to 85℃ and keep warm for 1.8h, then cool to below 40℃, filter, wash with water until neutral, dry, and pulverize to obtain high hiding power pigment red P.R170.

[0065] The mass ratio of water, p-aminobenzamide, hydrochloric acid, and sodium nitrite in step S1 is 500:35:69:18.2; the mass percentage concentration of hydrochloric acid in step S1 is 31.3%; the diazotization reaction time in step S1 is 1.8 h; and the mass percentage concentration of the aqueous urea solution in step S1 is 18%.

[0066] In step S2, the mass ratio of water, terephthalic acid oil, EDTA, other additives, naphthol AS-PH, and alkali solution is 800:30:3:3.5:79:770. The other additives in step S2 include the following components by weight: 5.5 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 3.5 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 2.5 parts of pyridinium hydroxypropanesulfonate. The alkali solution in step S2 has a mass percentage concentration of 33%. The alkali solution in step S2 is an aqueous sodium hydroxide solution. The ultrasonic frequency for the ultrasonic treatment in step S2 is 90 kHz, the power is 450 W, and the treatment time is 5.5 min. The magnetic field strength for the magnetic field treatment is 11000 Gs, and the treatment time is 4.5 min.

[0067] The mass ratio of the nonionic surfactant to the naphthol AS-PH in the diazo component solution in step S3 is 79:50; the nonionic surfactant in step S3 is fatty alcohol polyoxyethylene ether AEO-9; and the mass percentage concentration of sulfuric acid in step S3 is 7.7%.

[0068] Example 5

[0069] A method for preparing a high-coverage pigment red P.R170 includes the following steps:

[0070] Step S1, Preparation of diazo component: Add water, p-aminobenzamide and hydrochloric acid to the diazotization kettle in sequence, stir until completely dissolved and clear, add ice to cool to 1°C, add sodium nitrite to carry out diazotization reaction, after the reaction is completed, add aminosulfonic acid aqueous solution dropwise until starch-potassium iodide test paper no longer shows color, and obtain diazo component solution;

[0071] Step S2, Preparation of Coupling Component: Water, Taikoo Oil, EDTA and other additives are added sequentially to a dissolving tank, the temperature is raised to 38°C, naphthol AS-PH is added, and the mixture is stirred for 25 minutes. Then, alkaline solution is added, and the mixture is stirred for another 30 minutes. After ultrasonic treatment and magnetic field treatment, the coupling component solution is obtained.

[0072] Step S3, Coupling reaction: Place the diazo component solution into the coupling reaction vessel, add the nonionic surfactant while stirring, and then add the coupling component solution dropwise over a period of 30 minutes. After the addition is complete, continue stirring for 70 minutes to obtain the coupling product.

[0073] Step S4, Pigmentation treatment: Add sulfuric acid to the coupling product to adjust the pH to 7.5, then heat to 90℃ and keep warm for 2 hours. Then cool to below 40℃, filter, wash with water until neutral, dry, and pulverize to obtain high hiding power pigment red P.R170.

[0074] The mass ratio of water, p-aminobenzamide, hydrochloric acid, and sodium nitrite in step S1 is 500:35:69:18.2; the mass percentage concentration of hydrochloric acid in step S1 is 31.5%; the diazotization reaction time in step S1 is 2 hours; and the mass percentage concentration of the aqueous solution of aminosulfonic acid in step S1 is 15%.

[0075] The mass ratio of water, Taikoo oil, EDTA, other additives, naphthol AS-PH, and alkali solution in step S2 is 800:30:3:4:79:770; the other additives in step S2 include the following components by weight: 6 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 4 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 3 parts of pyridinium hydroxypropanesulfonate.

[0076] The mass percentage concentration of the alkaline solution in step S2 is 35%; the alkaline solution in step S2 is an aqueous pyridine solution; the ultrasonic frequency of the ultrasonic treatment in step S2 is 100kHz, the power is 500W, and the treatment time is 6min; the magnetic field strength of the magnetic field treatment is 12000Gs, and the treatment time is 5min.

[0077] The mass ratio of the nonionic surfactant to the naphthol AS-PH in the diazo component solution in step S3 is 79:50; the nonionic surfactant in step S3 is fatty alcohol polyoxyethylene ether AEO-9; and the mass percentage concentration of sulfuric acid in step S3 is 8%.

[0078] Comparative Example 1

[0079] A method for preparing a high-coverage pigment red P.R170 is basically the same as in Example 1, except that no EDTA or other additives are added, and no ultrasonic treatment is performed; the magnetic field treatment time is 6 minutes.

[0080] Comparative Example 2

[0081] A method for preparing a high-coverage pigment red P.R170 is basically the same as in Example 1, except that the temperature is raised to 85°C during the preparation of the coupling component, and there is no magnetic field treatment, and the ultrasonic treatment time is 6 minutes.

[0082] To further illustrate the beneficial technical effects of the preparation methods of high-octane pigment red P.R170 involved in the various embodiments of the present invention, relevant performance tests were conducted on the pigment red P.R170 prepared by the preparation methods of high-octane pigment red P.R170 involved in Examples 1-5 and Comparative Examples 1-2. The test results are shown in Table 1. The test methods are as follows: the opacity was tested according to GB / T 5211.17-2013 "General Test Methods for Pigments and Extenders - Part 17: Determination of Occlusive Power"; the tinting strength was tested according to GB / T 5211.19-2013 "General Test Methods for Pigments and Extenders - Part 19: Determination of Tinting Strength"; the weather resistance was evaluated with reference to GB / T 1766-2008 "Rating Methods for Aging of Paint and Varnish Coatings", and an artificial accelerated aging test was conducted using a xenon lamp aging test chamber with a light intensity of 0.55 W / m². 2 Light cycle: 8 hours under light, 4 hours under darkness; Temperature and humidity: 65℃ and 60%RH under light, 45℃ and 95%RH under darkness; Water spray cycle: 18 minutes of water spraying every 120 minutes; Test time: 1000 hours.

[0083] Table 1

[0084]

[0085] As can be seen from Table 1, the high-coverage pigment red P.R170 prepared by the preparation method involved in the embodiments of the present invention has higher hiding power, tinting strength and weather resistance than the comparative product; the combined use and design of EDTA, other additives, ultrasonic treatment, magnetic field treatment and low-temperature dissolution of coupling components are beneficial to improving the above properties.

[0086] The above embodiments are only for illustrating the technical concept and features of the present invention. Their purpose is to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be used to limit the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A method for preparing a high-coverage pigment red P.R170, characterized in that, Includes the following steps: Step S1, Preparation of diazo component: Add water, p-aminobenzamide and hydrochloric acid to the diazotization reactor in sequence, stir until completely dissolved and clear, add ice to cool to 0-5℃, add sodium nitrite to carry out diazotization reaction, after the reaction is completed, add aqueous solution of aminosulfonic acid or aqueous solution of urea dropwise until starch-potassium iodide test paper no longer shows color, and obtain diazo component solution; Step S2, Preparation of Coupling Components: Add water, terpineol, EDTA and other additives sequentially to a dissolving tank, heat to 35-38℃, add naphthol AS-PH, stir for 18-25 min, then add alkaline solution, continue stirring for 20-30 min, and after ultrasonic and magnetic field treatment, obtain the coupling component solution. Step S3, Coupling reaction: Place the diazo component solution into the coupling reaction vessel, add the nonionic surfactant while stirring, and then add the coupling component solution dropwise over a period of 20-30 minutes. After the addition is complete, continue stirring for 50-70 minutes to obtain the coupling product. Step S4, Pigmentation treatment: Add sulfuric acid to the coupling product to adjust the pH to 6.5-7.5, then heat to 70-90℃ and keep warm for 1-2 hours. Then cool to below 40℃, filter, wash with water until neutral, dry, and pulverize to obtain high-coverage pigment red P.R170.

2. The method for preparing high-coverage pigment red P.R170 according to claim 1, characterized in that, The mass ratio of water, p-aminobenzamide, hydrochloric acid, and sodium nitrite in step S1 is 500:35:69:18.

2.

3. The method for preparing high-octane pigment red P.R170 according to claim 1, characterized in that, The mass percentage concentration of hydrochloric acid in step S1 is 30%-31.5%; the diazotization reaction time in step S1 is 1-2 hours.

4. The method for preparing high-octane pigment red P.R170 according to claim 1, characterized in that, The mass percentage concentration of the aqueous solution of aminosulfonic acid in step S1 is 10%-15%; the mass percentage concentration of the aqueous solution of urea is 10-20%.

5. The method for preparing high-octane pigment red P.R170 according to claim 1, characterized in that, The mass ratio of water, Taikoo oil, EDTA, other additives, naphthol AS-PH, and alkali solution in step S2 is 800:30:3:(2-4):79:

770.

6. The method for preparing high-octane pigment red P.R170 according to claim 5, characterized in that, The other additives mentioned in step S2 include the following components in parts by weight: 4-6 parts of sodium 3-tris(hydroxymethyl)methylamine-2-hydroxypropanesulfonate, 2-4 parts of sodium 3-(N-morpholino)-2-hydroxypropanesulfonate, and 1-3 parts of pyridinium hydroxypropanesulfonate.

7. The method for preparing high-octane pigment red P.R170 according to claim 1, characterized in that, The mass percentage concentration of the alkaline solution in step S2 is 25%-35%; the alkaline solution in step S2 is at least one of sodium hydroxide aqueous solution, pyridine aqueous solution, and ethylenediamine aqueous solution.

8. The method for preparing high-octane pigment red P.R170 according to claim 1, characterized in that, In step S2, the ultrasonic frequency of the ultrasonic treatment is 50-100kHz, the power is 300-500W, and the treatment time is 3-6min; the magnetic field strength of the magnetic field treatment is 5000-12000Gs, and the treatment time is 3-5min.

9. The method for preparing high-octane pigment red P.R170 according to claim 1, characterized in that, In step S3, the mass ratio of the nonionic surfactant to the naphthol AS-PH in the coupling component solution is 79:50; the nonionic surfactant in step S3 is fatty alcohol polyoxyethylene ether AEO-9; and the mass percentage concentration of sulfuric acid in step S4 is 5%-8%.

Citation Information

Patent Citations

  • Production method of environment-friendly organic pigment red 170

    CN106046844B

  • Method for producing environment-friendly organic pigment red 170

    CN106046844A

  • Azo pigment red and synthesis method thereof

    CN107513288A