Method for coaxial conjugate electrospinning of nanofiber covered yarns for personal thermal management

The preparation of core-shell structured nanofiber-coated yarns by coaxial conjugate electrospinning solves the problem of easy leakage of phase change materials in textiles, achieves stable and continuous heat storage, temperature regulation and cooling effects, and improves the mechanical properties and service life of the fabric.

CN120174524BActive Publication Date: 2026-11-24XI'AN POLYTECHNIC UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510568495.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-30
Publication Date
2026-11-24
Estimated Expiration
2045-04-30

AI Technical Summary

Technical Problem

In existing technologies, phase change materials are prone to leakage in textiles, leading to reduced heat utilization efficiency and service life. Photothermal conversion and radiative cooling cannot achieve all-weather temperature regulation under unstable energy supply and demand conditions, and existing encapsulation methods have poor adhesion.

Method used

A core-shell structured nanofiber-coated yarn was prepared using a coaxial conjugate electrospinning method. The phase change material was used as the core layer, and the polymer and temperature-regulating functional material were used as the shell layer. The core-shell structured nanofibers were uniformly coated on the outside of the core yarn using coaxial conjugate electrospinning technology to form a core-shell structured nanofiber-coated yarn.

Benefits of technology

It improves the mechanical properties of the fabric, avoids leakage of phase change materials, achieves stable and continuous heat storage and temperature regulation and cooling effects, enhances the stability and durability of photothermal conversion and radiative cooling, and improves the breathability, comfort and aesthetics of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120174524B_ABST
    Figure CN120174524B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing nanofiber-coated yarn for personal thermal management using coaxial conjugate electrospinning, comprising: step 1, preparing core-layer spinning solution and shell-layer spinning solution; step 2, constructing a coaxial conjugate electrospinning apparatus; and step 3, forming a nanofiber-coated yarn for personal thermal management with a core yarn as the core layer and a core-shell structure nanofiber with temperature-regulating function as the outer layer. This invention combines coaxial electrospinning with conjugate electrospinning, rotating and wrapping the spun core-shell structure nanofibers (with phase change material as the core layer) onto the core yarn, while simultaneously loading temperature-regulating materials onto the core-shell structure nanofibers, forming a temperature-regulating nanofiber-coated yarn suitable for personal thermal management.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of personal thermal management, specifically a method for preparing nanofiber-coated yarns for personal thermal management using coaxial conjugate electrospinning. Background Technology

[0002] Currently, the goal of Personal Thermal Management (PTM) technology is to regulate human body temperature without wasting excess energy, including personal insulation, cooling, and temperature regulation. Related to this, smart textiles, capable of spontaneous temperature control, have more flexible and widespread applications, effectively promoting human thermal comfort. Smart textiles, due to their flexibility, scalability, and ability to meet energy-saving and diverse personal temperature regulation needs, show great promise in PTM technology. Reducing energy consumption is key to sustainable development, and to date, photothermal conversion and radiative cooling have shown great promise in smart textiles.

[0003] Solar energy, as a green, clean, and renewable energy source, primarily provides light and heat to the Earth in the form of electromagnetic radiation. Due to its inexhaustible nature, using solar energy for intelligent temperature regulation has become a research hotspot. By utilizing the photothermal conversion mechanism of photothermal conversion materials to convert absorbed light energy into heat energy, thereby providing warmth to fabrics and the human body, this can alleviate resource scarcity to some extent. However, solar energy is unstable and discontinuous, and cannot guarantee all-weather intelligent temperature regulation. To alleviate this instability in energy supply and demand, thermal energy storage technology can be employed. Phase change materials (PCMs), as energy storage media, can store or release large amounts of energy at near-constant temperatures during melting or solidification. Solid-liquid phase change materials are commonly used, but when the external temperature reaches their phase change temperature, a solid-liquid transition occurs, leading to drawbacks such as easy leakage during heat utilization, thus reducing heat utilization efficiency and lifespan. Therefore, encapsulation technology has become an essential process step. Currently, the main encapsulation methods for PCMs are: hollow fiber impregnation, microencapsulation, and electrospinning.

[0004] Passive radiative cooling (PRC) technology requires no energy input and relies primarily on the excellent light management capabilities of materials, including high solar reflectivity and mid-infrared emissivity. By reflecting sunlight (wavelengths 0.3–2.5 μm) and simultaneously utilizing its excellent mid-infrared emissivity, heat is emitted from the infrared atmospheric window (wavelengths 8–13 μm) into the external space, achieving spontaneous cooling of the object's surface without the need for external energy consumption. In recent years, researchers have applied PRC technology to fabrics to create PRC textiles with cooling or heat dissipation functions, showing broad application prospects in high-temperature energy saving and radiative cooling. PRC textiles can be designed using the optical properties and structure of materials. High infrared emissivity materials can dissipate heat quickly, while high solar reflectivity materials can minimize heat absorption. Simultaneously, structural designs can also achieve ideal cooling effects, including loaded nanoparticles, porous structures, and multilayer structures. These material and structural designs enable PRC textiles to exhibit ideal cooling performance.

[0005] Therefore, combining photothermal conversion, radiative cooling, and phase change materials for application in the field of personal thermal management textiles has practical significance and promising development prospects. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the technical problem this invention aims to solve is to provide a method for preparing nanofiber-coated yarns for personal thermal management using coaxial conjugate electrospinning.

[0007] The technical solution of this invention to solve the aforementioned technical problem is to provide a method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning, the method comprising the following steps:

[0008] Step 1: Prepare the core spinning solution and the shell spinning solution;

[0009] The phase change material is heated and melted into a liquid state to obtain the core spinning solution;

[0010] The polymer is dissolved in an organic solvent to obtain a polymer solution; then the temperature-regulating functional material is added to the polymer solution and dispersed evenly to obtain a shell spinning solution; the temperature-regulating functional material is one of photothermal material or radiative cooling material;

[0011] Step 2: Construct a coaxial conjugate electrospinning device;

[0012] The device includes a shell spinning solution propeller, a core spinning solution propeller, a coaxial needle, a positive electrode, a negative electrode, an unwinding roller, a metal rotating funnel, and a collection device.

[0013] The coaxial needle is a coaxial structure with a core layer channel and a shell layer channel, with the shell layer channel nested outside the core layer channel. Both the shell layer spinning solution propeller and the core layer spinning solution propeller are mounted on the coaxial needle. The shell layer spinning solution propeller is connected to the shell layer channel and pushes the shell layer spinning solution into the shell layer channel during spinning. The core layer spinning solution propeller is connected to the core layer channel and pushes the core layer spinning solution into the core layer channel during spinning.

[0014] Along the direction of core yarn advance, an unwinding roller, a metal rotating funnel, and a collecting device are arranged in sequence; the core yarn is wound on the unwinding roller and is released during spinning; the collecting device is used to collect the nanofiber-coated yarn for personal thermal management and control the moving speed of the core yarn.

[0015] The two coaxial needles are located on the same horizontal plane; the metal rotating funnel is equidistant from the two coaxial needles, located on the perpendicular bisector of the two needles, and within the electrostatic field generated by the coaxial needles when high voltage is applied; one of the two coaxial needles is connected to the positive terminal of the power supply, and the other is connected to the negative terminal of the power supply, in order to generate an electrostatic field; the metal rotating funnel can rotate along its own central axis.

[0016] Step 3: Prepare nanofiber-coated yarn for personal thermal management;

[0017] Set the spinning parameters; place the shell spinning solution in the shell spinning solution propeller and the core spinning solution in the core spinning solution propeller; one end of the core yarn is wound around the unwinding roller, passes through the metal rotating funnel, and the other end is wound around the collecting device, and the core yarn is pulled and moved by the collecting device;

[0018] The process begins with coaxial conjugate electrospinning to achieve uniform coating of core-shell structured nanofibers, with the core layer being a phase change material and the shell layer being a polymer and a temperature-regulating functional material, onto the outer side of the core yarn, forming a nascent coated yarn with the core yarn as the core layer and the core-shell structured nanofibers as the outer layer; the nascent coated yarn is then dried until all the solvent evaporates to obtain nanofiber coated yarn for personal thermal management.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] (1) This invention combines coaxial electrospinning with conjugate electrospinning, and rotates the spun phase change material as the core layer of the core-shell structure nanofibers onto the core yarn, while loading the core-shell structure nanofibers with temperature regulation function materials to form a temperature regulation nanofiber coated yarn suitable for personal thermal management.

[0021] (2) The nanofiber-coated yarn for personal thermal management prepared by coaxial conjugate electrospinning is formed by using a core yarn as the core layer and a core-shell structured nanofiber with temperature-regulating function as the outer layer. Compared with the film formed by spraying, this form of wrapping and winding the core-shell structured nanofibers on the core yarn greatly improves the mechanical properties of the fabric, makes it less prone to falling off and wear during use, and avoids the problem of poor adhesion of the film directly attached to the fabric.

[0022] (3) The temperature-regulating nanofiber-coated yarn of the present invention for personal thermal management can be woven as a basic unit, and further processed and compounded to make fabrics with various structures and patterns, realizing the functionalization and mechanical properties of intelligent temperature-regulating textiles. Compared with fabrics with nanofiber membranes, fabrics woven with the coated yarn as the matrix have greatly improved breathability, comfort, aesthetics and wearing performance.

[0023] (4) Compared with ordinary photothermal performance coated yarn, the photothermal phase change nanofiber coated yarn prepared in this invention uses photothermal phase change nanofibers with a core-shell structure. This type of nanofiber has stronger encapsulation properties for phase change materials, avoiding leakage during use. It has a long service life, is stable and continuous, and has good durability, achieving a stable and continuous heat storage and temperature regulation effect. Combining photothermal materials with phase change materials can store the solar heat absorbed by the photothermal materials in the phase change materials, achieving comprehensive performance such as high heat storage capacity, excellent photothermal conversion performance, and good thermal conductivity and heat dissipation.

[0024] (5) Compared with ordinary radiation-cooling yarn, the passive radiation-cooling nanofiber coated yarn prepared in this invention uses passive radiation-cooling nanofibers with a core-shell structure. The excellent heat storage effect of the core layer PCM and the high solar reflectance and high infrared emission of the shell layer combine internally and externally, making the cooling effect more stable and continuous. At the same time, the superior structure has a stronger encapsulation of PCM, avoiding leakage during use. It has a long service life, is stable and continuous, and has good durability, achieving a stable and continuous cooling effect. The porous structure of the interwoven nanofibers in the passive radiation-cooling nanofiber coated yarn can scatter and diffract the solar spectrum multiple times, and the added high reflectivity particles also have a high reflectivity to the solar spectrum. At the same time, the polymer used is also a high-emissivity material, which can dissipate heat in time, ultimately resulting in a high reflectivity and solar emissivity to the solar spectrum. Attached Figure Description

[0025] Figure 1 This is a schematic diagram of the preparation process of the nanofiber coated yarn of the present invention;

[0026] Figure 2 This is a schematic diagram of the coaxial needle of the present invention;

[0027] Figure 3 The surface SEM image of the photothermal phase change nanofiber coated yarn prepared in Example 1 of this invention is magnified 1000 times.

[0028] Figure 4 The surface SEM image of the photothermal phase change nanofiber coated yarn prepared in Example 1 of this invention is magnified 2000 times.

[0029] Figure 5 This is a cross-sectional SEM image magnified 150 times of the photothermal phase change nanofiber coated yarn prepared in Example 1 of the present invention.

[0030] Figure 6 This is a 300x magnified cross-sectional SEM image of the photothermal phase change nanofiber coated yarn prepared in Example 1 of the present invention.

[0031] Figure 7 This is a test diagram of the photothermal conversion performance of the photothermal phase change nanofiber coated yarn prepared in Example 1 of the present invention;

[0032] Figure 8 The image shows the DSC performance test results of the photothermal phase change nanofiber coated yarn prepared in Example 1 of this invention.

[0033] Figure 9 This is a 200x magnified SEM image of the surface of the passive radiation cooling nanofiber-coated yarn prepared in Example 5 of the present invention.

[0034] Figure 10 This is a 500x magnified SEM image of the surface of the passive radiation cooling nanofiber-coated yarn prepared in Example 5 of the present invention;

[0035] Figure 11 The image shows the DSC performance test results of the passive radiation cooling nanofiber coated yarn prepared in Example 5 of this invention.

[0036] Figure 12 Temperature curves comparing the cooling effects of the core yarn used in Example 5 of this invention and the passive radiation cooling nanofiber coated yarn.

[0037] Figure 1 In the middle, there are: shell spinning solution propeller 1, core spinning solution propeller 2, coaxial needle 3, positive electrode 4, negative electrode 5, core-shell structured nanofiber 6, core yarn 7, unwinding roller 8, metal rotating funnel 9, fiber web 10, personal thermal management nanofiber coated yarn 11, and collection device 12; shell channel 301 and core channel 302. Detailed Implementation

[0038] Specific embodiments of the present invention are given below. These specific embodiments are only used to further illustrate the present invention in detail and do not limit the scope of protection of the present invention.

[0039] This invention provides a method for preparing nanofiber-coated yarns for personal thermal management using coaxial conjugate electrospinning (hereinafter referred to as the method), which includes the following steps:

[0040] Step 1: Prepare the core spinning solution and the shell spinning solution;

[0041] The phase change material is heated and melted into a liquid state to obtain the core spinning solution;

[0042] The polymer is dissolved in an organic solvent to obtain a polymer solution; then the temperature-regulating material is added to the polymer solution and dispersed evenly to obtain a shell spinning solution;

[0043] Preferably, in step 1, the phase change material is one of n-octadecane, n-tetradecane, polyethylene glycol, or paraffin.

[0044] Preferably, in step 1, the phase change material heating process is: heating at 40-50°C for 0.5-1 hour; preferably, it is carried out in a water bath.

[0045] Preferably, in step 1, the polymer is polyacrylonitrile (PAN) or polyvinylidene fluoride (PVDF); the organic solvent is DMF (N,N-dimethylformamide) and / or acetone; when the polymer is PVDF, the organic solvent is a mixed solvent in which the mass ratio of DMF to acetone is 6-7:3-4.

[0046] Preferably, in step 1, the polymer dissolution process is: stirring at 1000-2000 rpm for 6-10 hours at 60-70°C.

[0047] Preferably, in step 1, the temperature-regulating material is either a photothermal material or a radiative cooling material.

[0048] Preferably, in step 1, the photothermal material is Mxene or graphene; the radiative cooling material is one or more of TiO2, SiO2, BaSO4 or ZnO (preferably a combination of ZnO and SiO2 in a mass ratio of 1:1); and the particle size of the radiative cooling material is 80-1600 nm (preferably 80-100 nm).

[0049] Preferably, in step 1, the dispersion process of the temperature-regulating functional material is as follows: first, stir at a speed of 1000-2000 rpm for 1-2 hours, and then sonicate at 80-120 Hz / min for 1-2 hours.

[0050] Preferably, in step 1, the mass fraction of the polymer in the shell spinning solution is 10-15%; the mass fraction of the photothermal material is 1-5%; and the mass fraction of the radiative cooling material is 2-8% (preferably 4-6%).

[0051] Preferably, in step 1, Mxene is subjected to centrifugal expansion treatment or graphene is subjected to dispersion treatment so that Mxene or graphene can be miscible with the organic solvent in step 1, which is the prior art.

[0052] Step 2: Construct a coaxial conjugate electrospinning device;

[0053] The device includes a shell spinning solution propeller 1, a core spinning solution propeller 2, a coaxial needle 3, a positive electrode 4, a negative electrode 5, an unwinding roller 8, a metal rotating funnel 9, and a collection device 12.

[0054] The coaxial needle 3 has a coaxial structure with a core layer channel 302 and a shell layer channel 301, with the shell layer channel 301 nested outside the core layer channel 302; both the shell layer spinning solution propeller 1 and the core layer spinning solution propeller 2 are mounted on the coaxial needle 3; the shell layer spinning solution propeller 1 is connected to the shell layer channel 301 and pushes the shell layer spinning solution into the shell layer channel 301 during spinning; the core layer spinning solution propeller 2 is connected to the core layer channel 302 and pushes the core layer spinning solution into the core layer channel 302 during spinning.

[0055] Along the forward direction of the core yarn 7, an unwinding roller 8, a metal rotating funnel 9, and a collecting device 12 are arranged in sequence; the core yarn 7 is wound on the unwinding roller 8 and is released during spinning; the collecting device 12 is used to collect the final product, namely the nanofiber coated yarn 11 for personal thermal management (referred to as coated yarn 11), and to control the moving speed of the core yarn 7.

[0056] Two coaxial needles 3 are located on the same horizontal plane; the metal rotating funnel 9 is equidistant from the two coaxial needles 3, located on the perpendicular plane between them, and within the range of the electrostatic field generated by the coaxial needles 3 when high voltage is applied; one of the two coaxial needles 3 is connected to the positive terminal 4 of the power supply, and the other is connected to the negative terminal 5 of the power supply, in order to generate an electrostatic field; the metal rotating funnel 9 can rotate along its own central axis.

[0057] Preferably, in step 2, the core yarn 7 is yarn, preferably one of cotton yarn, polyester yarn, nylon yarn or polyester-cotton yarn.

[0058] Preferably, in step 2, the metal rotating funnel 9 is funnel-shaped.

[0059] Preferably, in step 2, to avoid interference, the outer wall of the coaxial needle 3 is perforated, and the shell spinning liquid propeller 1 is fixed at the perforation on the outer wall of the coaxial needle 3 and communicates with the side wall of the shell channel 301; more preferably, the shell spinning liquid propeller 1 and the core spinning liquid propeller 2 are perpendicular to each other.

[0060] Step 3: Prepare nanofiber-coated yarn 11 for personal thermal management;

[0061] Set the spinning parameters; place the shell spinning solution in the shell spinning solution propeller 1 and the core spinning solution in the core spinning solution propeller 2; one end of the core yarn 7 is wound around the unwinding roller 8, passes through the metal rotating funnel 9, and the other end is wound around the collecting device 12, and the core yarn 7 is pulled and moved by the collecting device 12.

[0062] Coaxial conjugate electrospinning is initiated to achieve a core-shell structure nanofiber 6 with a core layer of phase change material and a shell layer of polymer and temperature-regulating functional material uniformly coated on the outside of the core yarn 7, forming a nascent coated yarn with the core yarn 7 as the core layer and the core-shell structure nanofiber 6 as the skin layer; the nascent coated yarn is then dried until all the solvent evaporates to obtain nanofiber coated yarn 11 for personal thermal management.

[0063] Preferably, in step 3, the specific process of coaxial conjugate electrospinning is as follows: The DC power supply is turned on, and spinning begins. During spinning, the core yarn 7 is in a straightened state. Under the action of a high-voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into fibers, forming core-shell structured nanofibers 6. The anisotropy of positive and negative charges causes the core-shell structured nanofibers 6 spun by the two coaxial needles 3 to become entangled. Simultaneously, electrostatic induction occurs between the two coaxial needles 3 and the rotating metal funnel 9, collecting the core-shell structured nanofibers 6 in the rotating metal funnel. On the funnel 9; through the traction of the electrospun fibers by the core yarn 7, a triangular pyramidal fiber web 10 is formed at the opening of the metal rotating funnel 9, which is composed of multiple bundles of core-shell structured nanofibers 6; through the stretching and traction of the core yarn 7 by the collecting device 12, the fiber bundles in the fiber web 10 are oriented; at the same time, the rotation of the metal rotating funnel 9 causes the fiber bundles to be evenly entangled and covered on the outer surface of the core yarn 7 to form an outer coating layer, and finally a nascent covered yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer is formed on the collecting device 12.

[0064] Preferably, in step 3, the spinning parameters are as follows: the distance between the two coaxial needles 3 is 15-20 cm; the distance between the coaxial needles 3 and the metal rotating funnel 9 is 12-15 cm; the voltage of the positive electrode 4 is 5-7 kV, and the voltage of the negative electrode 5 is -7 to -5 kV; the propulsion rate of the shell spinning solution is 0.4-0.7 mL / h, and the propulsion rate of the core spinning solution is 0.1-0.2 mL / h; the moving speed (i.e., the collection speed) of the core yarn 7 is adjusted by adjusting the rotation speed of the collecting device 12 so that the collection speed is adapted to the spinning speed, and the moving speed of the core yarn 7 is 0.1-0.4 mm / s; the rotation speed of the metal rotating funnel 9 is 300-500 rpm; the spinning environment temperature is 25±5℃, and the humidity is 40±5%.

[0065] Preferably, in step 3, the mass ratio of core-shell structured nanofibers 6 to core yarn 7 is 0.2 to 0.5:1 (preferably 0.2 to 0.3:1).

[0066] Preferably, in step 3, the average diameter of the nanofiber-coated yarn 11 for personal thermal management is 380–600 μm (preferably 400–500 μm).

[0067] Preferably, in step 3, the drying process is as follows: drying in an indoor environment (i.e., temperature of 20-35°C and humidity of 20-40%) for at least 4 hours.

[0068] Preferably, in step 3, the core-shell structured nanofiber 6 is a core-shell structured photothermal phase change nanofiber or a core-shell structured passive radiation cooling nanofiber.

[0069] Preferably, in step 3, the nanofiber coated yarn 11 for personal thermal management is a photothermal phase change nanofiber coated yarn or a passive radiation cooling nanofiber coated yarn.

[0070] Example 1:

[0071] (1) Preparation of core spinning solution and shell spinning solution;

[0072] The core spinning solution was obtained by heating n-octadecane crystals at 45°C for 0.5 h.

[0073] PAN was dissolved in DMF and heated at 60°C with stirring at 1000 rpm for 8 hours until completely dissolved, yielding a PAN solution. Then, centrifuged and expanded MXene was added to the PAN solution, stirred at 1000 rpm for 1.5 hours, and then sonicated at 100 Hz / min for 1.5 hours to ensure uniform dispersion, resulting in a PAN-MXene suspension used as the shell spinning solution. The shell spinning solution contained 13% PAN and 3% MXene by mass.

[0074] (2) Constructing a coaxial conjugate electrospinning device: Cotton yarn is wound as core yarn 7 on unwinding roller 8, and core yarn 7 is passed through the electrostatic field area and fixed on collection device 12 through the center of metal rotating funnel 9.

[0075] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0076] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0077] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured photothermal phase change nanofibers; the core-shell structured photothermal phase change nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured photothermal... The phase change nanofibers form a triangular pyramidal fiber network 10. The rotation of the metal rotating funnel 9 causes the fiber bundles to entangle evenly and coat the outer surface of the core yarn 7 to form an outer coating layer. Finally, a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer is formed on the collecting device 12. The nascent coated yarn is then dried at room temperature for 4 hours until all the solvent evaporates to obtain a photothermal phase change nanofiber coated yarn with an average diameter of 500 μm, wherein the mass ratio of the core-shell structure nanofibers 6 to the core yarn 7 is 0.4:1.

[0078] Depend on Figure 3 and Figure 4 It can be seen that the photothermal phase change nanofiber coated yarn prepared in Example 1 has a good structural morphology.

[0079] Depend on Figure 5 and Figure 6 It can be seen that the photothermal phase change nanofibers prepared in Example 1 are uniformly entangled and coated on the core yarn 7.

[0080] Depend on Figure 7 It can be seen that the photothermal phase change nanofiber coated yarn prepared in Example 1 has a good photothermal conversion effect.

[0081] Depend on Figure 8 It can be seen that the photothermal phase change nanofiber coated yarn prepared in Example 1 has good heat storage and temperature regulation performance.

[0082] Example 2:

[0083] (1) Preparation of core spinning solution and shell spinning solution;

[0084] Heating n-tetradecane crystals at 45°C for 1 hour yields a core spinning solution;

[0085] PAN was dissolved in DMF and heated at 60°C with stirring at 1000 rpm for 8 hours until completely dissolved, yielding a PAN solution. Then, dispersed graphene was added to the PAN solution, stirred at 1000 rpm for 1.5 hours, and then sonicated at 100 Hz / min for 1.5 hours to ensure uniform dispersion, resulting in a PAN-graphene suspension used as the shell spinning solution. The shell spinning solution contained 13% PAN and 3% graphene by mass.

[0086] (2) Constructing a coaxial conjugate electrospinning device: The polyester yarn is wound as the core yarn 7 on the unwinding roller 8, and the core yarn 7 is passed through the electrostatic field area and fixed on the collection device 12 through the center of the metal rotating funnel 9.

[0087] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0088] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0089] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured photothermal phase change nanofibers; the core-shell structured photothermal phase change nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured photothermal... The phase change nanofibers form a triangular pyramidal fiber network 10. The rotation of the metal rotating funnel 9 causes the fiber bundles to entangle and coat the outer surface of the core yarn 7 to form an outer coating layer. Finally, a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer is formed on the collecting device 12. The nascent coated yarn is then dried at room temperature for 5 hours until all the solvent evaporates to obtain a photothermal phase change nanofiber coated yarn with an average diameter of 450 μm, wherein the mass ratio of the core-shell structure nanofibers 6 to the core yarn 7 is 0.4:1.

[0090] Example 3:

[0091] (1) Preparation of core spinning solution and shell spinning solution;

[0092] Paraffin crystals were heated at 45°C for 0.5 h to obtain a core spinning solution;

[0093] PVDF was dissolved in a mixed solvent of DMF and acetone at a mass ratio of 7:3. The solution was heated at 60°C and stirred at 1000 rpm for 8 hours until completely dissolved, yielding a PVDF solution. Then, centrifuged and expanded MXene was added to the PVDF solution. The solution was stirred at 1000 rpm for 1.5 hours and then sonicated at 100 Hz / min for 1.5 hours to ensure uniform dispersion, resulting in a PVDF-MXene suspension used as the shell spinning solution. The shell spinning solution contained 12% PVDF and 3% MXene by mass.

[0094] (2) Constructing a coaxial conjugate electrospinning device: Nylon yarn is wound as core yarn 7 on unwinding roller 8, and core yarn 7 is passed through the electrostatic field area and fixed on collection device 12 through the center of metal rotating funnel 9.

[0095] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0096] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0097] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured photothermal phase change nanofibers; the core-shell structured photothermal phase change nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured photothermal... The phase change nanofibers form a triangular pyramidal fiber network 10. The rotation of the metal rotating funnel 9 causes the fiber bundles to entangle and coat the outer surface of the core yarn 7 to form an outer coating layer. Finally, a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer is formed on the collecting device 12. The nascent coated yarn is then dried at room temperature for 4 hours until all the solvent evaporates to obtain a photothermal phase change nanofiber coated yarn with an average diameter of 450 μm, wherein the mass ratio of the core-shell structure nanofibers 6 to the core yarn 7 is 0.3:1.

[0098] Example 4:

[0099] (1) Preparation of core spinning solution and shell spinning solution;

[0100] Polyethylene glycol crystals were heated at 45°C for 1 hour to obtain a core spinning solution;

[0101] PVDF was dissolved in a mixed solvent of DMF and acetone at a mass ratio of 7:3. The solution was heated at 60°C and stirred at 1000 rpm for 8 hours until completely dissolved, yielding a PVDF solution. Centrifugally dispersed graphene was added to the PVDF solution, stirred at 1000 rpm for 1.5 hours, and then sonicated at 100 Hz / min for 1.5 hours to ensure uniform dispersion, resulting in a PVDF-graphene suspension used as the shell spinning solution. The shell spinning solution contained 12% PVDF and 3% graphene by mass.

[0102] (2) Constructing a coaxial conjugate electrospinning device: The polyester-cotton yarn 7 is wound onto the unwinding roller 8, and the core yarn 7 is passed through the electrostatic field area and fixed on the collection device 12 through the center of the metal rotating funnel 9.

[0103] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0104] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0105] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured photothermal phase change nanofibers; the core-shell structured photothermal phase change nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured photothermal... The phase change nanofibers form a triangular pyramidal fiber network 10. The rotation of the metal rotating funnel 9 causes the fiber bundles to entangle and coat the outer surface of the core yarn 7 to form an outer coating layer. Finally, a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer is formed on the collecting device 12. The nascent coated yarn is then dried at room temperature for 4 hours until all the solvent evaporates to obtain a photothermal phase change nanofiber coated yarn with an average diameter of 500 μm, wherein the mass ratio of the core-shell structure nanofibers 6 to the core yarn 7 is 0.3:1.

[0106] Table 1

[0107]

[0108]

[0109] Table 1 shows the heat storage and temperature regulation performance of the photothermal phase change nanofiber coated yarn. As can be seen from Table 1, the photothermal phase change nanofiber coated yarn of the present invention has a good effect on thermal management.

[0110] Example 5:

[0111] (1) Preparation of core spinning solution and shell spinning solution;

[0112] The core spinning solution was obtained by heating n-octadecane crystals at 45°C for 0.5 h.

[0113] PVDF was dissolved in a mixed solvent of DMF and acetone at a mass ratio of 7:3. The solution was heated at 60°C and stirred at 1000 rpm for 8 hours until completely dissolved, yielding a PVDF solution. Subsequently, SiO2 was added to the PVDF solution in small amounts several times. The solution was first stirred at 1000 rpm for 1.5 hours, and then sonicated at 100 Hz / min for 1.5 hours to obtain a PVDF-SiO2 suspension, which was used as the shell spinning solution. The mass fraction of PVDF in the shell spinning solution was 10%, and the mass fraction of SiO2 was 5%.

[0114] (2) Constructing a coaxial conjugate electrospinning device: Cotton yarn is wound as core yarn 7 on unwinding roller 8, and core yarn 7 is passed through the electrostatic field area and fixed on collection device 12 through the center of metal rotating funnel 9.

[0115] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0116] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0117] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured passive radiation cooling nanofibers; the core-shell structured passive radiation cooling nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured passive radiation cooling nanofiber is formed. The fiber bundles of radiation-cooled nanofibers form a triangular pyramidal fiber network 10; the rotation of the metal rotating funnel 9 causes the fiber bundles to entangle evenly and coat the outer surface of the core yarn 7 to form an outer coating layer, and finally forms a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer on the collecting device 12; the nascent coated yarn is then dried at room temperature for 4 hours until all the solvent evaporates, to obtain a passive radiation-cooled nanofiber coated yarn with an average diameter of 400 μm, wherein the mass ratio of the core-shell structured nanofibers 6 to the core yarn 7 is 0.3:1.

[0118] Depend on Figure 9 and Figure 10 It can be seen that the prepared passive radiation cooling nanofiber coated yarn has a good morphology and structure.

[0119] Depend on Figure 11 It can be seen that the prepared passive radiation cooling nanofiber coated yarn has a good heat storage effect.

[0120] Depend on Figure 12 It can be seen that the prepared passive radiation cooling nanofiber coated yarn has a good cooling effect.

[0121] Example 6:

[0122] (1) Preparation of core spinning solution and shell spinning solution;

[0123] Heating n-tetradecane crystals at 45°C for 1 hour yields a core spinning solution;

[0124] PVDF was dissolved in a mixed solvent of DMF and acetone at a mass ratio of 7:3. The solution was heated at 60°C and stirred at 1000 rpm for 8 hours until completely dissolved, yielding a PVDF solution. Subsequently, ZnO was added to the PVDF solution in small amounts several times, first stirred at 1000 rpm for 1.5 hours, and then sonicated at 100 Hz / min for 1.5 hours to obtain a PVDF-ZnO suspension, which was used as the shell spinning solution. The mass fraction of PVDF in the shell spinning solution was 10%, and the mass fraction of ZnO was 5%.

[0125] (2) Constructing a coaxial conjugate electrospinning device: The polyester yarn is wound as the core yarn 7 on the unwinding roller 8, and the core yarn 7 is passed through the electrostatic field area and fixed on the collection device 12 through the center of the metal rotating funnel 9.

[0126] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0127] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0128] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured passive radiation cooling nanofibers; the core-shell structured passive radiation cooling nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured passive radiation cooling nanofiber is formed. The fiber bundles of radiation-cooled nanofibers form a triangular pyramidal fiber network 10; the rotation of the metal rotating funnel 9 causes the fiber bundles to entangle uniformly and coat the outer surface of the core yarn 7 to form an outer coating layer, and finally forms a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer on the collecting device 12; the nascent coated yarn is then dried at room temperature for 5 hours until all the solvent evaporates, to obtain a passive radiation-cooled nanofiber coated yarn with an average diameter of 400 μm, wherein the mass ratio of the core-shell structured nanofibers 6 to the core yarn 7 is 0.2:1.

[0129] Example 7:

[0130] (1) Preparation of core spinning solution and shell spinning solution;

[0131] Paraffin crystals were heated at 45°C for 0.5 h to obtain a core spinning solution.

[0132] PAN was dissolved in DMF and heated at 60°C with stirring at 1000 rpm for 8 hours until completely dissolved to obtain a PAN solution. Then, TiO2 was added to the PAN solution in small amounts several times, first stirred at 1000 rpm for 1.5 hours, and then sonicated at 100 Hz / min for 1.5 hours to obtain a PAN-TiO2 suspension, which was used as the shell spinning solution. The mass fraction of PAN in the shell spinning solution was 13%, and the mass fraction of TiO2 was 5%.

[0133] (2) Constructing a coaxial conjugate electrospinning device: Nylon yarn is wound as core yarn 7 on unwinding roller 8, and core yarn 7 is passed through the electrostatic field area and fixed on collection device 12 through the center of metal rotating funnel 9.

[0134] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0135] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0136] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured passive radiation cooling nanofibers; the core-shell structured passive radiation cooling nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured passive radiation cooling nanofiber is formed. The fiber bundles of radiation-cooled nanofibers form a triangular pyramidal fiber network 10; the rotation of the metal rotating funnel 9 causes the fiber bundles to entangle uniformly and coat the outer surface of the core yarn 7 to form an outer coating layer, and finally forms a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer on the collecting device 12; the nascent coated yarn is then dried at room temperature for 4 hours until all the solvent evaporates, to obtain a passive radiation-cooled nanofiber coated yarn with an average diameter of 500 μm, wherein the mass ratio of the core-shell structured nanofibers 6 to the core yarn 7 is 0.4:1.

[0137] Example 8:

[0138] (1) Preparation of core spinning solution and shell spinning solution;

[0139] Polyethylene glycol crystals were heated at 45°C for 1 hour to obtain a core spinning solution;

[0140] PAN was dissolved in DMF and heated at 60°C with stirring at 1000 rpm for 8 hours until completely dissolved, yielding a PAN solution. Then, BaSO4 was added to the PAN solution in small amounts several times, first stirred at 1000 rpm for 1.5 hours, and then sonicated at 100 Hz / min for 1.5 hours to ensure uniform dispersion, resulting in a PAN-BaSO4 suspension used as the shell spinning solution. The mass fraction of PAN in the shell spinning solution was 13%, and the mass fraction of BaSO4 was 3%.

[0141] (2) Constructing a coaxial conjugate electrospinning device: The polyester-cotton yarn 7 is wound onto the unwinding roller 8, and the core yarn 7 is passed through the electrostatic field area and fixed on the collection device 12 through the center of the metal rotating funnel 9.

[0142] (3) Preparation of nanofiber-coated yarn for personal thermal management 11;

[0143] The distance between the two coaxial needles 3 is 18 cm; the distance between the coaxial needle 3 and the metal rotating funnel 9 is 13 cm; the voltage of the positive electrode 4 is 6 kV, and the voltage of the negative electrode 5 is -6 kV; the propulsion rate of the shell spinning solution is 0.6 mL / h, and the propulsion rate of the core spinning solution is 0.15 mL / h; the moving speed of the core yarn 7 is 0.2 mm / s; the rotation speed of the metal rotating funnel 9 is 350 rpm; the spinning environment temperature is 25 ± 5℃, and the humidity is 40 ± 5%.

[0144] The shell spinning solution and the core spinning solution are respectively delivered to the shell channel 301 and the core channel 302 of the coaxial needle 3; the DC power supply is turned on to start spinning. During the spinning process, the core yarn 7 is in a straight state; under the action of the high voltage electric field, the spinning solution in the two coaxial needles 3 is stretched into a fibrous shape, forming core-shell structured passive radiation cooling nanofibers; the core-shell structured passive radiation cooling nanofibers are collected on a metal rotating funnel 9; at the opening of the metal rotating funnel 9, a multi-bundle core-shell structured passive radiation cooling nanofiber is formed. The fiber bundles of radiation-cooled nanofibers form a triangular pyramidal fiber network 10; the rotation of the metal rotating funnel 9 causes the fiber bundles to entangle uniformly and coat the outer surface of the core yarn 7 to form an outer coating layer, and finally forms a nascent coated yarn with the core yarn 7 as the core layer and the outer coating layer as the skin layer on the collecting device 12; the nascent coated yarn is then dried at room temperature for 5 hours until all the solvent evaporates, to obtain a passive radiation-cooled nanofiber coated yarn with an average diameter of 450 μm, wherein the mass ratio of the core-shell structured nanofibers 6 to the core yarn 7 is 0.3:1.

[0145] Table 2

[0146]

[0147]

[0148] Table 2 shows the heat storage and temperature regulation performance of the passive radiation cooling nanofiber-coated yarn. As can be seen from Table 2, the passive radiation cooling nanofiber-coated yarn of this invention has good thermal management effects.

[0149] Any aspects not covered in this invention are applicable to existing technologies.

Claims

1. A method for preparing nanofiber-coated yarns for personal thermal management using coaxial conjugate electrospinning, characterized in that, The method includes the following steps: Step 1: Prepare the core spinning solution and the shell spinning solution; The phase change material is heated and melted into a liquid state to obtain a core spinning solution; the phase change material is one of n-octadecane, n-tetradecane, polyethylene glycol or paraffin; The polymer is dissolved in an organic solvent to obtain a polymer solution; then the temperature-regulating material is added to the polymer solution and dispersed evenly to obtain a shell spinning solution; The temperature-regulating material is one of photothermal material or radiative cooling material; the polymer is PAN or PVDF; the photothermal material is Mxene or graphene; the radiative cooling material is one or more of TiO2, SiO2, BaSO4 or ZnO. In the shell spinning solution, the mass fraction of the polymer is 10-15%; the mass fraction of the photothermal material is 1-5%; and the mass fraction of the radiative cooling material is 2-8%. Step 2: Construct a coaxial conjugate electrospinning device; The device includes a shell spinning solution propeller (1), a core spinning solution propeller (2), a coaxial needle (3), a positive electrode (4), a negative electrode (5), an unwinding roller (8), a metal rotating funnel (9), and a collection device (12). The coaxial needle (3) has a coaxial structure with a core layer channel (302) and a shell layer channel (301), with the shell layer channel (301) nested outside the core layer channel (302); the shell layer spinning solution propeller (1) and the core layer spinning solution propeller (2) are both mounted on the coaxial needle (3); the shell layer spinning solution propeller (1) is connected to the shell layer channel (301) and pushes the shell layer spinning solution into the shell layer channel (301) during spinning; the core layer spinning solution propeller (2) is connected to the core layer channel (302) and pushes the core layer spinning solution into the core layer channel (302) during spinning. Along the forward direction of the core yarn (7), an unwinding roller (8), a metal rotating funnel (9), and a collecting device (12) are arranged in sequence; the core yarn (7) is wound on the unwinding roller (8), and the core yarn (7) is released during spinning; the collecting device (12) is used to collect the nanofiber coated yarn (11) for personal thermal management and control the moving speed of the core yarn (7); Two coaxial needles (3) are located on the same horizontal plane; the metal rotating funnel (9) is at the same distance from the two coaxial needles (3), located on the perpendicular plane between them, and within the range of the electrostatic field generated by the coaxial needles (3) when high voltage is applied; one of the two coaxial needles (3) is connected to the positive terminal (4) of the power supply, and the other is connected to the negative terminal (5) of the power supply, in order to generate an electrostatic field; the metal rotating funnel (9) can rotate along its own central axis; Step 3: Prepare nanofiber-coated yarn for personal thermal management (11); Set the spinning parameters; place the shell spinning solution in the shell spinning solution propeller (1) and the core spinning solution in the core spinning solution propeller (2); one end of the core yarn (7) is wound around the unwinding roller (8), passes through the metal rotating funnel (9), and the other end is wound around the collecting device (12). The core yarn (7) is pulled and moved by the collecting device (12). Coaxial conjugate electrospinning is initiated to achieve a core-shell structure nanofiber (6) with a core layer of phase change material and a shell layer of polymer and temperature-regulating functional material uniformly coated on the outside of the core yarn (7), forming a nascent coated yarn with the core yarn (7) as the core layer and the core-shell structure nanofiber (6) as the skin layer; the nascent coated yarn is then dried until all the solvent evaporates to obtain a nanofiber coated yarn (11) for personal thermal management. In step 3, the spinning parameters are as follows: the distance between the two coaxial needles (3) is 15~20cm; the distance between the coaxial needles (3) and the metal rotating funnel (9) is 12~15cm; the voltage of the positive electrode (4) is 5~7kV, and the voltage of the negative electrode (5) is -7~-5kV; the propulsion rate of the shell spinning solution is 0.4~0.7mL / h, and the propulsion rate of the core spinning solution is 0.1~0.2mL / h; the moving speed of the core yarn (7) is adjusted by adjusting the rotation speed of the collecting device (12) so that the collecting speed matches the spinning speed, and the moving speed of the core yarn (7) is 0.1~0.4mm / s; the rotation speed of the metal rotating funnel (9) is 300~500rpm; the spinning environment temperature is 25±5℃, and the humidity is 40±5%; In step 3, the mass ratio of core-shell structured nanofibers (6) to core yarn (7) is 0.2~0.5:1; In step 3, the average diameter of the nanofiber-coated yarn (11) for personal thermal management is 380~600µm.

2. The method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning according to claim 1, characterized in that, In step 1, the phase change material heating process is: heating at 40~50℃ for 0.5~1h.

3. The method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning according to claim 1, characterized in that, In step 1, the organic solvent is DMF and / or acetone; In step 1, the polymer dissolution process is as follows: stirring at 1000-2000 rpm for 6-10 hours at 60-70℃.

4. The method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning according to claim 1, characterized in that, In step 1, the particle size of the radiation cooling material is 80~1600nm; In step 1, the dispersion process of the temperature-regulating functional material is as follows: first, stir at a speed of 1000~2000 rpm for 1~2 hours, and then sonicate at 80~120 Hz / min for 1~2 hours.

5. The method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning according to claim 1, characterized in that, In step 2, the outer wall of the coaxial needle (3) is opened, and the shell spinning liquid propeller (1) is fixed at the opening on the outer wall of the coaxial needle (3) and communicates with the side wall of the shell channel (301).

6. The method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning according to claim 1, characterized in that, In step 2, the core yarn (7) is yarn; the metal rotating funnel (9) is trumpet-shaped.

7. The method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning according to claim 1, characterized in that, In step 3, the specific process of coaxial conjugate electrospinning is as follows: turn on the power and start spinning. During the spinning process, the core yarn (7) is in a straight state. Under the action of the high voltage electric field, the spinning solution in the two coaxial needles (3) is stretched into a fiber shape in the electric field, forming core-shell structured nanofibers (6) respectively. The oppositeity of positive and negative charges causes the core-shell structured nanofibers (6) spun by the two coaxial needles (3) to entangle with each other. At the same time, electrostatic induction will be generated between the two coaxial needles (3) and the metal rotating funnel (9), collecting the core-shell structured nanofibers (6) on the metal rotating funnel (9). Through the traction of the core yarn (7) on the electrospun fibers, a triangular pyramidal fiber web (10) formed by multiple core-shell structured nanofibers (6) is formed at the opening of the metal rotating funnel (9); through the stretching and traction of the core yarn (7) by the collecting device (12), the fiber bundles in the fiber web (10) are oriented; at the same time, the rotation of the metal rotating funnel (9) causes the fiber bundles to be evenly entangled and wrapped around the outer surface of the core yarn (7) to form an outer layer, and finally a new covered yarn with the core yarn (7) as the core layer and the outer layer as the skin layer is formed on the collecting device (12).

8. The method for preparing nanofiber-coated yarn for personal thermal management by coaxial conjugate electrospinning according to claim 1, characterized in that, In step 3, the drying process is as follows: dry in an indoor environment for at least 4 hours.

Citation Information

Patent Citations

  • Surgical suture and preparation method thereof

    CN117531037A

  • Electrostatic spinning preparation method of multifunctional composite nanofiber membrane

    CN119321021A