Multilayer polymeric piezoelectret materials and methods for their preparation
By employing a multilayer polymer piezoelectric electret material preparation method, fiber films and cast films are prepared using electrospinning and solution casting methods. The layers are stacked one by one and subjected to corona polarization treatment, which solves the problems of poor flexibility and low piezoelectric constant of existing piezoelectric electret materials and achieves high piezoelectric response and stability.
Patent Information
- Application Number
- CN202510416114.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-04-03
AI Technical Summary
Existing piezoelectric electret materials have poor flexibility and low piezoelectric constants, making it difficult to meet the requirements for flexibility and biocompatibility.
A method for preparing multilayer polymer piezoelectric electret materials was adopted, in which fiber films and cast films were prepared by electrospinning and solution casting, and then stacked layer by layer and subjected to corona polarization treatment to optimize mechanical and electrical properties.
It improves polarization efficiency and charge injection effect, enhances flexibility and mechanical strength, increases piezoelectric constant, extends electret lifetime and stability, and avoids interlayer peeling and mechanical damage.
Smart Images

Figure CN120206934B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of electret preparation methods, specifically relating to a method for preparing multilayer polymer piezoelectric electret materials, and also relating to multilayer polymer piezoelectric electret materials. Background Technology
[0002] With the rapid development of the Internet of Things (IoT), an increasing number of sensors are being applied in fields such as industrial manufacturing, medical and health care, security, and wearable devices, playing a crucial role in environmental monitoring, structural health monitoring, human health monitoring, human-machine interfaces, and motion analysis. Traditional rigid piezoelectric materials struggle to meet the requirements of flexibility and biocompatibility, driving the exploration of piezoelectric electrets. Therefore, developing a simple and effective method for preparing flexible piezoelectric electrets is of great significance. Currently used traditional single-process preparation methods all have certain limitations. For example, single-layer cast films are dense but brittle and prone to cracking; single-layer electrospun fiber films have good flexibility but low mechanical strength and are difficult to withstand high loads. Furthermore, the piezoelectric constant d... 33 The piezoelectric constants are relatively low (50-200 pC / N). Therefore, a method for preparing piezoelectric electrets with good flexibility, high mechanical strength, and high piezoelectric constant is needed. Summary of the Invention
[0003] The purpose of this invention is to provide a method for preparing multilayer polymer piezoelectric electret materials, thereby solving the problems of poor flexibility and low piezoelectric constant in existing piezoelectric electrets.
[0004] Another objective of this invention is to provide a multilayer polymer piezoelectric electret material.
[0005] The first technical solution adopted in this invention is: a method for preparing multilayer polymer piezoelectric electret materials, the specific operation steps of which are as follows: Step 1: Dissolve polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder and dopamine in N,N-dimethylformamide solvent and stir until homogeneous to obtain electrospinning solution; dissolve P (VDF-TrFE) in N,N-dimethylformamide solvent and stir until homogeneous to obtain casting solution; Step 2: Prepare fiber membranes by electrospinning and cast membranes by solution casting. Step 3: The cast film obtained by solution casting is coated on the surface of the fiber film, and then a multilayer P (VDF-TrFE) electret is obtained by alternating layers; Step 4: After single-sided gold sputtering on multilayer P(VDF-TrFE) electrets, corona polarization treatment is performed to obtain piezoelectric electret materials; Step 5: Test the piezoelectric constant d of the piezoelectric electret material after polarization. 33 .
[0006] The invention is further characterized in that, Furthermore, the molar ratios of vinylidene fluoride (VDF) and trifluoroethylene (TrFE) in the P(VDF-TrFE) powder used in step 1 are 80 / 20, 70 / 30, and 65 / 35, respectively.
[0007] Furthermore, the mass percentage of polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder in the electrospinning solution of step 1 is 13%-17%.
[0008] Furthermore, in step 3, the outermost layer of the multilayer P(VDF-TrFE) electret is a cast film, with a fiber film wrapped inside the cast film, and the total number of layers of the cast film and fiber film is not less than 3.
[0009] Furthermore, in step 1, the mass of dopamine is 1% of the mass of polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder; the mass percentage of polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder in the casting solution is 8%.
[0010] Furthermore, the electrospinning parameters for step 2 are as follows: voltage of 18-20kV, distance from needle to collecting roller of 10-15cm, electrospinning speed of 16.67μL / min, ambient temperature of 30-40℃, and humidity of 20%-30%.
[0011] Furthermore, in step 4, the polarization treatment voltage is 14-16kV and the polarization time is 10min; during the polarization process, the distance between the needle and the surface of the multilayer P (VDF-TrFE) electret is adjusted to 1cm-5cm.
[0012] The second technical solution adopted in this invention is: a multilayer polymer piezoelectric electret material, which is prepared according to the preparation method of multilayer polymer piezoelectric electret material.
[0013] The beneficial effects of this invention are: 1. Effectively improves polarization efficiency and charge injection effect The porous structure of the electrospun fiber membrane, serving as an intermediate layer, allows the high-voltage electric field during corona polarization to penetrate deeper into the material, promoting the directional alignment of dipoles in the P(VDF-TrFE) molecular chains, especially enhancing the β-phase transformation efficiency of the intermediate layer and adjacent cast layers. The high specific surface area and porous structure of the fiber membrane can act as charge trapping sites, capturing more injected ions or electrons during corona polarization, forming a stable space charge layer, and improving surface potential and polarization stability.
[0014] 2. Synergistic optimization of mechanical and electrical properties The outer cast film provides high density and tensile strength, preventing polarization or mechanical failure of the material during use; the middle fiber layer disperses stress through its porous structure, improving overall flexibility and fatigue resistance. The difference in dielectric constant between the cast layer and the fiber layer leads to interfacial polarization, forming an additional polarization electric field at the interface, further enhancing the overall piezoelectric response.
[0015] 3. Enhanced durability and stability The outer dense cast film can reduce charge escape caused by environmental humidity or mechanical deformation and extend the electret lifetime; the porous structure of the middle fiber layer uniformly disperses the polarization electric field and avoids the risk of breakdown caused by excessive local electric field.
[0016] 4. Corona polarization and multilayer thin film structure can effectively synergize. Corona polarization does not require high temperatures (traditional thermal polarization requires >100℃), avoiding interlayer delamination caused by differences in thermal expansion coefficients in multilayer structures; the non-contact nature of corona polarization avoids mechanical pressure damage to multilayer structures (such as contact electrode polarization which may cause fiber layer collapse); by adjusting the corona voltage, electrode distance and polarization time, the polarization depth and charge distribution can be optimized for structures with different numbers of layers. Attached Figure Description
[0017] Figure 1 This is a scanning electron microscope image of the P(VDF-TrFE) electrospun fiber membrane of the present invention; Figure 2 This is a scanning electron microscope image of the P(VDF-TrFE) electrospun fiber membrane of the present invention; Figure 3 The QT curve and d curve of the single-layer cast film sample prepared in Example 1 of this invention are measured. 33 value Figure 4 The QT curve and d curve of the single-layer electrospun fiber membrane sample prepared in Example 1 of this invention are measured. 33 value; Figure 5 The QT curve and d obtained from the 3-layer sample prepared in Example 1 of this invention are 33 value; Figure 6 The QT curve and d obtained from the sample prepared in Example 2 of this invention are 33 value; Figure 7 The QT curve and d obtained from the sample prepared in Example 3 of this invention are 33 value; Figure 8 The QT curve and d obtained from the sample prepared in Example 4 of this invention are 33 value; Figure 9 The QT curve and d obtained from the sample prepared in Example 5 of this invention are33 value; Figure 10 The QT curve and d obtained from the sample prepared in Example 6 of this invention are 33 value; Figure 11 The QT curve and d obtained from the sample prepared in Example 7 of this invention are 33 value. Detailed Implementation
[0018] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0019] Example 1 Step S1: Solution preparation; 1.8 g of P(VDF-TrFE) powder with a composition of 70 / 30 was dissolved in 12.6 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain an electrospinning solution with a P(VDF-TrFE) powder mass ratio of 13%; at the same time, 1.2 g of P(VDF-TrFE) powder was dissolved in 15 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain a solution for subsequent casting.
[0020] Step S2: Electrospinning to prepare fiber membranes and solution casting to prepare cast membranes; The electrospinning solution was transferred into a 10 mL syringe, and the electrospinning parameters were set as follows: voltage of 20 kV, distance from needle to collecting roller of 15 cm, electrospinning speed of 16.67 μL / min, ambient temperature of 30 ℃, and humidity of 20%. A fiber membrane was finally obtained on the collecting roller. The prepared solution was dropped onto a glass slide using a dropper to remove air bubbles and then placed in an oven. The solvent was evaporated at 70 ℃ for 3 hours, and the polymer was kept in a molten state at 170 ℃ for 2 hours. Finally, the slide was annealed at 120 ℃ for 12 hours to improve crystallinity, and a cast film was obtained.
[0021] Step S3: Stacking and corona polarization of multilayer P (VDF-TrFE) electrets.
[0022] Electrostatic adsorption forces remain on the fiber membrane after electrospinning. Two cast films obtained by solution casting are tightly attached to both sides of the fiber membrane to obtain a three-layer electret. The three-layer sample, the single-layer cast film, and the single-layer spun fiber membrane are then coated with gold on one side and placed in a corona polarization device. They are polarized at 15.4kV for 10 minutes. During the polarization process, the distance between the needle and the sample is adjusted appropriately to avoid breakdown.
[0023] Step S4: d of the polarized sample 33 test.
[0024] Two copper wires were drawn onto the polarized sample surface and encapsulated. The constructed testing system was then used for d-testing.33 The testing system of this invention mainly comprises three parts: a high-frequency exciter-force control module, an electrometer, and a host computer. The high-frequency exciter, connected to a signal generator and signal amplifier, can accurately achieve excitation forces of different frequencies and amplitudes. Combined with a pressure sensor diaphragm block assembly, it displays the magnitude of the excitation force in real time. The electrometer allows for immediate observation of charge change trends. The host computer allows for observation of real-time data curves (Qt curves) of charge versus time. Based on the charge and excitation force measured by the electrometer, the system uses formula d... 33 The piezoelectric constant d can be calculated using Q / F. 33 The test results for the single-layer cast film are as follows: Figure 3 d 33 The value is 150 pC / N; the test results for the single-layer electrospun fiber membrane are as follows: Figure 4 d 33 The value is 80 pC / N; the test results for the 3-layer sample are as follows: Figure 5 d 33 The value is 1800 pC / N; this demonstrates that increasing the number of piezoelectric electret layers can significantly increase the piezoelectric constant.
[0025] Example 2 Step S1: Solution preparation; 1.8 g of P(VDF-TrFE) powder with a composition of 70 / 30 and 0.018 g of dopamine were dissolved in 12.6 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain an electrospinning solution with a P(VDF-TrFE) powder content of 13% by mass. At the same time, 1.2 g of P(VDF-TrFE) powder was dissolved in 15 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain a solution for subsequent casting.
[0026] Step S2: Electrospinning to prepare fiber membranes and solution casting to prepare cast membranes; The electrospinning solution was transferred into a 10 mL syringe. The electrospinning parameters were set as follows: voltage 20 kV, needle-to-collecting roller distance 15 cm, electrospinning speed 16.67 μL / min, ambient temperature 30℃, and humidity 20%. A fiber membrane was finally obtained on the collecting roller. The fiber membrane was characterized using a scanning electron microscope. Figure 1 The prepared solution was dropped onto a glass slide using a dropper to remove air bubbles and then placed in an oven. The solvent was evaporated at 70 °C for 3 hours, and the polymer was kept in a molten state at 170 °C for 2 hours. Finally, the slide was annealed at 120 °C for 12 hours to improve crystallinity and obtain the cast film.
[0027] Step S3: Stacking and corona polarization of multilayer P (VDF-TrFE) electrets.
[0028] Electrostatic adsorption forces remain on the fiber membrane after electrospinning. Two cast films obtained by solution casting are tightly attached to both sides of the fiber membrane to obtain a 3-layer electret. The 3-layer sample is then sputter-coated with gold on one side and placed in a corona polarization device. It is polarized at 15.4kV for 10 minutes. During the polarization process, the distance between the needle and the sample is adjusted appropriately to avoid breakdown.
[0029] Step S4: d of the polarized sample 33 test.
[0030] Two copper wires were drawn onto the polarized sample surface and encapsulated. The test system built in Example 1 was used for d. 33 The test results are as follows Figure 6 d 33 The value is 3314 pC / N, indicating that the addition of dopamine increases the piezoelectric constant.
[0031] Example 3 Step S1: Solution preparation; 1.8 g of P(VDF-TrFE) powder with a composition of 80 / 20 and 0.018 g of dopamine were dissolved in 12.6 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain an electrospinning solution with a P(VDF-TrFE) powder content of 13% by mass. At the same time, 1.2 g of P(VDF-TrFE) powder was dissolved in 15 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain a solution for subsequent casting.
[0032] Step S2: Electrospinning to prepare fiber membranes and solution casting to prepare cast membranes; The electrospinning solution was transferred into a 10 mL syringe, and the electrospinning parameters were set as follows: voltage of 20 kV, distance from needle to collecting roller of 15 cm, electrospinning speed of 16.67 μL / min, ambient temperature of 30 ℃, and humidity of 20%. A fiber membrane was finally obtained on the collecting roller. The prepared solution was dropped onto a glass slide using a dropper to remove air bubbles and then placed in an oven. The solvent was evaporated at 70 ℃ for 3 hours, and the polymer was kept in a molten state at 170 ℃ for 2 hours. Finally, the slide was annealed at 120 ℃ for 12 hours to improve crystallinity, and a cast film was obtained.
[0033] Step S3: Stacking and corona polarization of multilayer P (VDF-TrFE) electrets.
[0034] Electrostatic adsorption forces remain on the fiber membrane after electrospinning. Two cast films obtained by solution casting are tightly attached to both sides of the fiber membrane to obtain a 3-layer electret. On this basis, one layer of spun fiber membrane and one layer of cast film are attached to obtain a 5-layer electret. The 5-layer sample is sputter-coated with gold on one side and placed in a corona polarization device and polarized at 15.4kV for 10 minutes. During the polarization process, the distance between the needle and the sample is adjusted appropriately to avoid breakdown.
[0035] Step S4: d of the polarized sample 33 test.
[0036] Two copper wires were drawn onto the polarized sample surface and encapsulated. The test system built in Example 1 was used for d. 33 The test results are as follows Figure 7 d 33 It is 1076 pC / N.
[0037] Example 4 Step S1: Solution preparation; 2.9 g of 70 / 30P (VDF-TrFE) powder and 0.029 g of dopamine were dissolved in 14.25 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain an electrospinning solution with a P (VDF-TrFE) powder concentration of 17%; at the same time, 1.2 g of P (VDF-TrFE) powder was dissolved in 15 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain a solution for subsequent casting.
[0038] Step S2: Electrospinning to prepare fiber membranes and solution casting to prepare cast membranes; The electrospinning solution was transferred into a 10 mL syringe. The electrospinning parameters were set as follows: voltage of 18 kV, distance from the needle to the collecting roller of 12 cm, electrospinning speed of 0.4 mL / h, ambient temperature of 30 °C, and humidity of 30%. A fiber membrane was finally obtained on the collecting roller. The prepared solution was dropped onto a glass slide using a dropper to remove air bubbles and then placed in an oven. The solvent was evaporated at 70 °C for 3 hours, and the polymer was kept in a molten state at 170 °C for 2 hours. Finally, the slide was annealed at 120 °C for 12 hours to improve crystallinity, and a cast film was obtained.
[0039] Step S3: Stacking and corona polarization treatment of multilayer P (VDF-TrFE) electrets Electrostatic adsorption forces remain on the fiber membrane after electrospinning. Two cast films obtained by solution casting are tightly attached to both sides of the fiber membrane to obtain a 3-layer electret. The 3-layer sample is then sputter-coated with gold on one side and placed in a corona polarization device. It is polarized at 15.4kV for 10 minutes. During the polarization process, the distance between the needle and the sample is adjusted appropriately to avoid breakdown.
[0040] Step S4: d of the polarized sample 33 test.
[0041] Two copper wires were drawn onto the polarized sample surface and encapsulated. The sample was then subjected to d-processing using equipment. 33 The test results are as follows Figure 8 d 33 It is 1882 pC / N.
[0042] Example 5 Step S1: Solution preparation; 2.9 g of 80 / 20P (VDF-TrFE) powder and 0.029 g of dopamine were dissolved in 14.25 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain an electrospinning solution with a P (VDF-TrFE) powder concentration of 17%; at the same time, 1.2 g of P (VDF-TrFE) powder was dissolved in 15 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain a solution for subsequent casting.
[0043] Step S2: Electrospinning to prepare fiber membranes and solution casting to prepare cast membranes; The electrospinning solution was transferred into a 10 mL syringe. The electrospinning parameters were set as follows: voltage of 18 kV, distance from the needle to the collecting roller of 12 cm, electrospinning speed of 0.4 mL / h, ambient temperature of 30 °C, and humidity of 30%. A fiber membrane was finally obtained on the collecting roller. The prepared solution was dropped onto a glass slide using a dropper to remove air bubbles and then placed in an oven. The solvent was evaporated at 70 °C for 3 hours, and the polymer was kept in a molten state at 170 °C for 2 hours. Finally, the slide was annealed at 120 °C for 12 hours to improve crystallinity, and a cast film was obtained.
[0044] Step S3: Stacking and corona polarization treatment of multilayer P (VDF-TrFE) electrets Electrostatic adsorption forces remain on the fiber membrane after electrospinning. Two cast films obtained by solution casting are tightly attached to both sides of the fiber membrane to obtain a 3-layer electret. On this basis, one layer of spun fiber membrane and one layer of cast film are attached to obtain a 5-layer electret. The 5-layer sample is sputter-coated with gold on one side and placed in a corona polarization device and polarized at 15.4kV for 10 minutes. During the polarization process, the distance between the needle and the sample is adjusted appropriately to avoid breakdown.
[0045] Step S4: d of the polarized sample 33 test.
[0046] Two copper wires were drawn onto the polarized sample surface and encapsulated. The sample was then subjected to d-processing using equipment. 33 The test results are as follows Figure 9 d 33 It is 1112pC / N.
[0047] Example 6 Step S1: Solution preparation.
[0048] 1.8 g of P(VDF-TrFE) powder with a composition of 65 / 35 and 0.018 g of dopamine were dissolved in 12.6 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain an electrospinning solution with a P(VDF-TrFE) powder content of 13% by mass. At the same time, 1.2 g of P(VDF-TrFE) powder was dissolved in 15 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain a solution for subsequent casting.
[0049] Step S2: Electrospinning to prepare fiber membranes and solution casting to prepare cast membranes; The electrospinning solution was transferred into a 10 mL syringe. The electrospinning parameters were set as follows: voltage of 18 kV, distance from the needle to the collecting roller of 12 cm, electrospinning speed of 0.4 mL / h, ambient temperature of 30 °C, and humidity of 30%. A fiber membrane was finally obtained on the collecting roller. The prepared solution was dropped onto a glass slide using a dropper to remove air bubbles and then placed in an oven. The solvent was evaporated at 70 °C for 3 hours, and the polymer was kept in a molten state at 170 °C for 2 hours. Finally, the slide was annealed at 120 °C for 12 hours to improve crystallinity, and a cast film was obtained.
[0050] Step S3: Stacking and corona polarization treatment of multilayer P (VDF-TrFE) electrets Electrostatic adsorption forces remain on the fiber membrane after electrospinning. Two cast films obtained by solution casting are tightly attached to both sides of the fiber membrane to obtain a 3-layer electret. The 3-layer electret is then sputter-coated with gold on one side and placed in a corona polarization device. It is polarized at 15.4kV for 10 minutes. During the polarization process, the distance between the needle and the sample is adjusted appropriately to avoid breakdown.
[0051] Step S4: d of the polarized sample 33 test.
[0052] Two copper wires were drawn onto the polarized sample surface and encapsulated. The sample was then subjected to d-processing using equipment. 33 The test results are as follows Figure 10 d 33 It is 1645pC / N.
[0053] Example 7 Step S1: Solution preparation; 2.9 g of 65 / 35P (VDF-TrFE) powder and 0.029 g of dopamine were dissolved in 14.25 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain an electrospinning solution with a P (VDF-TrFE) powder concentration of 17%; at the same time, 1.2 g of P (VDF-TrFE) powder was dissolved in 15 mL of N,N-dimethylformamide solvent and stirred for 12 h to obtain a solution for subsequent casting.
[0054] Step S2: Electrospinning to prepare fiber membranes and solution casting to prepare cast membranes; The electrospinning solution was transferred into a 10 mL syringe. The electrospinning parameters were set as follows: voltage of 18 kV, distance from the needle to the collecting roller of 12 cm, electrospinning speed of 0.4 mL / h, ambient temperature of 30 °C, and humidity of 30%. A fiber membrane was finally obtained on the collecting roller. The prepared solution was dropped onto a glass slide using a dropper to remove air bubbles and then placed in an oven. The solvent was evaporated at 70 °C for 3 hours, and the polymer was kept in a molten state at 170 °C for 2 hours. Finally, the slide was annealed at 120 °C for 12 hours to improve crystallinity, and a cast film was obtained.
[0055] Step S3: Stacking and corona polarization treatment of multilayer P (VDF-TrFE) electrets Electrostatic adsorption forces remain on the fiber membrane after electrospinning. Two cast films obtained by solution casting are tightly attached to both sides of the fiber membrane to obtain a 3-layer electret. On this basis, one layer of spun fiber membrane and one layer of cast film are attached to obtain a 5-layer electret. The 5-layer sample is sputter-coated with gold on one side and placed in a corona polarization device and polarized at 15.4kV for 10 minutes. During the polarization process, the distance between the needle and the sample is adjusted appropriately to avoid breakdown.
[0056] Step S4: d of the polarized sample 33 test.
[0057] Two copper wires were drawn onto the polarized sample surface and encapsulated. The sample was then subjected to d-processing using equipment. 33 The test results are as follows Figure 11 d 33 It is 1063 pC / N.
[0058] This invention includes solution preparation, preparation of electrospun fiber membranes and solution casting membranes, stacking of multilayer electrets and corona polarization treatment, encapsulation, and d-electret preparation. 33 The process includes testing and other steps. The prepared multilayer piezoelectric electret material not only integrates the advantages of single-layer electret materials, exhibiting better flexibility and mechanical strength, but also demonstrates a higher piezoelectric response.
[0059] Figure 1This is a scanning electron microscope image of the P(VDF-TrFE) electrospun fiber membrane of the present invention, magnified at 1000x. The fiber network is intact and has no obvious defects. Figure 2 The magnification is 4000 times, and the fiber diameter is relatively uniform.
[0060] In summary, the present invention utilizes multilayer stacking and polarization of fiber membranes and cast membranes prepared by electrospinning and solution casting methods to prepare P(VDF-TrFE) electrets, which have the characteristics of good flexibility, high mechanical strength, and good piezoelectric response. The technical effect is best when the molar ratio of polyvinylidene fluoride to trifluoroethylene in P(VDF-TrFE) powder is 70 / 30.
[0061] The above are only some embodiments of the present invention. For those skilled in the art, any improvements and modifications made to the present invention without departing from the principle of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing multilayer polymer piezoelectric electret materials, characterized in that, The specific steps are as follows: Step 1: Dissolve polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder and dopamine in N,N-dimethylformamide solvent and stir until homogeneous to obtain electrospinning solution; dissolve P (VDF-TrFE) in N,N-dimethylformamide solvent and stir until homogeneous to obtain casting solution; The molar ratio of vinylidene fluoride (VDF) to trifluoroethylene (TrFE) in the P(VDF-TrFE) powder used in step 1 is any one of 80 / 20, 70 / 30, or 65 / 35; The mass percentage of polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder in the electrospinning solution described in step 1 is 13%-17%. The mass of dopamine in step 1 is 1% of the mass of polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder; the mass percentage of polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE) powder in the casting solution is 8%. Step 2: Prepare fiber membranes by electrospinning and cast membranes by solution casting. Step 3: The cast film obtained by solution casting method is applied to the surface of the fiber film, and then layered alternately to obtain a multilayer P (VDF-TrFE) electret. The outermost layer of the multilayer P(VDF-TrFE) electret described in step 3 is a cast film, with a fiber film wrapped inside the cast film. The total number of layers of the cast film and the fiber film is not less than 3. Step 4: After single-sided gold sputtering on multilayer P(VDF-TrFE) electrets, corona polarization treatment is performed to obtain piezoelectric electret materials; Step 5: Test the piezoelectric constant d of the piezoelectric electret material after polarization. 33 .
2. The method for preparing the multilayer polymer piezoelectric electret material according to claim 1, characterized in that, The electrospinning parameters in step 2 are as follows: voltage 18-20kV, distance from needle to collecting roller 10-15cm, electrospinning speed 16.67μL / min, ambient temperature 30-40℃, and humidity 20%-30%.
3. The method for preparing the multilayer polymer piezoelectric electret material according to claim 1, characterized in that, The polarization treatment voltage in step 4 is 14-16kV, and the polarization time is 10min.
4. The method for preparing the multilayer polymer piezoelectric electret material according to claim 3, characterized in that, During polarization, adjust the distance between the needle tip and the surface of the multilayer P (VDF-TrFE) electret to 1cm-5cm.
5. A multilayer polymer piezoelectric electret material, characterized in that, The multilayer polymer piezoelectric electret material is prepared according to any one of claims 1 to 4.
Citation Information
Patent Citations
Method for preparing high-dielectric and high-energy storage nanocomposite material
CN107901523A
Silk fibroin fiber membrane with electret effect and application thereof
CN108744056A
Preparation method of synergistically doped modified polyvinylidene fluoride piezoelectric nano-generator
CN112468018A