Method for preparing flexible thin film of highly oriented graphene aggregates for electromagnetic shielding

By preparing flexible films of highly oriented graphene aggregates through confined growth and mechanical pressing, the problems of high cost and defects in traditional graphene film preparation are solved, and the high conductivity and electromagnetic shielding performance are improved, making them suitable for small and ultra-thin devices.

CN120229713BActive Publication Date: 2026-11-24YANSHAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510399455.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-01
Publication Date
2026-11-24
Estimated Expiration
2045-04-01

AI Technical Summary

Technical Problem

Existing methods for preparing graphene films are costly and complex, and the defects and impurities caused by traditional methods are difficult to remove, which affects their application value in the field of electromagnetic shielding.

Method used

Highly oriented graphene aggregates were grown in a confined growth container, and combined with high-temperature impurity removal and mechanical pressing to prepare a flexible film of highly oriented graphene aggregates.

Benefits of technology

A graphene aggregate film with high conductivity and excellent electromagnetic wave shielding performance has been developed for low-cost, large-scale production and adjustable thickness, making it suitable for small, ultra-thin devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120229713B_ABST
    Figure CN120229713B_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing a flexible film of highly oriented graphene aggregates for electromagnetic shielding. The method employs a confined growth container for orientation and confinement, thereby obtaining highly oriented, directionally grown graphene aggregates. This, combined with simple subsequent mechanical pressing, yields a flexible film of highly oriented graphene aggregates. The method is simple, low-cost, and has potential advantages for large-scale production. The directionally grown graphene aggregates obtained in this invention can be completely removed from the impurities introduced during the preparation process by temperature treatment, thereby maximizing the intrinsic high conductivity of graphene. Compared to traditional electromagnetic shielding materials, the flexible film of highly oriented graphene aggregates prepared by this invention maintains excellent conductivity while exhibiting excellent flexibility, with a maximum conductivity of 4.072 × 10⁻⁶. 5 It has a high S / m and excellent electromagnetic wave shielding performance, which can be stably maintained at around 105dB in the 8-12Hz range, while also having good shielding bandwidth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electromagnetic shielding film technology, specifically to a method for preparing a flexible film of highly oriented graphene aggregates for electromagnetic shielding. Background Technology

[0002] With the rapid development of 5G digital cellular networks, the application of electromagnetic waves, primarily in the GHz range, has brought great convenience to our lives. However, the widespread use of wireless communication devices and electronic components has also exacerbated the problem of electromagnetic interference (EMI), seriously affecting the normal operation and health of interfered electronic devices and living organisms. Therefore, protective measures against electromagnetic interference are crucial, directly driving the rapid development of electromagnetic shielding films. Using highly conductive materials as shielding materials generates a large number of free charges, forming continuous conductive paths on the dielectric surface. These charges interact with the EMI and generate an induced counter-field, causing strong reflection of electromagnetic waves and achieving a shielding effect. Therefore, the development of highly conductive electromagnetic shielding materials has received widespread attention.

[0003] Graphene nanosheets, as an emerging sp2 two-dimensional material, possess extremely high conductivity. How to assemble graphene into macroscopic graphene films to fully utilize its high conductivity for EMI shielding has attracted widespread attention. Methods such as CVD, wet assembly of graphene oxide combined with high-temperature / chemithermal reduction, and graphite interlayer compounds combined with high-temperature exfoliation / ultrasonic dispersion with dispersants have all proven successful in preparing and assembling graphene films and applying them to electromagnetic shielding. However, these methods still suffer from high costs and complex processes, increasing the cost of large-scale production and application of graphene films. More importantly, the preparation of traditional graphene films often suffers from significant defects caused by ultrasonic exfoliation and difficulty in removing impurities and solvents, which severely affects the intrinsic high conductivity of graphene and its application value in the field of electromagnetic shielding.

[0004] Graphene aggregates, as a macroscopic 3D graphene structure, can be obtained through simple oxidation intercalation and interlayer exfoliation. Graphene in aggregate form can retain its intrinsic high conductivity while avoiding the high concentration defects and additional impurity solvents introduced by excessive oxidation. This avoids the problems that are common in the current assembly of graphene films. Therefore, it is particularly important to find out how to use graphene aggregates as assembly monomers for directional alignment and combine them with mechanical pressing to prepare macroscopic graphene films in order to improve the serious problems of current traditional graphene films. Summary of the Invention

[0005] This invention provides a flexible film of highly oriented graphene aggregates for electromagnetic shielding, its preparation method, and its application, in order to solve the problems mentioned in the background art.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] This invention provides a method for preparing a flexible film of highly oriented graphene aggregates, comprising the following steps: Step (1) mixing raw graphite, persulfate and concentrated sulfuric acid to obtain a slurry; placing the slurry in a confined growth container in a flat manner and allowing it to react statically to obtain oriented graphene aggregates; Step (2) removing residual chemical reagents from the oriented graphene aggregates by high-temperature impurity removal to obtain oriented graphene aggregate foam; Step (3) mechanically pressing the oriented graphene aggregate foam to obtain the flexible film of highly oriented graphene aggregates.

[0008] Furthermore, the volume-to-mass ratio of the original graphite to persulfate and concentrated sulfuric acid in step (1) is 1-3 g: 3-5 g: 1-2 mL.

[0009] Furthermore, in step (1), the original graphite is flake graphite or block graphite; the persulfate includes potassium persulfate and / or ammonium persulfate.

[0010] Furthermore, the confined growth container mentioned in step (1) is specifically a cylindrical and hollow quartz container. The bottom of the container has several circular holes evenly distributed. After depositing slurry at the bottom of the container, quartz discs are horizontally covered on the surface of the slurry. Preferably, the specific dimensions of the container are a bottom diameter of 30 mm and a height of 20 mm; the size of the circular holes is a diameter of 0.5 mm; the size of the quartz discs includes a diameter of 30 mm and a thickness of 0.5 mm, 1 mm, 1.5 mm, 2 mm, or 2.5 mm.

[0011] Furthermore, the spreading described in step (1) specifically includes: spinning the slurry at a speed of 3000 to 4000 rpm for 15 to 30 seconds, and then vacuum filtering it for 3 to 5 seconds through the pre-reserved circular hole at the bottom of the growth container at a pressure of -0.1 MPa.

[0012] Furthermore, the static reaction described in step (1) is specifically carried out at a temperature of 25℃~80℃ for 7h~24h.

[0013] Furthermore, the high-temperature purification described in step (2) specifically includes: heating from 25°C to 450°C, 550°C or 650°C at a heating rate of 7°C / min in an argon atmosphere, and holding at that temperature for 90 minutes.

[0014] Furthermore, the mechanical pressing described in step (3) specifically involves holding the pressure at 15–30 MPa for 60 minutes.

[0015] The present invention also provides a highly oriented graphene aggregate flexible film prepared by the above-described method for preparing highly oriented graphene aggregate flexible films.

[0016] The present invention also provides the application of the above-mentioned highly oriented graphene aggregate flexible film in the field of electromagnetic shielding.

[0017] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows:

[0018] The present invention provides a method for preparing highly oriented graphene aggregate flexible films, which uses a confined growth container for orientation and confinement, thereby obtaining highly oriented, oriented graphene aggregates. Combined with subsequent simple mechanical pressing, highly oriented graphene aggregate flexible films can be obtained. The preparation method is simple, low-cost, and has potential advantages for large-scale production.

[0019] In this invention, the directionally grown graphene aggregates obtained can be completely freed from impurities introduced during the preparation process by combining temperature treatment, thereby maximizing the intrinsic high conductivity of graphene. Compared to traditional electromagnetic shielding materials, the highly oriented graphene aggregate flexible film prepared in this invention maintains excellent conductivity while possessing extremely high flexibility, with a maximum conductivity of up to 4.072 × 10⁻⁶. 5 It has a high S / m and excellent electromagnetic wave shielding performance, which can be stably maintained at around 105dB in the 8-12Hz range, while also having a good shielding bandwidth.

[0020] This invention broadens the applications of graphene aggregates and enhances their practical value. Highly oriented graphene aggregates obtained through confined growth possess high density, and mechanical pressing yields a highly compacted graphene layered structure, endowing the film with extremely high conductivity and EMI SE capability. The highly oriented graphene aggregate foam obtained in this invention can be mechanically pressed into graphene aggregate films. Compared to traditional graphene assembly methods, this avoids mechanical ultrasonic processing, preserves the large-size structure of graphene, and maximizes its high conductivity advantage.

[0021] The highly oriented graphene aggregate flexible film developed in this invention, obtained by combining highly oriented confined growth with mechanical pressing, can have its thickness controlled to be only between 40 and 60 micrometers, fully meeting the practical application requirements of small, ultra-thin devices. By adjusting the size of the confined growth container, the thickness of the highly oriented graphene aggregate flexible film can be controlled to suit different application scenarios. Attached Figure Description

[0022] One or more embodiments are illustrated by way of example with reference to the accompanying drawings. These illustrations do not constitute a limitation on the embodiments, and unless otherwise stated, the figures in the drawings are not to be limited by scale.

[0023] Figure 1 These are SEM images of the GAs pressed films prepared in Examples 1 and 2 of this invention.

[0024] Figure 2 A comparison of the conductivity of the GAS pressed films prepared in Examples 1 and 2 of the present invention;

[0025] Figure 3 A comparison of the Raman spectra of directionally grown GAs foams in Examples 1 and 3 of this invention;

[0026] Figure 4 A comparison of the conductivity of mechanically pressed GAs thin films prepared in Examples 1 and 4 of this invention.

[0027] Figure 5 Comparison of EMI SE of GAs pressed films in Examples 1 and 5 of the present invention;

[0028] Figure 6 This is a comparison of SEM images of the GAs foam cross sections in Examples 1 and 6 of the present invention. Detailed Implementation

[0029] In view of the problems existing in the prior art, the present invention provides a flexible film of highly oriented graphene aggregates for electromagnetic shielding, its preparation method and application.

[0030] One method for preparing a flexible thin film of highly oriented graphene aggregates includes the following steps:

[0031] Step 1: Mix persulfate, concentrated sulfuric acid, and raw graphite evenly to form a slurry. Then, transfer the slurry to a confined growth container and horizontally cover the slurry surface with quartz discs as a confinement method. At the same time, vacuum filter through the pre-reserved circular hole at the bottom of the container to promote the deposition and spreading of raw graphite in the slurry. Transfer the reaction system to a specific temperature and let it stand. After room temperature exfoliation, directionally grown graphene aggregates are obtained.

[0032] Step 2: Transfer the directionally grown graphene aggregates to an argon environment and treat them at high temperature to remove residual impurities to obtain directionally grown graphene aggregate foam.

[0033] Step 3: Mechanically press and hold the directionally grown graphene aggregate foam to obtain a highly oriented graphene aggregate shielding film.

[0034] In step 1, the persulfate is potassium persulfate or ammonium persulfate; the original graphite can be flake graphite.

[0035] The amounts used in step 1 are: 1g of flake graphite, 3g of persulfate, and 2mL of concentrated sulfuric acid.

[0036] In step 1, the confined growth container is a quartz growth container with 30 circular holes (0.5 mm in diameter) distributed at the bottom, a bottom diameter of 30 mm, a height of 20 mm, and circular quartz discs with a diameter of 30 mm and a thickness of 0.5 mm, 1 mm, 1.5 mm, 2 mm, or 2.5 mm that are vertically covered on the material surface.

[0037] In step 1, the auxiliary methods for spreading the graphite raw material are spin coating (3000-4000 rpm) and vacuum deposition spreading (-0.1 MPa).

[0038] In step 2, the high-temperature condition is to start at 25°C, raise the temperature to 350°C, 450°C, 550°C or 650°C at a rate of 7°C / min, and hold the temperature for 90 minutes.

[0039] In step 3, the mechanical pressing conditions are an arbitrary pressure of 15-30 MPa and a holding pressure of 60 min.

[0040] The present invention will now be described in detail with reference to specific embodiments.

[0041] Example 1:

[0042] A method for preparing a flexible thin film of highly oriented graphene aggregates includes the following steps:

[0043] First, mix 1g of flake graphite, 3g of ammonium persulfate and 2mL of concentrated sulfuric acid to form a mixed slurry.

[0044] The slurry was transferred into a confined growth vessel, spin-coated at 3000 rpm, and vacuum filtered at -0.1 MPa to assist in slurry deposition.

[0045] The reaction vessel was transferred to room temperature (25°C) and allowed to stand at room temperature for peeling. The C-axis confined quartz disc was slowly lifted, and after 24 hours, directionally grown graphene aggregates were obtained.

[0046] The obtained graphene aggregates were heated in an argon atmosphere from an initial temperature of 25°C to 350°C at a rate of 7°C / min, and held at the target temperature for 90 minutes to obtain highly oriented graphene aggregate foam.

[0047] The obtained graphene aggregate foam was mechanically pressed at 30 MPa and held for 60 minutes to obtain a highly oriented graphene aggregate film.

[0048] from Figure 1As can be seen from the right, the GAS pressed film pressed at 30 MPa has good density, the interlayer structure is highly ordered, and the surface is flat without any bumps or unevenness.

[0049] from Figure 2 It can be seen that the high pressure of 30 MPa can effectively promote the conductivity of the GAS pressed film;

[0050] from Figure 3 It can be seen that the GAS foam obtained by high-temperature purification under argon atmosphere has good structural integrity and a very low degree of overall defects;

[0051] from Figure 4 It can be seen that a purification temperature of 350℃ can maximize the removal of strong acid / oxidant impurities in the stripping system, thereby maximizing the intrinsic high conductivity of the film.

[0052] from Figure 5 It can be seen that the 1:3:2 stripping system ratio can fully strip NG into GAs, thereby maximizing the electromagnetic shielding performance of the subsequent pressing film, and can reach the 105dB level.

[0053] from Figure 6 It can be seen that after applying the confinement effect along the C-axis, GAs exhibit a highly oriented growth state overall.

[0054] Example 2:

[0055] A method for preparing a flexible thin film of highly oriented graphene aggregates includes the following steps:

[0056] First, mix 1g of flake graphite, 3g of ammonium persulfate and 2mL of concentrated sulfuric acid to form a mixed slurry.

[0057] The slurry was transferred into a confined growth vessel, spin-coated at 3000 rpm, and vacuum filtered at -0.1 MPa to assist in slurry deposition.

[0058] The reaction vessel was transferred to room temperature (25°C) and allowed to stand at room temperature for peeling. The confined quartz discs covering the slurry surface were slowly lifted up, and directionally grown graphene aggregates were obtained after 24 hours.

[0059] The obtained graphene aggregates were heated in an argon atmosphere from an initial temperature of 25°C to 350°C at a rate of 7°C / min, and held at the target temperature for 90 minutes to obtain highly oriented graphene aggregate foam.

[0060] The obtained graphene aggregate foam was mechanically pressed at 10 MPa and held for 60 minutes to obtain a highly oriented graphene aggregate film.

[0061] from Figure 1As can be seen from the left, due to the lower mechanical pressure applied in the vertical direction, the film exhibits significantly larger interlayer porosity and a certain degree of orientation, but lower density, indicating that pressure plays an important role in the film structure during mechanical pressing.

[0062] Example 3:

[0063] A method for preparing a flexible thin film of highly oriented graphene aggregates includes the following steps:

[0064] First, mix 1g of flake graphite, 3g of ammonium persulfate and 3mL of concentrated sulfuric acid to form a mixed slurry.

[0065] The slurry was transferred into a confined growth vessel, spin-coated at 3000 rpm, and vacuum filtered at -0.1 MPa to assist in slurry deposition.

[0066] The reaction vessel was transferred to a room temperature (25°C) environment and allowed to stand at room temperature for peeling. The quartz discs covering the slurry surface were slowly lifted up, and after 24 hours, directionally grown graphene aggregates were obtained.

[0067] The obtained graphene aggregates were gradually heated from an initial temperature of 25°C to 350°C in air at a rate of 7°C / min, and then held at the target temperature for 90 minutes to obtain highly oriented graphene aggregate foam.

[0068] The obtained graphene aggregate foam was mechanically pressed at 10 MPa and held for 60 minutes to obtain a highly oriented graphene aggregate film.

[0069] from Figure 3 It can be seen that, since the purification atmosphere is air, the presence of oxygen at high temperature causes certain oxidative damage to the GAS foam structure, which indirectly leads to a significant increase in the D peak of the Raman spectrum.

[0070] Example 4:

[0071] A method for preparing a flexible thin film of highly oriented graphene aggregates includes the following steps:

[0072] First, mix 1g of flake graphite, 3g of ammonium persulfate and 2mL of concentrated sulfuric acid to form a mixed slurry.

[0073] The slurry was transferred into a confined growth vessel, spin-coated at 3000 rpm, and vacuum filtered at -0.1 MPa to assist in slurry deposition.

[0074] The reaction vessel was transferred to a room temperature (25°C) environment and allowed to stand at room temperature for peeling. The quartz discs covering the slurry surface were slowly lifted up, and after 24 hours, directionally grown graphene aggregates were obtained.

[0075] The obtained graphene aggregates were heated in air at a rate of 7°C / min from an initial temperature of 25°C to 150°C, and then held at the target temperature for 90 minutes to obtain highly oriented graphene aggregate foam.

[0076] The obtained graphene aggregate foam was mechanically pressed at 30 MPa and held for 60 minutes to obtain a highly oriented graphene aggregate film.

[0077] Depend on Figure 4 It can be seen that due to the low purification temperature (150℃), the residual oxidant on the surface of the GAs foam was not fully removed. After remaining in the interlayer, it had a significant negative impact on the conductivity of the constructed GAs film. This indicates that the purification temperature plays an important role in demonstrating the high conductivity of the film.

[0078] Example 5:

[0079] A method for preparing a flexible thin film of highly oriented graphene aggregates includes the following steps:

[0080] First, mix 1g of flake graphite, 1g of ammonium persulfate and 3mL of concentrated sulfuric acid to form a mixed slurry.

[0081] The slurry was transferred into a confined growth vessel, spin-coated at 3000 rpm, and vacuum filtered at -0.1 MPa to assist in slurry deposition.

[0082] The reaction vessel was transferred to an Ar (25°C) environment and allowed to stand at room temperature for peeling. The quartz discs covering the slurry surface were slowly lifted up, and after 24 hours, directionally grown graphene aggregates were obtained.

[0083] The obtained graphene aggregates were gradually heated from an initial temperature of 25°C to 450°C in air at a rate of 7°C / min, and then held at the target temperature for 90 minutes to obtain highly oriented graphene aggregate foam.

[0084] The obtained graphene aggregate foam was mechanically pressed at 30 MPa and held for 60 min to obtain a highly oriented graphene aggregate film.

[0085] from Figure 5 It can be seen that, due to the low content of oxidant in the oxidative stripping system, the sheet stripping of GAs cannot be fully completed, resulting in a significant decrease in the EMI SE performance of the constructed film.

[0086] Example 6:

[0087] A method for preparing a flexible thin film of highly oriented graphene aggregates includes the following steps:

[0088] First, mix 1g of flake graphite, 3g of ammonium persulfate and 3mL of concentrated sulfuric acid to form a mixed slurry.

[0089] The slurry is transferred into a confined growth vessel without any additional auxiliary deposition treatment.

[0090] The reaction vessel was transferred to an Ar (25°C) environment and allowed to stand at room temperature for peeling. The quartz discs covering the slurry surface were slowly lifted up, and after 24 hours, directionally grown graphene aggregates were obtained.

[0091] The obtained graphene aggregates were gradually heated from an initial temperature of 25°C to 450°C in air at a rate of 7°C / min, and then held at the target temperature for 90 minutes to obtain highly oriented graphene aggregate foam.

[0092] The obtained graphene aggregate foam was mechanically pressed at 10 MPa and held for 60 minutes to obtain a highly oriented graphene aggregate film.

[0093] Depend on Figure 6 As shown in b, due to the lack of confinement by the quartz discs covering the slurry surface, GAs exhibited significant orientation disorder during the growth and exfoliation process, failing to construct highly oriented GAs foam. This indicates that the confinement effect of the C-axis plays a crucial role in obtaining GAs foam through the highly oriented confined growth method. Figure 6 After confined quartz discs were coated on the surface of the slurry, GAs foam with obvious orientation was obtained.

[0094] Those skilled in the art will understand that the above embodiments are specific examples of implementing the present invention, and in practical applications, various changes in form and detail can be made without departing from the spirit and scope of the present invention. Any person skilled in the art can make their own modifications and alterations without departing from the spirit and scope of the present invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding, characterized in that, Includes the following steps: Step (1): Mix raw graphite, persulfate and concentrated sulfuric acid to obtain a slurry; place the slurry in a confined growth container in a flat manner and allow it to react statically to obtain directionally grown graphene aggregates; the confined growth container is specifically a cylindrical and hollow quartz container with several circular holes evenly distributed at the bottom of the container, and after the slurry is deposited at the bottom of the container, quartz discs are horizontally covered on the surface of the slurry. Step (2): Remove the residual chemical reagents in the directionally grown graphene aggregates by high-temperature impurity removal to obtain directionally grown graphene aggregate foam. Step (3): Mechanically press the oriented graphene aggregate foam to obtain the highly oriented graphene aggregate flexible film.

2. The method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding according to claim 1, characterized in that, The original graphite, persulfate, and concentrated sulfuric acid mentioned in step (1) are in the ratio of 1~3g: 3~5g: 1~2mL.

3. The method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding according to claim 1, characterized in that, In step (1), the original graphite is flake graphite or block graphite; the persulfate includes potassium persulfate and / or ammonium persulfate.

4. The method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding according to claim 1, characterized in that, In step (1), the specific dimensions of the container are a bottom diameter of 30mm and a height of 20mm; the size of the circular hole is a diameter of 0.5mm; the size of the quartz disc includes a diameter of 30mm and a thickness of 0.5mm, 1mm, 1.5mm, 2mm or 2.5mm.

5. The method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding according to claim 4, characterized in that, The flat paving in step (1) specifically includes: spin coating the slurry at a speed of 3000~4000rpm for 15~30 seconds, and then vacuum filtering it through the pre-reserved circular hole at the bottom of the growth container at a pressure of -0.1Mpa for 3~5 seconds.

6. The method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding according to claim 1, characterized in that, The static reaction described in step (1) is specifically a reaction at a temperature of 25℃~80℃ for 7h~24h.

7. The method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding according to claim 1, characterized in that, The high-temperature purification process described in step (2) specifically includes: heating from 25°C to 450°C, 550°C or 650°C at a heating rate of 7°C / min in an argon atmosphere, and holding at that temperature for 90 minutes.

8. The method for preparing a flexible thin film of highly oriented graphene aggregates for electromagnetic shielding according to claim 1, characterized in that, The mechanical pressing mentioned in step (3) specifically refers to holding the pressure at 15~30 MPa for 60 minutes.

9. The flexible film for electromagnetic shielding made by the method for preparing a highly oriented graphene aggregate flexible film for electromagnetic shielding as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Graphene preparation method based on insulation substrate

    CN107032331A

  • Method for preparing high-quality graphene-copper composite powder and high-strength and high-conductivity composite material thereof based on graphene confinement growth