Manganese iron phosphate precursor, preparation method thereof, lithium manganese iron phosphate cathode material and preparation method thereof, cathode sheet and lithium ion battery

CN120246960BActive Publication Date: 2026-11-20SHANGHAI XUANYI NEW ENERGY DEV CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510343541.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-21
Publication Date
2026-11-20
Estimated Expiration
2045-03-21

AI Technical Summary

Technical Problem

[0004]本发明的主要目的在于提供一种磷酸锰铁前驱体及其制备方法、磷酸锰铁锂正极材料及其制备方法、正极片和锂离子电池,以解决现有技术中磷酸锰铁锂正极材料存在压实密度和放电容量较低以及循环稳定性较差的问题

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120246960B_ABST
    Figure CN120246960B_ABST
Patent Text Reader

Abstract

The application provides a manganese iron phosphate precursor, a preparation method of the manganese iron phosphate precursor, a lithium manganese iron phosphate positive electrode material, a preparation method of the lithium manganese iron phosphate positive electrode material, a positive electrode sheet and a lithium ion battery. a Fe b PO4, wherein 0.67<= (a / b) <=9 and 1.15<= (a+b) <=1.43; the manganese iron phosphate precursor has a secondary particle structure formed by primary particles, the Dmax of the manganese iron phosphate precursor is 30-40 microns, and the average particle size of the primary particles is 50-500 nm. By controlling the molar ratio of Mn and Fe in the manganese iron phosphate precursor within the above range, the high-voltage characteristics of manganese and the stable characteristics of iron are combined, which helps to improve the structural stability of the lithium manganese iron phosphate positive electrode material in the charging and discharging process, reduces the dissolution of transition metal ions and the decomposition of the electrode material, and thus helps to improve the discharge capacity and cycle stability of the lithium manganese iron phosphate positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to a manganese iron phosphate precursor and its preparation method, a lithium manganese iron phosphate cathode material and its preparation method, a cathode sheet, and a lithium-ion battery. Background Technology

[0002] Currently, commonly used new energy power generation methods such as hydropower, geothermal energy, wind power, tidal energy, and solar energy are limited by time, space, and usage conditions, requiring large-scale energy storage devices to store the electricity generated by these new energy sources, thereby truly solving the problem of sustainable energy production and consumption. Lithium-ion batteries have received widespread attention from researchers and the market due to their advantages such as high operating voltage, low self-discharge, high energy density, long cycle life, no memory effect, and environmental friendliness. Lithium iron phosphate (LFP) batteries have received unprecedented attention from the market and researchers due to their safety and cost advantages; however, LFP cathode materials are currently at a development bottleneck, with difficulties in increasing energy density to meet higher market demands. Because iron has a low voltage plateau, introducing manganese, which has a high voltage plateau, into LFP can yield lithium manganese iron phosphate (LMFP) cathode materials with a higher average voltage. Its energy density is 10-15% higher than that of LFP, while still retaining the high safety of phosphate-based cathode materials and the low cost advantage compared to ternary cathode materials. Therefore, LMFP has attracted widespread attention from industry and related researchers.

[0003] Solid-state synthesis and coprecipitation precursor synthesis are commonly used methods for synthesizing LMFP. Solid-state synthesis offers a simple process and stable, controllable raw materials; however, the raw materials are difficult to disperse uniformly during physical mixing, resulting in slightly poorer crystallinity and consistency of the synthesized LMFP, lower powder compaction, and significant disadvantages in discharge capacity and long-term cycling performance. Coprecipitation precursor synthesis utilizes ferromanganese precursors to prepare LMFP. Due to the highly homogeneous distribution of metal elements in the ferromanganese precursor, the synthesized LMFP exhibits superior performance and good consistency. However, the improvement in compaction density, discharge capacity, and cycling stability of LMFP using the coprecipitation precursor method is currently limited. Summary of the Invention

[0004] The main objective of this invention is to provide a precursor of manganese iron phosphate and its preparation method, a cathode material of manganese iron phosphate and its preparation method, a cathode sheet, and a lithium-ion battery, so as to solve the problems of low compaction density, low discharge capacity, and poor cycle stability of lithium manganese iron phosphate cathode materials in the prior art.

[0005] To achieve the above objectives, according to one aspect of the present invention, a manganese ferric phosphate precursor is provided, the chemical formula of which is Mn a Fe bPO4, wherein 0.67≤(a / b)≤9, 1.15≤(a+b)≤1.43; the manganese iron phosphate precursor has a secondary particle structure formed by primary particles, the Dmax of the manganese iron phosphate precursor is 30~40μm, and the average particle size of the primary particles is 50~500nm.

[0006] Furthermore, the D10 of the aforementioned ferromanganese phosphate precursor is 1–3 μm, the D50 is 5–10 μm, and the D90 is 18–30 μm; and / or, the specific surface area of ​​the ferromanganese phosphate precursor is 5.0–11.0 m². 2 / g; and / or, the tap density of the manganese ferric phosphate precursor is 0.5–2.0 g / cm³. 3 .

[0007] According to another aspect of the present invention, a method for preparing the aforementioned manganese-iron phosphate precursor is provided, the method comprising the following steps: step S1, mixing a divalent manganese source, a trivalent iron source, an antioxidant and water to obtain a manganese-iron mixed solution; step S2, under a protective gas, the manganese-iron mixed solution, a phosphoric acid solution and an ammonia solution are added dropwise in parallel to water under stirring to carry out a co-precipitation reaction and aging in sequence to obtain the manganese-iron phosphate precursor.

[0008] Further, the temperature of the coprecipitation reaction is 20–45°C; and / or, the time for co-current dripping is the coprecipitation reaction time, which is 10–20 h; and / or, the stirring speed of the coprecipitation reaction is 250–650 rpm; and / or, the pH value of the solution in the coprecipitation reaction is 2–5; preferably, the coprecipitation reaction includes a first coprecipitation reaction and a second coprecipitation reaction performed sequentially, the time of the first coprecipitation reaction is 5–10 h; and / or, the stirring speed of the first coprecipitation reaction is 350–650 rpm; and / or, the pH value of the solution in the first coprecipitation reaction is 3–5; and / or, the time of the second coprecipitation reaction is 5–10 h; and / or, the stirring speed of the second coprecipitation reaction is 250–350 rpm; and / or, the pH value of the solution in the second coprecipitation reaction is 2–3; and / or, the aging temperature is 20–45°C; and / or, the aging time is 1–5 h.

[0009] Further, the total concentration of manganese and iron in the above-mentioned manganese-iron mixed solution is 0.25–2.5 mol / L; and / or, the concentration of antioxidant in the manganese-iron mixed solution is 0.001–0.05 mol / L; and / or, the concentration of phosphoric acid solution is 0.25–2.5 mol / L; and / or, the concentration of ammonia solution is 0.25–5 mol / L; and / or, the ratio of the total molar amount of manganese in the divalent manganese source and iron in the trivalent iron source to the molar amount of phosphate in the phosphoric acid solution is (1.15–1.43):1; and / or, the divalent manganese source is selected from any one or more of manganese sulfate, manganese carbonate, manganese nitrate, manganese oxalate, manganese acetate, and manganese chloride; and / or, the trivalent iron source is selected from any one or more of ferric sulfate, ferric nitrate, ferric oxalate, ferric acetate, and ferric chloride; and / or, the antioxidant is selected from any one or more of ascorbic acid, hydrazine hydrate, and sodium borohydride.

[0010] According to another aspect of the present invention, a method for preparing lithium manganese iron phosphate cathode material is provided, the method comprising: sequentially mixing raw materials including the aforementioned manganese iron phosphate precursor, carbon source, phosphorus source and lithium source with water, performing drying treatment and sintering treatment to obtain lithium manganese iron phosphate cathode material.

[0011] Further, the above mixing treatment is a sand milling treatment, and the particle size D50 of the slurry after sand milling treatment does not exceed 0.6 μm; and / or, the drying treatment is a spray drying treatment, and the inlet air temperature of the spray drying treatment is 200-400℃; and / or, the outlet air temperature of the spray drying treatment is 90-120℃; and / or, the heating rate of the sintering treatment is 2-5℃ / min; and / or, the sintering temperature is 650-800℃; and / or, the holding time of the sintering treatment is 5-15h; and / or, the molar ratio of lithium in the lithium source, the total molar ratio of manganese and iron in the manganese iron phosphate precursor, and the molar ratio of phosphorus in the phosphorus source is (1.1-1.4):(1.1-1.3):(1.11-1.37); preferably, the raw material also includes a doped metal source, and the lithium source contains lithium... The molar ratio of water to the molar ratio of the doped metal in the doped metal source is (1.1–1.4):0.003; and / or, the mass percentage of the carbon source in the raw material is 1%–30%; and / or, the mass ratio of water to the raw material is (65–200):100; preferably, the lithium source is selected from any one or more of lithium hydroxide, lithium carbonate, lithium oxalate, and lithium nitrate; and / or, the phosphorus source is selected from any one or more of lithium phosphate, lithium dihydrogen phosphate, ammonium phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; and / or, the doped metal source is selected from any one or more of magnesium source, titanium source, aluminum source, tungsten source, vanadium source, niobium source, nickel source, cobalt source, and yttrium source; and / or, the carbon source is selected from any one or more of glucose, citric acid, sucrose, chitosan, polyethylene glycol, polyvinyl alcohol, conductive carbon black, carbon nanotubes, and graphene.

[0012] According to another aspect of the present invention, a lithium manganese iron phosphate cathode material is provided, which is prepared by the aforementioned preparation method; preferably, the compaction density of the lithium manganese iron phosphate cathode material is 2.41–2.55 g / cm³. 3 .

[0013] According to another aspect of the present invention, a positive electrode sheet is provided, comprising a current collector and a positive electrode active layer, wherein the positive electrode active layer contains the aforementioned lithium manganese iron phosphate positive electrode material.

[0014] According to another aspect of the present invention, a lithium-ion battery is provided, comprising a positive electrode, an electrolyte, and a negative electrode, wherein the positive electrode is the aforementioned positive electrode.

[0015] By applying the technical solution of this invention, controlling the molar ratio of Mn and Fe in the ferromanganese phosphate precursor within the aforementioned range, the high voltage characteristics of manganese combined with the stable characteristics of iron help improve the structural stability of the lithium iron manganese phosphate cathode material during charge and discharge processes, reduce the dissolution of transition metal ions and the decomposition of electrode materials, thereby contributing to improving the discharge capacity and cycle stability of the lithium iron manganese phosphate cathode material. The ferromanganese phosphate precursor has a secondary particle structure formed from primary particles, which is beneficial for improving the compaction density and electrical performance of the lithium iron manganese phosphate cathode material. Controlling the Dmax of the ferromanganese phosphate precursor within the aforementioned range helps to form a denser structure during subsequent sintering, thereby further improving the compaction density of the lithium iron manganese phosphate cathode material and thus contributing to increasing the energy density of the battery. Controlling the average particle size of the primary particles within the aforementioned range helps to reduce the lithium ion diffusion path and increase the lithium ion diffusion rate, thereby contributing to improving the rate performance of the lithium iron manganese phosphate cathode material. Attached Figure Description

[0016] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0017] Figure 1 SEM images of the manganese iron phosphate precursor in Example 2 of this application are shown;

[0018] Figure 2 The SEM image of the lithium manganese iron phosphate cathode material in Example 2 of this application is shown. Detailed Implementation

[0019] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0020] Terminology Explanation: In this application, Dmax represents the maximum particle size in the particle size distribution.

[0021] As analyzed in the background section of this application, the existing lithium manganese iron phosphate cathode materials have problems such as low compaction density, low discharge capacity, and poor cycle stability. In order to solve the above problems, this application provides a manganese iron phosphate precursor and its preparation method, a lithium manganese iron phosphate cathode material and its preparation method, a cathode sheet, and a lithium-ion battery.

[0022] In a typical embodiment of this application, a manganese iron phosphate precursor is provided, the chemical formula of which is Mn a Fe b PO4, wherein 0.67≤(a / b)≤9, 1.15≤(a+b)≤1.43; the manganese iron phosphate precursor has a secondary particle structure formed by primary particles, the Dmax of the manganese iron phosphate precursor is 30~40μm, and the average particle size of the primary particles is 50~500nm.

[0023] By controlling the molar ratio of Mn and Fe in the ferromanganese phosphate precursor within the aforementioned range, the high voltage characteristics of manganese combined with the stable properties of iron help improve the structural stability of the lithium iron phosphate cathode material during charge and discharge processes, reduce the dissolution of transition metal ions and the decomposition of electrode materials, thereby contributing to improved discharge capacity and cycle stability. The ferromanganese phosphate precursor has a secondary particle structure formed from primary particles, which is beneficial for improving the compaction density and electrical performance of the lithium iron phosphate cathode material. Controlling the Dmax of the ferromanganese phosphate precursor within the aforementioned range helps to form a denser structure during subsequent sintering, further improving the compaction density of the lithium iron phosphate cathode material and thus increasing the energy density of the battery. Controlling the average particle size of the primary particles within the aforementioned range helps to reduce the lithium-ion diffusion path and increase the lithium-ion diffusion rate, thereby contributing to improved rate performance of the lithium iron phosphate cathode material.

[0024] In one embodiment of this application, the chemical formula of the above-mentioned manganese iron phosphate precursor is Mn a Fe b PO4, where 1≤a / b≤2.3 and 1.2≤a+b≤1.3, helps to further enhance the synergistic effect between Mn and Fe, thereby helping to further improve the structural stability of lithium manganese iron phosphate cathode material during cycling.

[0025] In one embodiment of this application, the average particle size of the primary particles is 100-150 nm, which helps to improve the structural stability of the lithium manganese iron phosphate cathode material while reducing the diffusion path of lithium ions, thereby helping to improve the rate performance and cycle stability of the lithium manganese iron phosphate cathode material.

[0026] In one embodiment of this application, the D10 of the aforementioned ferromanganese phosphate precursor is 1–3 μm, the D50 is 5–10 μm, and the D90 is 18–30 μm; and / or, the specific surface area of ​​the ferromanganese phosphate precursor is 5.0–11.0 m². 2 / g; and / or, the tap density of the manganese ferric phosphate precursor is 0.5–2.0 g / cm³. 3 .

[0027] Controlling the particle size distribution, specific surface area, and tap density of the manganese iron phosphate precursor within the aforementioned range helps to enable the lithium manganese iron phosphate cathode material to form a dense and uniform structure during the compaction process. This reduces the risk of excessively large or small particle distribution leading to a decrease in compaction density or uneven distribution of porosity within the electrode, thereby helping to improve the compaction density and electrochemical performance consistency of the lithium manganese iron phosphate cathode material.

[0028] In another typical embodiment of this application, a method for preparing the aforementioned manganese-iron phosphate precursor is provided. The preparation method includes the following steps: Step S1, mixing a divalent manganese source, a trivalent iron source, an antioxidant, and water to obtain a manganese-iron mixed solution; Step S2, under a protective gas, the manganese-iron mixed solution, a phosphoric acid solution, and an ammonia solution are added dropwise in parallel to water under stirring to carry out co-precipitation reaction and aging in sequence to obtain the manganese-iron phosphate precursor.

[0029] In step S1, a manganese-iron mixed solution is formed by mixing divalent manganese and trivalent iron sources with an antioxidant and water. This process facilitates the uniform distribution of metal ions in the solution. Uniformly distributed metal ions contribute to the formation of a consistent manganese-iron phosphate precipitate in the subsequent co-precipitation reaction, reducing the risk of material inhomogeneity and performance degradation caused by localized metal concentration differences. The presence of the antioxidant in the manganese-iron mixed solution helps control the oxidation state of the metal ions, thereby reducing side reactions. In step S2, the co-precipitation reaction is carried out under a protective gas atmosphere, which effectively isolates oxygen and reduces the oxidation of metal ions. The co-current addition of the manganese-iron mixed solution, phosphoric acid solution, and ammonia solution to water under stirring allows for more precise control of the pH and reaction rate, thus helping to regulate the morphology and size of the primary and secondary particles of the manganese-iron phosphate precursor. The aging step further optimizes the crystallinity and morphology of the precursor, contributing to the formation of a more uniform secondary particle structure, thereby improving the compaction density and electrochemical activity of the lithium manganese-iron phosphate cathode material.

[0030] The protective gas is selected from any one or more of nitrogen, helium, and argon.

[0031] In one embodiment of this application, the aged product is subjected to solid-liquid separation, washing, drying and classification in sequence to obtain manganese iron phosphate precursor; preferably, the drying temperature is 50-180°C.

[0032] In one embodiment of this application, the temperature of the coprecipitation reaction is 20–45°C; and / or, the time for co-current dripping is the coprecipitation reaction time, which is 10–20 h; and / or, the stirring speed of the coprecipitation reaction is 250–650 rpm; and / or, the pH value of the solution in the coprecipitation reaction is 2–5; preferably, the coprecipitation reaction includes a first coprecipitation reaction and a second coprecipitation reaction performed sequentially, the time of the first coprecipitation reaction is 5–10 h; and / or, the stirring speed of the first coprecipitation reaction is 350–650 rpm; and / or, the pH value of the solution in the first coprecipitation reaction is 3–5; and / or, the time of the second coprecipitation reaction is 5–10 h; and / or, the stirring speed of the second coprecipitation reaction is 250–350 rpm; and / or, the pH value of the solution in the second coprecipitation reaction is 2–3; and / or, the aging temperature is 20–45°C; and / or, the aging time is 1–5 h.

[0033] Excessive temperature can lead to overly rapid particle growth, resulting in larger or irregular particles; while excessively low temperature can negatively impact the reaction rate and crystallization quality. Controlling the temperature of the coprecipitation reaction within the aforementioned range helps balance the reaction rate and crystallization process, thus contributing to obtaining a precursor with moderate particle size and uniform morphology. Controlling the coprecipitation reaction time, especially the times of the first and second coprecipitations, within the aforementioned range helps control the growth of primary particles and the formation of secondary particles, thereby improving the tap density of the manganese ferrophosphate precursor. Excessive stirring can cause primary particles to break down, affecting the formation of secondary particles; while excessively low stirring speed can lead to particle agglomeration. Controlling the stirring speed of the coprecipitation reaction, especially the stirring speeds of the first and second coprecipitations, within the aforementioned range helps control the degree of particle agglomeration and optimize the structure and size of the secondary particles. Both excessively low and high pH values ​​can affect particle size and morphology. Controlling the pH of the solution in the coprecipitation reaction, especially the pH of the solution in the first and second coprecipitation reactions, within the aforementioned range, can control the precipitation rate of metal ions, optimize particle growth conditions, and control the morphology and size of the manganese iron phosphate precursor. The aging process helps to further optimize the crystallinity and morphology of the precursor. Controlling the aging temperature and time within the aforementioned range helps to form a more uniform and consistent secondary structure. Simultaneously, this also helps to reduce impurities and improve material purity, thereby contributing to improved discharge capacity and cycle stability of the lithium manganese iron phosphate cathode material.

[0034] In one embodiment of this application, the total concentration of manganese and iron in the above-mentioned manganese-iron mixed solution is 0.25–2.5 mol / L; and / or, the concentration of antioxidant in the manganese-iron mixed solution is 0.001–0.05 mol / L; and / or, the concentration of phosphoric acid solution is 0.25–2.5 mol / L; and / or, the concentration of ammonia solution is 0.25–5 mol / L; and / or, the ratio of the total molar amount of manganese in the divalent manganese source and iron in the trivalent iron source to the molar amount of phosphate in the phosphoric acid solution is (1.15–1.43):1; and / or, the divalent manganese source is selected from any one or more of manganese sulfate, manganese carbonate, manganese nitrate, manganese oxalate, manganese acetate, and manganese chloride; and / or, the trivalent iron source is selected from any one or more of ferric sulfate, ferric nitrate, ferric oxalate, ferric acetate, and ferric chloride; and / or, the antioxidant is selected from any one or more of ascorbic acid, hydrazine hydrate, and sodium borohydride.

[0035] High concentrations of metal ion solutions can accelerate the coprecipitation reaction rate and shorten the reaction time, but excessively high concentrations may lead to excessively rapid particle growth, uneven size, and affect the tap density of the ferromanganese phosphate precursor. Controlling the total concentration of manganese and iron in the ferromanganese mixed solution within the aforementioned range helps improve the uniformity of metal ion distribution and control the growth rate and size of primary and secondary particles. Controlling the concentration of antioxidants in the ferromanganese mixed solution within the aforementioned range helps reduce the oxidation of metal ions without excessively affecting the chemical composition of the material, thus contributing to improved purity of the ferromanganese phosphate precursor. Controlling the concentrations of phosphoric acid solution and ammonia solution within the aforementioned range helps to better control the pH value in the coprecipitation reaction solution, thereby facilitating more precise control of the morphology and size of the ferromanganese phosphate precursor.

[0036] In another typical embodiment of this application, a method for preparing lithium manganese iron phosphate cathode material is provided. The method includes: mixing raw materials including the aforementioned manganese iron phosphate precursor, carbon source, phosphorus source and lithium source with water in sequence, performing drying treatment and sintering treatment to obtain lithium manganese iron phosphate cathode material.

[0037] Using manganese iron phosphate precursor as the manganese and iron source for forming lithium manganese iron phosphate cathode material, it is mixed with carbon source, phosphorus source, lithium source and water in sequence, dried and sintered to obtain lithium manganese iron phosphate cathode material. The preparation method is simple, and the prepared lithium manganese iron phosphate cathode material has high compaction density, discharge capacity and cycle stability.

[0038] In one embodiment of this application, the above-mentioned mixing treatment is a sand milling treatment, and the particle size D50 of the slurry after sand milling treatment does not exceed 0.6 μm; and / or, the drying treatment is a spray drying treatment, and the inlet air temperature of the spray drying treatment is 200-400℃; and / or, the outlet air temperature of the spray drying treatment is 90-120℃; and / or, the heating rate of the sintering treatment is 2-5℃ / min; and / or, the sintering temperature is 650-800℃; and / or, the holding time of the sintering treatment is 5-15h; and / or, the molar ratio of lithium in the lithium source, the total molar ratio of manganese and iron in the manganese iron phosphate precursor, and the molar ratio of phosphorus in the phosphorus source is (1.1-1.4):(1.1-1.3):(1.11-1.37); preferably, the raw material also includes a doped metal source, and the molar ratio of lithium in the lithium source is (1.1-1.4):(1.1-1.3):(1.11-1.37). The molar ratio of water to the doped metal in the doped metal source is (1.1-1.4):0.003; and / or, the mass percentage of carbon source in the raw material is 1%-30%, preferably 5%-10%; and / or, the mass ratio of water to the raw material is (65-200):100; preferably, the lithium source is selected from any one or more of lithium hydroxide, lithium carbonate, lithium oxalate, and lithium nitrate; and / or, the phosphorus source is selected from any one or more of lithium phosphate, lithium dihydrogen phosphate, ammonium phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; and / or, the doped metal source is selected from any one or more of magnesium source, titanium source, aluminum source, tungsten source, vanadium source, niobium source, nickel source, cobalt source, and yttrium source; and / or, the carbon source is selected from any one or more of glucose, citric acid, sucrose, chitosan, polyethylene glycol, polyvinyl alcohol, conductive carbon black, carbon nanotubes, and graphene.

[0039] Controlling the particle size D50 of the slurry after sand milling within the above-mentioned range helps improve the uniformity of the distribution among the components and increase the contact area between them, thereby contributing to the formation of lithium manganese iron phosphate cathode materials with better structural consistency. Controlling the inlet and outlet air temperatures of the spray drying process within the above-mentioned range helps improve drying efficiency and enhances the particle size uniformity and structural stability of the powder. Controlling the heating rate, temperature, and holding time of the sintering process within the above-mentioned range helps promote the crystallization of the material, improve its conductivity and structural stability, while a reasonable heating rate helps reduce internal stress, decrease crack formation, and improve the integrity and consistency of the material.

[0040] Including but not limited to, the magnesium source is magnesium oxide, the titanium source is titanium oxide, the aluminum source is aluminum oxide, the tungsten source is tungsten oxide, the vanadium source is vanadium oxide, the niobium source is niobium oxide, the nickel source is nickel oxide, the cobalt source is cobalt oxide, and the yttrium source is yttrium oxide.

[0041] In one embodiment of this application, the sintering process described above is carried out in a protective gas, which is selected from any one or more of nitrogen, helium, and argon.

[0042] In one embodiment of this application, the spray drying is centrifugal spray drying or pressure spray drying. The centrifugal atomizing disc frequency of the centrifugal spray drying is 40-100Hz, and the pressure atomizing disc frequency of the pressure spray drying is 100-400Hz.

[0043] In one embodiment of this application, the product after the above sintering treatment is subjected to air jet milling and demagnetization in sequence to obtain lithium manganese iron phosphate cathode material; preferably, the temperature of air jet milling is 100-200°C.

[0044] In one embodiment of this application, the carbon source is a combination of glucose and polyethylene glycol, and the mass ratio of glucose to polyethylene glycol is 5:(2-5), specifically 5:2, 5:3, 5:4, 5:5, and any range between two ratios.

[0045] During sintering, glucose decomposes to form carbon, providing excellent conductivity for lithium manganese iron phosphate materials. Polyethylene glycol, on the other hand, decomposes more slowly at high temperatures, which helps form a more stable carbon skeleton and create a more uniform and dense conductive network. Controlling the mass ratio of glucose to polyethylene glycol within the aforementioned range helps to further improve the compaction density, discharge capacity, and cycle stability of lithium manganese iron phosphate cathode materials.

[0046] In one embodiment of this application, the doped metal source is a combination of a magnesium source and a titanium source, and the molar ratio of magnesium in the magnesium source to titanium in the titanium source is 2:(1~2), specifically 2:1, 2:1.1, 2:1.2, 2:1.3, 2:1.4, 2:1.5, 2:1.6, 2:1.7, 2:1.8, 2:1.9, 2:2, and any range between two ratios.

[0047] Magnesium can enter the crystal lattice, helping to enhance the lithium-ion transport pathway while reducing manganese ion dissolution and maintaining the structural integrity of the material during cycling. Titanium doping further strengthens the crystal lattice, preventing volume changes during lithium-ion insertion and extraction, thereby improving the material's cycle stability and lifespan. Controlling the mass ratio of magnesium to titanium sources within the aforementioned range helps improve their synergistic effect, thus enhancing the structural stability of the lithium manganese iron phosphate cathode material and consequently improving its cycle stability.

[0048] In another typical embodiment of this application, a lithium manganese iron phosphate cathode material is provided, which is prepared by the aforementioned preparation method; preferably, the compaction density of the lithium manganese iron phosphate cathode material is 2.41–2.55 g / cm³. 3 .

[0049] The lithium manganese iron phosphate cathode material prepared by the method of this application has high compaction density, discharge capacity and cycle stability. Controlling the compaction density of the lithium manganese iron phosphate cathode material within the above range helps to further improve the cycle stability of the lithium manganese iron phosphate cathode material.

[0050] In another typical embodiment of this application, a positive electrode sheet is provided, including a current collector and a positive electrode active layer, wherein the positive electrode active layer contains the aforementioned lithium manganese iron phosphate positive electrode material.

[0051] Because the above-mentioned cathode contains the lithium manganese iron phosphate cathode material of this application, the cathode has high discharge capacity and cycle stability.

[0052] In another typical embodiment of this application, a lithium-ion battery is provided, including a positive electrode, an electrolyte, and a negative electrode, wherein the positive electrode is the aforementioned positive electrode.

[0053] Because the above-mentioned positive electrode contains the lithium manganese iron phosphate positive electrode material of this application, the battery has high discharge capacity, cycle stability and safety.

[0054] The beneficial effects of this application will be further illustrated below with reference to the embodiments.

[0055] Example 1

[0056] Manganese sulfate and ferric sulfate were dissolved in water according to the elemental molar ratio (Mn:Fe = 50:50), and ascorbic acid was added to prepare a manganese-ferric mixed solution with a total manganese-ferric ion concentration of 1.2 mol / L and an ascorbic acid concentration of 0.002 mol / L. A 1 mol / L phosphoric acid solution and a 2 mol / L ammonia solution were also prepared. Nitrogen gas was introduced into the reaction vessel, and the reaction temperature was controlled at 25℃. The stirring speed for the first coprecipitation was 500 rpm. Then, the manganese-ferric mixed solution, phosphoric acid solution, and ammonia solution were added dropwise in a parallel stream to the reaction vessel. In the reactor, the time for the co-precipitation reaction and the time for the second coprecipitation reaction are equal, respectively. The peristaltic pump rate is controlled to maintain the pH of the solution at 4 during the reaction. After 5 hours of reaction, the second coprecipitation reaction begins. The stirring speed is adjusted to 300 rpm, and the peristaltic pump rate is controlled to maintain the pH of the solution at 2 during the reaction. The reaction continues for another 5 hours, followed by aging at 25°C for 3 hours. After filtration, ferromanganese phosphate precipitate is obtained. After three repeated water washings and pressure filtrations, it is dried at 120°C and then fractionated to obtain ferromanganese phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (2.60 μm), D50 (6.25 μm), D90 (22.37 μm), and Dmax (35.83 μm), has an average primary particle size of 150 nm in the ferromanganese phosphate precursor, and a specific surface area of ​​7.36 m². 2The tap density of the manganese iron phosphate precursor is 1.1 g / cm³. 3 .

[0057] Lithium carbonate, the aforementioned manganese iron phosphate precursor, lithium dihydrogen phosphate, magnesium oxide, and titanium dioxide were mixed in an elemental molar ratio (Li:(Mn+Fe):P:Mg:Ti=1.125:1.1:1.12:0.002:0.001). Then, glucose and polyethylene glycol were added and mixed to obtain a mixture with a glucose mass percentage of 5% and a polyethylene glycol mass percentage of 2%. The mixture was then mixed and dispersed with water for 2 hours at a mass ratio of 100:150. After sand milling, a slurry with a D50 particle size of 0.55 μm was obtained. The inlet air temperature of the centrifugal atomizer was set to 290℃, the outlet air temperature to 100℃, and the centrifugal atomization disk frequency to 50Hz. After spray drying, the dried material was obtained and sintered at 750℃ at a rate of 2℃ / min under a nitrogen atmosphere for 12 hours. Finally, after pulverization and demagnetization, the lithium manganese iron phosphate cathode material was obtained.

[0058] Example 2

[0059] The difference from Example 1 is that manganese sulfate and ferric sulfate were dissolved in water according to the elemental molar ratio (Mn:Fe = 60:40), and ascorbic acid was added to prepare a manganese-ferric mixed solution with a total manganese-ferric metal ion concentration of 1.25 mol / L and an ascorbic acid concentration of 0.0025 mol / L. A 1 mol / L phosphoric acid solution and a 2 mol / L ammonia solution were also prepared. Nitrogen gas was introduced into the reaction vessel, the reaction temperature was controlled at 25°C, and the stirring speed for the first coprecipitation was 500 rpm. Then, the manganese-ferric mixed solution, phosphoric acid solution, and ammonia solution were... The solution was added dropwise into the reactor simultaneously, with the dropwise addition time equal to the time of the first and second coprecipitation reactions. The peristaltic pump rate was controlled to maintain the pH of the solution at 4 during the reaction. After 5 hours of reaction, the second coprecipitation reaction was initiated. The stirring speed was adjusted to 300 rpm, and the peristaltic pump rate was controlled to maintain the pH of the solution at 2 during the reaction. The reaction was continued for another 5 hours, followed by aging at 25°C for 3 hours. The precipitate was obtained by filtration, and after three repeated washings with water and pressure filtrations, it was dried at 120°C. The resulting fraction was then graded to obtain the manganese ferric phosphate precursor powder Mn. 0.75 Fe 0.5 PO4, with fractionated particle sizes of D10 (1.85 μm), D50 (5.68 μm), D90 (20.48 μm), and Dmax (34.75 μm), has an average primary particle size of 120 nm in the ferromanganese phosphate precursor, and a specific surface area of ​​8.71 m². 2 The tap density of the manganese iron phosphate precursor is 0.93 g / cm³. 3 .

[0060] Lithium carbonate, the aforementioned manganese iron phosphate precursor, lithium dihydrogen phosphate, magnesium oxide, and titanium dioxide were mixed in an elemental molar ratio (Li:(Mn+Fe):P:Mg:Ti=1.125:1.1:1.12:0.002:0.001). Then, glucose and polyethylene glycol were added and mixed to obtain a mixture with a glucose mass percentage of 5% and a polyethylene glycol mass percentage of 2%. The mixture was then mixed and dispersed with water for 2 hours at a mass ratio of 100:150. After sand milling, a slurry with a D50 particle size of 0.55 μm was obtained. The inlet air temperature of the centrifugal atomizer was set to 290℃, the outlet air temperature to 100℃, and the centrifugal atomization disk frequency to 50Hz. After spray drying, the dried material was obtained and sintered at 750℃ at a rate of 2℃ / min under a nitrogen atmosphere for 12 hours. Finally, after pulverization and demagnetization, the lithium manganese iron phosphate cathode material was obtained.

[0061] Example 3

[0062] The difference from Example 1 is that manganese sulfate and ferric sulfate were dissolved in water according to the elemental molar ratio (Mn:Fe = 70:30), and ascorbic acid was added to prepare a manganese-ferric mixed solution with a total manganese-ferric metal ion concentration of 1.3 mol / L and an ascorbic acid concentration of 0.0035 mol / L. A 1 mol / L phosphoric acid solution and a 2 mol / L ammonia solution were also prepared. Nitrogen gas was introduced into the reaction vessel, the reaction temperature was controlled at 25°C, and the stirring speed for the first coprecipitation was 500 rpm. Then, the manganese-ferric mixed solution, phosphoric acid solution, and ammonia solution were dissolved... The liquid was dripped into the reactor in a parallel flow, with the dripping time equal to the time of the first and second coprecipitation reactions. The peristaltic pump rate was controlled to maintain the pH of the solution at 4 during the reaction. After 5 hours of reaction, the second coprecipitation reaction was initiated. The stirring speed was adjusted to 300 rpm, and the peristaltic pump rate was controlled to maintain the pH of the solution at 2 during the reaction. The reaction was continued for another 5 hours, followed by aging at 25°C for 3 hours. The precipitate was obtained by filtration, and after three repeated washings with water and pressure filtrations, it was dried at 120°C. Then, the precipitate was fractionated to obtain the manganese ferric phosphate precursor powder Mn. 0.91 Fe 0.39 PO4, with fractionated particle sizes of D10 (1.89 μm), D50 (5.86 μm), D90 (18.37 μm), and Dmax (32.63 μm), has an average primary particle size of 100 nm in the manganese ferric phosphate precursor, and a specific surface area of ​​10.36 m². 2 The tap density of the manganese iron phosphate precursor is 0.81 g / cm³. 3 .

[0063] Lithium carbonate, the aforementioned manganese iron phosphate precursor, lithium dihydrogen phosphate, magnesium oxide, and titanium dioxide were mixed in an elemental molar ratio (Li:(Mn+Fe):P:Mg:Ti=1.125:1.1:1.12:0.002:0.001). Then, glucose and polyethylene glycol were added and mixed to obtain a mixture with a glucose mass percentage of 5% and a polyethylene glycol mass percentage of 2%. The mixture was then mixed and dispersed with water for 2 hours at a mass ratio of 100:150. After sand milling, a slurry with a D50 particle size of 0.55 μm was obtained. The inlet air temperature of the centrifugal atomizer was set to 290℃, the outlet air temperature to 100℃, and the centrifugal atomization disk frequency to 50Hz. After spray drying, the dried material was obtained and sintered at 750℃ at a rate of 2℃ / min under a nitrogen atmosphere for 12 hours. Finally, after pulverization and demagnetization, the lithium manganese iron phosphate cathode material was obtained.

[0064] Example 4

[0065] The difference from Example 1 is that the molar ratio of manganese in manganese sulfate to iron in ferric sulfate is 73:28, resulting in lithium manganese iron phosphate cathode material.

[0066] Example 5

[0067] The difference from Example 1 is that the pH value of the solution in the first coprecipitation reaction is controlled to be 3, and the pH value of the solution in the second coprecipitation reaction is controlled to be 2, to obtain the manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (2.40 μm), D50 (5.95 μm), D90 (24.45 μm), and Dmax (38.72 μm), has an average primary particle size of 145 nm in the ferromanganese phosphate precursor, and a specific surface area of ​​8.16 m². 2 The tap density of the manganese iron phosphate precursor is 1.03 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0068] Example 6

[0069] The difference from Example 1 is that the pH value of the solution in the first coprecipitation reaction is controlled to be 5, and the pH value of the solution in the second coprecipitation reaction is controlled to be 3, to obtain the manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (2.51 μm), D50 (5.87 μm), D90 (24.39 μm), and Dmax (38.93 μm), has an average primary particle size of 140 nm in the manganese ferric phosphate precursor, and a specific surface area of ​​9.34 m². 2The tap density of the manganese iron phosphate precursor is 0.98 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0070] Example 7

[0071] The difference from Example 1 is that the pH value of the solution in the first coprecipitation reaction was controlled to be 4, and the pH value of the solution in the second coprecipitation reaction was controlled to be 4, to obtain the manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (2.30 μm), D50 (5.57 μm), D90 (23.45 μm), and Dmax (37.23 μm), has an average primary particle size of 122 nm in the ferromanganese phosphate precursor, and a specific surface area of ​​10.56 m². 2 The tap density of the manganese iron phosphate precursor is 0.97 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0072] Example 8

[0073] The difference from Example 1 is that the pH value of the solution in the first coprecipitation reaction is controlled to be 6, and the pH value of the solution in the second coprecipitation reaction is controlled to be 1, to obtain the manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (2.10 μm), D50 (6.39 μm), D90 (22.55 μm), and Dmax (36.72 μm), has an average primary particle size of 110 nm and a specific surface area of ​​12.17 m². 2 The tap density of the manganese iron phosphate precursor is 0.95 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0074] Example 9

[0075] The difference from Example 1 is that the stirring speed of the first coprecipitation reaction was controlled at 350 rpm, and the stirring speed of the second coprecipitation reaction was controlled at 250 rpm, to obtain manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (1.95 μm), D50 (5.96 μm), D90 (20.58 μm), and Dmax (34.67 μm), has an average primary particle size of 143 nm and a specific surface area of ​​8.17 m². 2 The tap density of the manganese iron phosphate precursor is 1.03 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0076] Example 10

[0077] The difference from Example 1 is that the stirring speed of the first coprecipitation reaction was controlled at 650 rpm, and the stirring speed of the second coprecipitation reaction was controlled at 350 rpm, to obtain manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (2.34 μm), D50 (5.69 μm), D90 (21.45 μm), and Dmax (32.86 μm), has an average primary particle size of 146 nm in the ferromanganese phosphate precursor, and a specific surface area of ​​8.21 m². 2 The tap density of the manganese iron phosphate precursor is 1.01 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0078] Example 11

[0079] The difference from Example 1 is that the stirring speed of the first coprecipitation reaction was controlled at 650 rpm, and the stirring speed of the second coprecipitation reaction was controlled at 450 rpm, to obtain manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (1.93 μm), D50 (7.12 μm), D90 (19.48 μm), and Dmax (33.89 μm), has a primary particle size of 130 nm in the manganese ferric phosphate precursor, and a specific surface area of ​​10.71 m². 2 The tap density of the manganese iron phosphate precursor is 0.98 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0080] Example 12

[0081] The difference from Example 1 is that the stirring speed of both the first and second coprecipitation reactions was controlled at 200 rpm, resulting in the production of manganese iron phosphate precursor powder Mn. 0.6 Fe 0.6 PO4, with fractionated particle sizes of D10 (2.95 μm), D50 (7.96 μm), D90 (24.58 μm), and Dmax (37.73 μm), has an average primary particle size of 113 nm in the manganese ferric phosphate precursor, and a specific surface area of ​​11.23 m². 2 The tap density of the manganese iron phosphate precursor is 0.91 g / cm³. 3 Ultimately, lithium manganese iron phosphate cathode material was obtained.

[0082] Example 13

[0083] The difference from Example 1 is that the addition of titanium dioxide is omitted, and lithium carbonate, manganese iron phosphate precursor, lithium dihydrogen phosphate, and magnesium oxide are mixed in an elemental molar ratio (Li:(Mn+Fe):P:Mg=1.125:1.1:1.12:0.003) to finally obtain lithium manganese iron phosphate cathode material.

[0084] Example 14

[0085] The difference from Example 1 is that the addition of polyethylene glycol was omitted, and the mass percentage of glucose in the mixture was 7%, ultimately yielding lithium manganese iron phosphate cathode material.

[0086] Comparative Example 1

[0087] The difference from Example 1 is that the molar ratio of manganese in manganese sulfate to iron in ferric sulfate is 30:70, and the final product is lithium manganese iron phosphate cathode material.

[0088] Comparative Example 2

[0089] The difference from Example 1 is that the parallel dripping is eliminated, and a manganese-iron mixed solution, phosphoric acid solution and ammonia solution are added to water to carry out a co-precipitation reaction, and finally the lithium manganese iron phosphate cathode material is obtained.

[0090] Comparative Example 3

[0091] The difference from Example 1 is that ferrous sulfate is used instead of ferric sulfate, and ammonium dihydrogen phosphate is used instead of phosphoric acid solution and ammonia solution. The pH value of the coprecipitation solution is controlled to 4, and finally lithium manganese iron phosphate cathode material is obtained.

[0092] The lithium manganese iron phosphate cathode materials prepared in the examples and comparative examples were subjected to compaction density testing. The lithium manganese iron phosphate cathode materials prepared in the examples and comparative examples were used to prepare cathode sheets, which were then assembled with anode sheets, electrolyte and separator to form batteries for electrical performance testing. The test conditions were as follows: the specific capacity, specific capacity, coulombic efficiency and capacity retention after 1000 cycles at 1C were tested within a voltage range of 2.0 to 4.5V. The compaction density and electrical performance test results are shown in Table 1.

[0093] Table 1

[0094]

[0095]

[0096] Figure 1 This is a SEM image of the manganese iron phosphate precursor in Example 2 of this application. Figure 1 The average particle size of the primary particles of the manganese iron phosphate precursor can be measured to be 120 nm.

[0097] Figure 2 This is a SEM image of the lithium manganese iron phosphate cathode material in Example 2 of this application. Figure 2 As can be seen from the paper, the lithium manganese iron phosphate cathode material of this application has a relatively regular morphology.

[0098] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:

[0099] By controlling the molar ratio of Mn and Fe in the ferromanganese phosphate precursor within the aforementioned range, the high voltage characteristics of manganese combined with the stable properties of iron help improve the structural stability of the lithium iron phosphate cathode material during charge and discharge processes, reduce the dissolution of transition metal ions and the decomposition of electrode materials, thereby contributing to improved discharge capacity and cycle stability. The ferromanganese phosphate precursor has a secondary particle structure formed from primary particles, which is beneficial for improving the compaction density and electrical performance of the lithium iron phosphate cathode material. Controlling the Dmax of the ferromanganese phosphate precursor within the aforementioned range helps to form a denser structure during subsequent sintering, further improving the compaction density of the lithium iron phosphate cathode material and thus increasing the energy density of the battery. Controlling the average particle size of the primary particles within the aforementioned range helps to reduce the lithium-ion diffusion path and increase the lithium-ion diffusion rate, thereby contributing to improved rate performance of the lithium iron phosphate cathode material.

[0100] The above are merely embodiments of the present invention and are not intended to limit the invention. Those skilled in the art will recognize that the present invention can have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A manganese iron phosphate precursor, characterized in that, The chemical formula of the manganese iron phosphate precursor is Mn. a Fe b PO4, wherein 0.67≤(a / b)≤9, 1.15≤(a+b)≤1.43; the manganese iron phosphate precursor has a secondary particle structure formed by primary particles, the Dmax of the manganese iron phosphate precursor is 30~40µm, and the average particle size of the primary particles is 50~500nm. The preparation method of the manganese iron phosphate precursor includes the following steps: Step S1, mixing divalent manganese source, trivalent iron source, antioxidant and water to obtain manganese iron mixed solution; Step S2, under protective gas, the manganese iron mixed solution, phosphoric acid solution and ammonia solution are added dropwise in parallel to water under stirring to carry out co-precipitation reaction and aging in sequence to obtain manganese iron phosphate precursor; The coprecipitation reaction includes a first coprecipitation reaction and a second coprecipitation reaction performed sequentially. The pH value of the solution in the first coprecipitation reaction is 3-5, and the pH value of the solution in the second coprecipitation reaction is 2-3. The temperature of the coprecipitation reaction is 20~45℃; the time of the co-flow droplet is the time of the coprecipitation reaction, which is 10~20h; the stirring speed of the coprecipitation reaction is 250~650rpm. The aging temperature is 20~45℃, and the aging time is 1~5h.

2. The manganese iron phosphate precursor according to claim 1, characterized in that, The D10 of the ferromanganese phosphate precursor is 1~3µm, the D50 is 5~10µm, and the D90 is 18~30µm; and / or, the specific surface area of ​​the ferromanganese phosphate precursor is 5.0~11.0m². 2 / g; and / or, the tap density of the manganese iron phosphate precursor is 0.5~2.0 g / cm³. 3 .

3. A method for preparing the manganese iron phosphate precursor according to claim 1 or 2, characterized in that, The preparation method includes the following steps: Step S1: Mix divalent manganese source, trivalent iron source, antioxidant and water to obtain manganese-iron mixed solution; Step S2: Under a protective gas atmosphere, the manganese-iron mixed solution, phosphoric acid solution, and ammonia solution are added dropwise into water under stirring to carry out co-precipitation reaction and aging in sequence to obtain manganese-iron phosphate precursor; The coprecipitation reaction includes a first coprecipitation reaction and a second coprecipitation reaction performed sequentially. The pH value of the solution in the first coprecipitation reaction is 3-5, and the pH value of the solution in the second coprecipitation reaction is 2-3. The temperature of the coprecipitation reaction is 20~45℃; the time of the co-flow droplet is the time of the coprecipitation reaction, which is 10~20h; the stirring speed of the coprecipitation reaction is 250~650rpm. The aging temperature is 20~45℃, and the aging time is 1~5h.

4. The preparation method according to claim 3, characterized in that, The time for the first coprecipitation reaction is 5-10 hours; and / or the stirring speed for the first coprecipitation reaction is 350-650 rpm. And / or, the second coprecipitation reaction takes 5 to 10 hours; and / or, the stirring speed of the second coprecipitation reaction is 250 to 350 rpm.

5. The preparation method according to claim 3, characterized in that, The total concentration of manganese and iron in the manganese-iron mixed solution is 0.25~2.5 mol / L; and / or, the concentration of the antioxidant in the manganese-iron mixed solution is 0.001~0.05 mol / L; and / or, the concentration of the phosphoric acid solution is 0.25~2.5 mol / L; and / or, the concentration of the ammonia solution is 0.25~5 mol / L; and / or, the ratio of the total molar amount of manganese in the divalent manganese source and the total molar amount of iron in the trivalent iron source to the molar amount of phosphate in the phosphoric acid solution is (1.15~1.43):1; And / or, the divalent manganese source is selected from any one or more of manganese sulfate, manganese carbonate, manganese nitrate, manganese oxalate, manganese acetate, and manganese chloride; And / or, the trivalent iron source is selected from any one or more of ferric sulfate, ferric nitrate, ferric oxalate, ferric acetate, and ferric chloride; And / or, the antioxidant is selected from any one or more of ascorbic acid, hydrazine hydrate, and sodium borohydride.

6. A lithium iron phosphate cathode material, characterized in that, The lithium manganese iron phosphate cathode material is prepared from the manganese iron phosphate precursor as described in claim 1 or 2; the compaction density of the lithium manganese iron phosphate cathode material is 2.41~2.55 g / cm³. 3 .

7. A positive electrode sheet, comprising a current collector and a positive electrode active layer, characterized in that, The positive electrode active layer contains the lithium manganese iron phosphate positive electrode material as described in claim 6.

8. A lithium-ion battery, comprising a positive electrode, an electrolyte, and a negative electrode, characterized in that, The positive electrode is the positive electrode as described in claim 7.

Citation Information

Patent Citations

  • Lithium manganese iron phosphate precursor as well as preparation method and application thereof

    CN114940485A

  • Method for preparing lithium iron manganese phosphate positive electrode material by manganese-iron coprecipitation

    CN118771336A