PHA / PVA nanoscale paper-based barrier emulsion as well as preparation method and application thereof

The PHA particles were nanocensored to 100 nanometers to 300 nanometers by high-pressure homogenization method, blended with PVA to form a stable aqueous nanoemulsion, which solved the environmental protection, barrier performance and degradability of the paper-based coating, and achieved a stable barrier effect under high humidity.

CN120250392AActive Publication Date: 2025-07-04DU BAI CHENG NEW MATERIAL TECH (SHANGHAI) CO LTD +1

Patent Information

Application Number
CN202510673202.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2025-07-04
Estimated Expiration
2045-05-23

AI Technical Summary

Technical Problem

The existing paper-based coating technology has problems such as non-degradable, difficulty in recycling, health risks, insufficient barrier performance and difficulty in preparing stable aqueous nanoemulsions, especially in high humidity, performance has significantly decreased.

Method used

The PHA particles with an initial average particle size of 1 micron to 100 micron were nanocrysted into 100 nanometers to 300 nanometers by high-pressure homogenization method, and a stable aqueous nanoscale emulsion was formed in combination with PVA. By optimizing the ratio of PHA to PVA and the use of additives, a uniform and dense barrier coating was formed.

Benefits of technology

Maintain excellent water vapor, oxygen and grease barrier properties under high humidity, good biodegradability of the coating, controllable cost, suitable for large-scale production, and meet sustainable packaging needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a PHA / PVA nano-scale paper-based barrier emulsion as well as a preparation method and application thereof. The water-based emulsion comprises PHA particles with the average particle size ranging from 100 nanometers to 300 nanometers and PVA, the PHA and the PVA are blended according to a specific proportion, and the PVA serves as a main film forming component and a barrier property contribution component and is blended with the PHA to form the nano-emulsion. The preparation method comprises the following steps: mixing PHA particles with an initial average particle size of 1-100 microns with a PVA aqueous solution, and carrying out high-pressure homogenization and other nanocrystallization means to obtain the nano-emulsion. The emulsion can be coated on the surfaces of paper-based materials such as paper and paperboards, and a barrier coating is formed after the emulsion is dried. The obtained emulsion is small in particle size, good in stability and good in leveling property, a uniform and compact barrier film is easily formed on a paper base, the film has excellent water vapor, oxygen and grease barrier performance, and the material is bio-based, biodegradable and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and particularly to a PHA / PVA nano-scale paper-based barrier emulsion, its preparation method and application, especially a barrier coating technology for paper-based packaging materials. The present invention also relates to the preparation method of this nano-scale emulsion and the application of this emulsion in the preparation of paper-based barrier materials. Background Art

[0002] With the enhancement of environmental protection awareness and the growth of the demand for green packaging, traditional petroleum-based plastics face challenges due to non-degradability and difficult recycling, and biodegradable materials have become a research hotspot. Paper-based materials are widely used in the packaging field due to their renewable and degradable characteristics. However, their porous structure results in poor gas and water vapor barrier properties, and they are prone to moisture absorption under high humidity, leading to a decrease in mechanical strength. Therefore, surface coating modification is required to improve their performance.

[0003] Existing paper-based coating technologies have significant deficiencies. Although polyethylene PE lamination has waterproof and heat-sealing properties, it is derived from petrochemical resources, is non-degradable, has complex recycling, increases energy consumption and reduces fiber recovery rate. Paraffin coatings have low costs, but their gas barrier properties are limited, are prone to cracking at low temperatures or when bent, and are not degradable. Coatings containing per- and polyfluoroalkyl substances PFAS were widely used in food packaging due to their excellent water and oil repellency, but their environmental persistence and potential health risks have led to global restrictions on them. Biobased coatings such as polylactic acid PLA are renewable, but their water vapor barrier properties are insufficient, degradation requires industrial composting conditions, and the coatings have poor flexibility and are difficult to meet high-barrier requirements.

[0004] As a biodegradable polyester, polyhydroxyalkanoate PHA has multi-environment degradability in soil, water bodies, compost, etc. and certain water vapor and oxygen barrier properties. However, the production cost of PHA is high and its processing performance is limited. For example, polyhydroxybutyrate PHB is hard and brittle, has a narrow processing window, and is prone to thermal degradation. There are technical difficulties in preparing a stable aqueous nanoemulsion of hydrophobic PHA with a size of 100 nanometers to 300 nanometers. Traditional methods mostly obtain micron-sized particles of 0.5 microns to 5 microns, which are prone to agglomeration and sedimentation, or require organic solvents, increasing environmental risks. Polyvinyl alcohol PVA has excellent film-forming properties and oxygen barrier properties under dry conditions, but its strong hydrophilicity leads to a sharp decline in barrier performance under high humidity (relative humidity > 60% - 70%), limiting its water-resistant applications.

[0005] Existing PHA / PVA blending studies mostly use melting or organic solvent methods to prepare film or bulk materials, and it is difficult to achieve the environmentally friendly preparation of aqueous nanoemulsions and their application in paper-based barrier coatings.

[0006] In summary, there is an urgent need in the art for an environmentally friendly and cost - controllable PHA / PVA nano - emulsion preparation technology to convert PHA particles with an initial average particle size of 1 micrometer to 100 micrometers into a stable dispersion with a particle size of 100 nanometers to 300 nanometers, forming a uniform and dense paper - based barrier coating with excellent water vapor, oxygen, and oil barrier properties, especially stable performance under high humidity, to replace traditional coatings and meet the requirements of sustainable packaging. Summary of the Invention

[0007] The present invention provides a PHA / PVA nano - scale paper - based barrier emulsion, its preparation method and application for paper - based barrier coatings, which have excellent water vapor, oxygen, and oil barrier properties, especially stable performance in a high - humidity environment, are easy to coat and process, and have both biodegradability and potential cost - effectiveness.

[0008] The purpose of the present invention is to solve the following problems of the existing paper - based barrier coating technology:

[0009] 1. Traditional coatings such as PE lamination, paraffin, and PFAS have environmental problems such as non - degradability, difficult recycling, or health risks.

[0010] 2. Bio - based coatings such as PLA have insufficient barrier properties, and the barrier properties of pure PVA coatings decrease significantly under high humidity.

[0011] 3. Pure PHA materials are hard, brittle, and difficult to process, and it is difficult to prepare a stable aqueous nano - emulsion.

[0012] 4. Existing PHA / PVA blending technologies mostly rely on organic solvents or melt processing, and have not achieved the environmentally friendly preparation of aqueous nano - emulsions and the application in paper - based barrier coatings.

[0013] To achieve the above objectives, the present invention provides the following technical solutions:

[0014] First aspect: PHA / PVA nano - scale paper - based barrier emulsion

[0015] The present invention provides an aqueous nano - scale emulsion, comprising:

[0016] Polyhydroxyalkanoate (PHA) particles;

[0017] Polyvinyl alcohol (PVA).

[0018] Among them, the average particle size of PHA particles in the emulsion is 100 nanometers to 300 nanometers, preferably 150 nanometers to 250 nanometers, and the polydispersity index (PDI) of the particle size distribution ≤ 0.3, more preferably < 0.25.

[0019] Properties of PHA:

[0020] The PHA is selected from polyhydroxybutyrate (PHB), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBHHx), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (P3HB4HB), or a mixture thereof.

[0021] The PHA is poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV), wherein the molar fraction of the 3-hydroxyvalerate unit is from 2 mol% to 30 mol%, preferably from 5 mol% to 20 mol%.

[0022] The PHA has a weight-average molecular weight of from 100,000 to 1,000,000 g / mol.

[0023] Properties of PVA:

[0024] The degree of alcoholysis of PVA is from 75 mol% to 100 mol%, preferably from 86 mol% to 90 mol% (partially alcoholyzed) or from 98 mol% to 99.9 mol% (fully alcoholyzed).

[0025] The degree of polymerization of PVA is from 300 to 2500, preferably the viscosity of its 4% aqueous solution at 20°C is from 3 mPa·s to 75 mPa·s.

[0026] Emulsion composition:

[0027] The weight ratio of PHA to PVA is from 30:70 to 70:30, most preferably 70:30.

[0028] The total solids content of the emulsion is from 30 wt% to 55 wt%, preferably from 35 wt% to 50 wt%.

[0029] The viscosity of the emulsion at 25°C is from 100 mPa·s to 2500 mPa·s, and the specific value depends on the total solids content and the specific type and dosage of PVA.

[0030] Auxiliaries may be included, such as stabilizers, plasticizers, pH regulators, defoamers, preservatives, and the total content does not exceed 10 wt% of the solid weight. PVA itself can be used as a stabilizer, providing steric hindrance or electrostatic stabilization by adsorbing on the surface of PHA particles. In the case of high solids content, a small amount of additional non-ionic surfactant or protective colloid can be added as appropriate to further enhance the long-term storage stability, and its addition amount usually does not exceed 2% of the total solids weight. The non-ionic surfactant is preferably polyoxyethylene sorbitan monooleate.

[0031] Emulsion stability:

[0032] The zeta potential is usually -30 mV to -45 mV, and the emulsion has good physical stability.

[0033] The emulsion has no obvious sedimentation or stratification after standing at room temperature for 30 days and has good centrifugal stability.

[0034] Second aspect: Preparation method

[0035] The present invention provides a method for preparing the above-mentioned PHA / PVA nano-scale paper-based barrier emulsion, which includes the following steps:

[0036] Provide PHA raw materials with an initial average particle size of 1 μm to 100 μm, preferably 5 μm to 20 μm.

[0037] Dissolve PVA in water to prepare an aqueous PVA solution, and the dissolution temperature is 60°C to 95°C.

[0038] Mix the PHA raw materials and the aqueous PVA solution in a weight ratio of 30:70 to 70:30, and form a uniform PHA / PVA mixture by mechanical stirring or high-speed dispersion.

[0039] Perform nanosizing treatment on the mixture to reduce the average particle size of PHA particles to 100 nm to 300 nm and PDI ≤ 0.3 to obtain a nano-scale emulsion.

[0040] Nanosizing treatment:

[0041] Generally, high-pressure homogenization (HPH) is adopted, and the process parameters are:

[0042] Homogenization pressure: 50 MPa to 200 MPa, preferably 80 MPa to 180 MPa. For emulsions with a higher solid content, such as approaching 55%, a higher homogenization pressure may be required or the number of cycles may be appropriately increased to achieve the target particle size and PDI.

[0043] Number of cycles: 1 to 10 times, preferably 3 to 7 times.

[0044] Temperature control: The material temperature is below 80°C to prevent the degradation of PHA or PVA.

[0045] Other optional methods include ultrasonic treatment, such as ultrasonic treatment with a frequency not lower than 20 kHz and a treatment time of 10 minutes to 60 minutes, microfluidic homogenization, high-speed shearing, or ball milling.

[0046] Auxiliaries can be added after mixing or nanosizing to optimize the emulsion performance.

[0047] This method utilizes the hydrophilic and hydrophobic chain segment characteristics of PVA to adsorb on the surface of PHA particles under high-shear action, preventing particle aggregation and realizing the preparation of a stable nano-emulsion without a large amount of surfactant.

[0048] Third aspect: Application

[0049] The present invention provides the application of the above-mentioned PHA / PVA nanoscale paper-based barrier emulsion in the preparation of paper-based barrier materials. The emulsion is coated on at least one surface of paper-based materials such as paper, cardboard, and molded fiber products, and a barrier coating is formed after drying.

[0050] Coating process:

[0051] The coating methods include blade coating, roll coating, spray coating, dip coating, flexographic printing, gravure printing, or curtain coating.

[0052] The dry weight coating amount is 1 g / m² to 30 g / m², preferably 3 g / m² to 15 g / m², and more preferably 5 g / m².

[0053] The drying temperature is 50°C to 130°C, preferably 80°C to 110°C, and the drying time is until the coating is completely film-formed.

[0054] Fourth aspect: Paper-based barrier material

[0055] The present invention provides a paper-based barrier material, comprising:

[0056] A paper-based substrate;

[0057] A barrier coating coated and cured on at least one surface of the substrate, and the coating is derived from the above-mentioned PHA / PVA nanoscale emulsion.

[0058] Properties:

[0059] Water vapor transmission rate (WVTR, 38°C, 90%RH) < 100 g / (m²·24h), preferably 45 g / (m²·24h).

[0060] Oxygen transmission rate (OTR, 23°C, 50%RH) < 50 cm³ / (m²·24h·atm), preferably 8 cm³ / (m²·24h·atm).

[0061] Oil resistance (Kit test) grade ≥ 10.

[0062] The contact angle of the coating surface is 95° to 100°, showing excellent hydrophobicity.

[0063] The adhesion between the coating and the substrate is good, without peeling or slight peeling.

[0064] Beneficial effects

[0065] Compared with the prior art, using a PHA / PVA nanoscale paper-based barrier emulsion and its preparation method and application of the present invention can obtain the following significant beneficial effects:

[0066] Excellent emulsion properties: The average particle size of PHA particles in the emulsion is 100 to 300 nanometers, preferably 150 to 250 nanometers, PDI < 0.3, and the Zeta potential is usually between -30 mV and -45 mV. The emulsion has high stability and shows no obvious sedimentation after 30 days of storage. The nanoscale particles promote the formation of a uniform and dense coating film with good leveling properties, which is suitable for various industrial coating processes. Even at a total solid content as high as 55%, through optimized preparation processes, nanoemulsions meeting the requirements can still be obtained, which is beneficial for reducing transportation and drying costs and improving production efficiency.

[0067] Excellent barrier properties: The coating maintains a low WVTR (45 g / (m²·24 h)) and a low OTR (8 cm³ / (m²·24 h·atm)) at high humidity (90% RH), which is superior to pure PVA coatings (WVTR > 300 g / (m²·24 h) at high humidity) and PE laminated paper (OTR is 150 cm³ / (m²·24 h·atm)). The hydrophobicity and nanostructure of PHA increase the tortuosity of the permeation path, significantly enhancing the moisture resistance.

[0068] Improved physical properties: The blending of PHA and PVA improves the flexibility of the coating and reduces the risk of cracking. The adhesiveness of PVA ensures a strong bonding force between the coating and the paper substrate.

[0069] Environmentally friendly: The emulsion uses water as the dispersion medium and has no volatile organic compound emissions. PHA and PVA are bio-based or biodegradable materials. The coating has a biodegradation rate of 90% within 180 days according to the EN 13432 standard, is easy to recycle or compost, and meets the requirements of the circular economy.

[0070] Cost-effectiveness: The preferred 70:30 formulation and a coating amount of 5 g / m² achieve high-efficiency barrier performance, reduce the PHA usage, and the preliminary estimated cost is $0.05 per m², which is economically competitive. The high-pressure homogenization process is mature and suitable for large-scale production. Using high-solid-content emulsions can further reduce the energy consumption and production time per unit product.

[0071] In addition, the coating obtained by the present invention has the potential to be applied to food packaging. The formed barrier coating can be further tested through relevant tests to confirm compliance with the food contact material regulations of specific countries or regions. On the premise of meeting the relevant migration limits, it meets the requirements of EU 10 / 2011 regulations and US FDA 21 CFR 176.170 and other standards, and the total migration amount should not exceed 10 mg / dm² or 60 mg / kg of food or food simulants. Detailed Description of the Invention

[0072] The present invention will be described in detail below through specific examples, but the protection scope of the present invention is not limited to these examples.

[0073] The following are the raw materials used in the examples. The present invention is not limited to the use of these specific grades, and materials from other sources with similar key properties are expected to give similar results:

[0074] The poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) PHA, also known as PHBH, and poly(3-hydroxybutyrate-co-3-hydroxypentanoate) PHA, also known as PHBV, used are in powder form or can be micronized.

[0075] The degree of alcoholysis of the partially alcoholized polyvinyl alcohol PVA used is 87 mol% to 89 mol%, and the degree of polymerization is 1700.

[0076] The degree of alcoholysis of the fully alcoholized polyvinyl alcohol PVA used is 98 mol% to 99 mol%, and the degree of polymerization is 1700.

[0077] The basis weight of the unsized kraft paper substrate used is 80 g / ㎡.

[0078] The PE-coated kraft paper used as a comparative material has a PE coating amount of 15 g / ㎡.

[0079] The raw materials are shown in Table 1:

[0080]

[0081] Emulsion property characterization

[0082] According to the ISO 22412:2017 standard, the dynamic light scattering (DLS) technique was used to measure the average particle size and the polydispersity index (PDI) of PHA particles in the emulsion. According to the ISO 13099-2 standard, a Zeta potential analyzer was used to measure the surface charge of the particles to evaluate the emulsion stability. The optimized emulsions, such as PHA:PVA at 70:30, generally showed an average particle size of about 150 nm, a PDI value of 0.2 to 0.25, and a Zeta potential of -30 mV to -40 mV at different solid contents.

[0083] Formulation optimization experiments

[0084] To determine the optimal weight ratio of PHA to PVA, a series of experiments were conducted to investigate the effects of different ratios on the key performance indicators of the coating, including the water vapor transmission rate (WVTR), the oxygen transmission rate (OTR), and the water contact angle. The results are shown in Table 2 below:

[0085]

[0086] Table 2 The experimental results show that when the weight ratio of PHA to PVA is 70:30, the coating exhibits the lowest water vapor transmission rate and oxygen transmission rate, as well as the highest contact angle, with the best comprehensive performance. Therefore, 70:30 is determined as a preferred weight ratio of PHA to PVA.

[0087] Example

[0088] Example 1: Tian'an PHBV / PVA 1799 high-solid nanoemulsion (weight ratio of PHA to PVA is 70:30, using the HPH method, homogenization pressure is 180 MPa, total solid content is 40 wt%)

[0089] Dissolve PVA 1799 in deionized water to prepare a 12% weight percentage aqueous PVA solution, which can be heated to 90°C to 95°C to facilitate dissolution. Weigh 56 grams of Tian'an Enmat Y1000P micropowder. If the raw material is in pellet form, it needs to be pre-micronized to an initial average particle size of 5 microns to 20 microns, and slowly add it to the corresponding amount of PVA 1799 aqueous solution, corresponding to 30 parts of PVA, and adjust the total solid content to 40 wt%, with a total emulsion amount of 200 grams. Stir with a high-speed stirrer for 60 minutes to obtain a preliminary mixture. Transfer this mixture to a high-pressure homogenizer HPH, set the homogenization pressure to 180 MPa, and perform 5 cycles of homogenization treatment, controlling the material temperature < 75°C. Emulsion 1 is obtained. This emulsion is characterized by dynamic light scattering DLS, with an average PHA particle size of 170 nm and a PDI equal to 0.22. The Zeta potential is measured using a Malvern Zetasizer Nano ZS at 25°C, with deionized water as the dispersion medium, and the result is -34 mV. The viscosity of the emulsion at 25°C is 1300 mPa·s, and after standing at 25°C for 30 days, there is no obvious stratification visually, and the sedimentation rate is < 5% after centrifugation at 3000 rpm for 15 minutes.

[0090] Example 2: Tian'an PHBV / PVA 1799 extremely high-solid nanoemulsion (weight ratio of PHA to PVA is 70:30, total solid content is 55 wt%)

[0091] Dissolve PVA 1799 in deionized water to prepare a 16.5 wt% PVA aqueous solution. The total amount of PVA is 33 grams, corresponding to 30 parts. Weigh 77 grams of Tianan Enmat Y1000P fine powder. If the raw material is in pellet form, it needs to be pre-micronized to an initial average particle size of 5 to 20 microns, and slowly add it to the above PVA 1799 aqueous solution to make the total solid content 55 wt% and the total emulsion amount 200 grams. Stir with a high-speed stirrer for 60 - 90 minutes. To assist in dispersion and maintain fluidity at high solid content, add 0.8% of polyoxyethylene sorbitan monooleate (Tween 80) based on the total solid weight at this stage. Transfer the mixture to a high-pressure homogenizer HPH, set the homogenization pressure at 200 MPa, and perform 7 - 10 cycles of homogenization treatment, controlling the material temperature < 78 °C. Obtain Emulsion 2. This emulsion is characterized by dynamic light scattering DLS, and the average particle size of PHA particles is 190 nm, with PDI ≤ 0.25. The Zeta potential is measured using a Malvern Zetasizer Nano ZS at 25 °C with deionized water as the dispersion medium, and the result is -32 mV. The viscosity of the emulsion is 2300 mPa·s at 25 °C, and after standing at 25 °C for 30 days, there is no obvious stratification or only extremely slight sedimentation visually, and the sedimentation rate < 5 - 7% after centrifugation at 3000 rpm for 15 minutes.

[0092] Example 3: Kaneka PHBH / PVA 1788 high-solid-content nanoemulsion (weight ratio of PHA to PVA is 50:50, using the HPH method, homogenization pressure is 150 MPa, total solid content is 30 wt%)

[0093] Dissolve PVA 1788 in deionized water to prepare a 15% by weight aqueous PVA solution, and it can be appropriately heated until completely dissolved. Weigh 30 grams of Kaneka Green Planet X151A fine powder. If the raw material is in pellet form, it needs to be pre - micronized to an initial average particle size of 5 to 20 microns, and slowly add it to the corresponding amount of the above - mentioned PVA 1788 aqueous solution so that the total solid content is 30 wt%, the total emulsion amount is 200 grams, and use a high - speed stirrer to stir for 60 minutes to obtain a preliminary mixture. Transfer this mixture to a high - pressure homogenizer HPH, set the homogenization pressure to 150 MPa, and perform 5 cycles of homogenization treatment. During the process, control the material temperature < 70 °C through a cooling jacket or other means. Obtain Emulsion 3. This emulsion is characterized by dynamic light scattering DLS. The average particle size of PHA particles is 190 nm, and PDI is equal to 0.24. The Zeta potential is measured using a Malvern Zetasizer Nano ZS at 25 °C with deionized water as the dispersion medium, and the result is - 32 mV. The viscosity of the emulsion at 25 °C is 800 mPa·s, and after standing for 30 days at 25 °C, there is no obvious layering visually, and the sedimentation rate is < 5% after centrifugation at 3000 rpm for 15 minutes.

[0094] Example 4: Kaneka PHBH / PVA 1788 high - solid - content nano - emulsion (weight ratio of PHA to PVA is 50:50, ultrasonic method, total solid content 30 wt%)

[0095] Prepare a preliminary mixture of Kaneka PHBH / PVA 1788 according to the method of Example 3 with a total solid content of 30 wt%. Transfer this mixture to a container with a cooling cycle, use a probe - type ultrasonic processor with a power of 500 W and a frequency of 20 kHz, set the power to 70%, and use a pulsed mode, for example, work for 5 seconds and pause for 2 seconds, and perform ultrasonic treatment for 40 minutes. During the treatment process, control the material temperature < 60 °C through a cooling water bath. Obtain Emulsion 4. This emulsion is characterized by dynamic light scattering DLS. The average particle size of PHA particles is 230 nm, and PDI is equal to 0.27. The Zeta potential is measured using a Malvern Zetasizer Nano ZS at 25 °C with deionized water as the dispersion medium, and the result is - 29 mV. The viscosity of the emulsion at 25 °C is 750 mPa·s, and after standing for 30 days at 25 °C, there is no obvious layering visually, and the sedimentation rate is < 5% after centrifugation at 3000 rpm for 15 minutes.

[0096] Example 5: Tian'an PHBV / PVA 1799 high - solid - content nano - emulsion (weight ratio of PHA to PVA is 30:70, using the HPH method, homogenization pressure is 160 MPa, total solid content 35 wt%).

[0097] Dissolve PVA 1799 in deionized water to prepare a 24.5% by weight PVA aqueous solution, which can be heated to 90 °C to 95 °C to facilitate dissolution. Weigh 21 grams of Tianan Enmat Y1000P fine powder. If the raw material is in pellet form, it needs to be pre - micronized to an initial average particle size of 5 microns to 20 microns, and slowly add it to the corresponding amount of PVA 1799 aqueous solution, corresponding to 70 parts of PVA, and adjust the total solid content to 35 wt%, with a total emulsion amount of 200 grams. Stir with a high - speed stirrer for 60 minutes to obtain a preliminary mixture. Transfer this mixture to a high - pressure homogenizer HPH, set the homogenization pressure at 160 MPa, and perform 5 cycles of homogenization treatment, controlling the material temperature < 75 °C. Emulsion 5 is obtained. This emulsion is characterized by dynamic light scattering DLS. The average particle size of PHA particles is 175 nanometers, and the PDI is equal to 0.23. The Zeta potential is measured using a Malvern Zetasizer Nano ZS at 25 °C with deionized water as the dispersion medium, and the result is - 33 mV. The viscosity of the emulsion at 25 °C is 1100 mPa·s, and after standing at 25 °C for 30 days, there is no obvious layering visually, and the sedimentation rate is < 5% after centrifugation at 3000 rpm for 15 minutes. Coat this emulsion on unsized kraft paper with a dry weight coating amount of 5 g / m² and dry at 80 °C for 5 minutes. Coating properties: WVTR is 58 g / (m²·24 h), OTR is 11 cm³ / (m²·24 h·atm), the oil - resistance grade is 10, and the contact angle is 96°.

[0098] Example 6: Study on different coating amounts using high - solid - content emulsions (based on the emulsion of Example 1, PHA:PVA is 70:30, total solid content 40 wt%)

[0099] Use the same emulsion preparation method as in Example 1 to prepare an emulsion with PHA:PVA of 70:30 and a total solid content of 40 wt%. Coat this emulsion on unsized kraft paper respectively, and control the dry weight coating amounts to be 3 g / m² and 10 g / m². After coating, dry in an 80 °C oven for 5 minutes. Coating amount 3 g / m²: WVTR is 55 g / (m²·24 h), OTR is 13 cm³ / (m²·24 h·atm), the oil - resistance grade is 9, and the contact angle is 96°. Coating amount 10 g / m²: WVTR is 38 g / (m²·24 h), OTR is 6 cm³ / (m²·24 h·atm), the oil - resistance grade is 11, and the contact angle is 103°. The Zeta potential of this emulsion (Example 1) is - 34 mV. After standing at 25 °C for 30 days, there is no obvious layering visually, and the sedimentation rate is < 5% after centrifugation at 3000 rpm for 15 minutes.

[0100] Coating and performance testing

[0101] The emulsions prepared in Examples 1 to 6, as well as the pure PVA 1788 solution as Comparative Example 1, with a solid content similar to the total solid content of Example 3, were coated using an optimized coating process: coated on one surface of an IPACK STRONG PRO 80 g / ㎡ unsized kraft paper produced by MM Group using a wire bar coater, controlling the dry weight coating amount to be 5 g / ㎡. Except for Example 6, Example 6 was tested according to its specific coating amount. The coated paper samples were dried in an oven at 80°C for 5 minutes. The obtained coated paper samples were subjected to performance tests together with the untreated kraft paper base paper - i.e., Comparative Example 2 (MM Group IPACK STRONG PRO 80 g / ㎡) - and the CKB PE 15 commercial PE laminated kraft paper produced by Stora Enso - i.e., Comparative Example 3.

[0102] Test items and methods:

[0103] Coating amount: Calculate the mass per unit area of the dried coating by the weighing method.

[0104] Water vapor transmission rate WVTR: According to ASTM E96 / E96M, using the water cup method, the test conditions are 38°C, 90%RH.

[0105] Oxygen transmission rate OTR: According to ASTM D3985, tested using instruments such as MOCON, the conditions are 23°C, 50%RH.

[0106] Oil resistance grade Kit: According to the TAPPI T559 standard, use the Kit test solution to test the grease penetration resistance of the coating, and record the highest non-permeation grade.

[0107] Adhesion evaluation: Adopt the tape peeling method, similar to the ASTM D3359 method, and observe the situation of the coating being peeled off by the tape.

[0108] Contact angle: Use a contact angle measuring instrument to measure the static contact angle of water droplets on the coating surface.

[0109] Biodegradability test: Conducted according to the EN 13432 standard. The coated paper samples were tested under standard composting conditions, and their biodegradation rates within 180 days were monitored.

[0110] Comparative analysis of performance test results

[0111] Table 3 below summarizes the main performance test results of some samples:

[0112]

[0113] Analysis of the test results in Table 3 is as follows:

[0114] Emulsion Stability and Particle Characteristics: As determined by dynamic light scattering technology in this invention, the average particle size of PHA particles in the optimized PHA / PVA nanoemulsion can be precisely controlled at around 150 nm, and the PDI value is 0.2, indicating that the particle size distribution is very uniform. Zeta potential tests show that the emulsion particle surface carries a charge of -30 mV to -40 mV, and this negative charge provides electrostatic repulsion, effectively preventing particle aggregation and ensuring the physical stability of the emulsion during storage and use. The stability test further verifies this: after standing at 25°C for 30 days, there is no visible layering in the emulsion; after centrifuging at 3000 rpm for 15 minutes, the sedimentation rate < 5%, showing excellent centrifugal stability. Even under high solid content conditions (30 wt% to 55 wt%) as shown in Examples 1 - 6, by adjusting the homogenization process parameters and PVA concentration, nanoemulsions meeting the requirements can still be obtained. These characteristics indicate that the emulsion has good leveling properties and coating applicability, and can form a uniform and dense barrier film on paper-based materials.

[0115] Formulation Optimization and Improvement of Barrier Performance: Through the formulation optimization experiments shown in Table 2, it is shown that the weight ratio of PHA to PVA has a significant impact on the barrier performance of the coating. When the PHA:PVA ratio is 70:30, the coating exhibits the best comprehensive performance:

[0116] Water Vapor Transmission Rate (WVTR): 45 g / (m²·24 h) (38°C, 90% RH);

[0117] Oxygen Transmission Rate (OTR): 8 cm³ / (m²·24 h·atm) (23°C, 50% RH);

[0118] Contact Angle: 100°, showing excellent hydrophobicity.

[0119] At this ratio, the hydrophobicity of PHA and the film-forming property and oxygen barrier property of PVA reach the best balance. The high hydrophobicity of PHA reduces the permeation of water vapor, while the molecular chain structure of PVA enhances the oxygen barrier ability, and the two work together to form a uniform and dense barrier film. This result indicates that 70:30 is a preferred formulation for achieving high barrier performance.

[0120] Effect of Coating Amount on Barrier Performance: Example 6 studied the effect of different coating amounts on the barrier performance under the PHA:PVA = 70:30 formulation (total solid content of the emulsion is 40 wt%), and the results are as follows:

[0121] Coating amount 3 g / m²:

[0122] WVTR is 55 g / (m²·24 h);

[0123] OTR is 13 cm³ / (m²·24 h·atm);

[0124] The oil resistance level is 9;

[0125] The contact angle is 96°.

[0126] Coating weight 10 g / m²:

[0127] WVTR is 38 g / (m²·24 h);

[0128] OTR is 6 cm³ / (m²·24 h·atm);

[0129] The oil resistance level is 11;

[0130] The contact angle is 103°.

[0131] Compared with the coating weight of 5 g / m², as in Example 1, WVTR = 46 g / (m²·24 h) and OTR = 8 cm³ / (m²·24 h·atm)), the increase in coating weight significantly improves the barrier performance and hydrophobicity. At 10 g / m², both WVTR and OTR reach the optimal values, indicating that the increase in coating thickness extends the penetration paths of gas and water vapor, thus enhancing the barrier effect.

[0132] Properties of the high solid content emulsion coating: Different high solid content emulsions prepared from Examples 1 to 5, at the same coating weight of 5 g / m², their coating properties are shown in Table 3, all showing excellent performance, all meeting the requirements of WVTR < 100 g / (m²·24 h) and OTR < 50 cm³ / (m²·24 h·atm), while maintaining good oil resistance and hydrophobicity. This indicates that the method of the present invention can prepare a high solid content and excellent performance nano-barrier emulsion.

[0133] Performance comparison with the comparative example:

[0134] Taking Examples 1 and 2 of the coating of the present invention as examples, the performance comparison with the comparative example is as follows:

[0135] Pure PVA coating, Comparative Example 1:

[0136] Under high humidity conditions: WVTR > 300 g / (m²·24 h);

[0137] Under high humidity conditions: OTR > 100 cm³ / (m²·24 h·atm);

[0138] Contact angle = 65°.

[0139] Analysis: Pure PVA has a sharp decline in barrier performance due to strong hydrophilicity under high humidity, and the moisture resistance is insufficient.

[0140] Untreated paper, Comparative Example 2:

[0141] WVTR > 500 g / (m²·24 h);

[0142] OTR > 10000 cm³ / (m²·24 h·atm);

[0143] Oil resistance level < 1;

[0144] Contact angle < 20°.

[0145] Analysis: The porous structure of the untreated paper results in extremely poor barrier properties and cannot meet the packaging requirements.

[0146] PE-coated paper, Comparative Example 3:

[0147] WVTR = 10 g / (m²·24 h);

[0148] OTR = 150 cm³ / (m²·24 h·atm);

[0149] Oil resistance level = 12;

[0150] Contact angle = 105°.

[0151] Analysis: PE-coated paper performs well in terms of water vapor and grease barrier, but has poor oxygen barrier and is non-degradable.

[0152] The coating of the present invention, Example 1:

[0153] WVTR = 46 g / (m²·24 h);

[0154] OTR = 8 cm³ / (m²·24 h·atm);

[0155] Oil resistance level = 11;

[0156] Contact angle = 101°.

[0157] The coating of the present invention, Example 2:

[0158] WVTR = 45 g / (m²·24 h);

[0159] OTR = 7 cm³ / (m²·24 h·atm);

[0160] Oil resistance level = 11;

[0161] Contact angle = 102°.

[0162] Analysis: The coating of the present invention, i.e., the coating prepared from high-solid content emulsion, still maintains excellent barrier properties under high humidity. Especially, the OTR is much lower than that of PE-coated paper, and it also has biodegradability, taking into account both environmental protection and functionality.

[0163] Surface properties and adhesion: As in Example 1 and Example 2, the surface contact angle of the coating of the present invention is as high as 101° to 102°, significantly higher than that of the pure PVA coating (65°) and the untreated paper (<20°), showing excellent hydrophobicity. This property benefits from the hydrophobic nature of PHA and the dense coating film formed by nano-sized particles. The tape peeling test shows that the coating has good adhesion to the paper substrate, with no peeling or only slight peeling, indicating that the emulsion coating prepared by the high-pressure homogenization method has excellent adhesion to the substrate and meets the requirements for durability in practical applications.

[0164] Biodegradability: According to the EN 13432 standard, under the standard composting conditions at 58°C, taking Example 1 as a representative sample, the biodegradation rate of the coating reaches 92% within 180 days, demonstrating its excellent biodegradation performance. As a biodegradable polyester, PHA can be decomposed in various environments, and PVA can also be degraded by microorganisms under specific conditions. The combination of the two makes the coating fully meet the environmental friendly requirements of sustainable packaging and solves the problem of non-degradability of traditional PE-coated paper.

[0165] Production feasibility and cost: The high-pressure homogenization process adopted in the present invention has been maturely applied in industry, with a pressure range of 50 - 200 MPa and a circulation times of 1 - 10 times. The process parameters are controllable and have the potential for large-scale production. The preliminary cost estimate shows that at a coating amount of 5 g / m², the material cost is $0.05 per square meter, which has certain economic competitiveness compared with traditional materials such as PE-coated paper. At the same time, the use of organic solvents is avoided, reducing the environmental cost. Using high-solid-content emulsion for production can significantly reduce the energy and time required for water evaporation, thereby reducing the drying cost, improving the output efficiency of the production line, and further enhancing the overall economic efficiency.

[0166] In summary, the PHA / PVA nano-scale paper-based barrier emulsion and its preparation method provided by the present invention, through nano-technology and formulation optimization, successfully combine the hydrophobicity of PHA with the film-forming property and oxygen barrier property of PVA, significantly improving the comprehensive barrier performance of the paper-based material. The emulsion has a small particle size of 150 nm, high stability, and the Zeta potential is usually between -30 mV and -45 mV, with no delamination in 30 days. The coating performs well under high humidity, with low WVTR and OTR values, overcoming the bottleneck of poor moisture resistance of pure PVA. Compared with PE-coated paper, the present invention has better oxygen barrier performance and biodegradability, with a degradation rate of 92% in 180 days. The preparation process is environmentally friendly, and it can prepare high-solid-content emulsion with up to 55%. The cost is controllable at $0.05 per square meter, suitable for industrial production, showing great potential to replace traditional coatings and meet the needs of sustainable packaging.

[0167] The above embodiments are only for illustrating the technical solutions of the present invention, rather than limiting the scope thereof. Those skilled in the art can make various modifications, equivalent substitutions or variations to the above embodiments without departing from the principle and spirit of the present invention, and all such modifications, equivalent substitutions or variations should be included within the protection scope defined by the claims of the present invention.

Claims

1. A PHA / PVA nano-scale paper-based barrier emulsion, characterized in that, The emulsion is an aqueous emulsion and contains: Polyhydroxyalkanoate (PHA) particles; Polyvinyl alcohol (PVA); Wherein, the average particle size of the PHA particles in the emulsion is 100 nanometers to 300 nanometers, the weight ratio of the PHA to the PVA is 30:70 to 70:30, and the polydispersity index (PDI) of the particle size distribution of the PHA particles is ≤ 0.3 as measured according to the ISO 22412:2017 standard.

2. The emulsion according to claim 1, characterized in that, The PHA is selected from polyhydroxybutyrate (PHB), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBHHx), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (P3HB4HB), or a mixture thereof.

3. The emulsion according to claim 1 or 2, characterized in that, The degree of alcoholysis of the PVA is 75 mol% to 100 mol%, and its degree of polymerization is 300 to 2500.

4. The emulsion according to claim 1, wherein The total solid content of the emulsion is 30 wt% to 55 wt%.

5. A method for preparing the PHA / PVA nano-scale paper-based barrier emulsion according to any one of claims 1 to 4, characterized in that, Comprising the following steps: Step a. Providing a polyhydroxyalkanoate (PHA) raw material with an initial average particle size of 1 micrometer to 100 micrometers; Step b. Dissolving polyvinyl alcohol (PVA) in water to prepare a PVA aqueous solution; Step c. Mixing the PHA raw material in step a with the PVA aqueous solution in step b according to a weight ratio of 30:70 to 70:30 to obtain a PHA / PVA mixture; Step d. Subjecting the mixture obtained in step c to a nanosizing treatment to reduce the average particle size of the PHA particles in the mixture to 100 nanometers to 300 nanometers and the polydispersity index (PDI) of the particle size distribution to ≤ 0.3, wherein the material temperature during the nanosizing treatment process is controlled below 80°C.

6. The method according to claim 5, wherein The nanosizing treatment in step d is selected from high-pressure homogenization, ultrasonic treatment, microfluidic homogenization, high-speed shearing, ball milling, or a combination thereof.

7. The method according to claim 6, wherein The nanosizing treatment uses high-pressure homogenization, the homogenization pressure is 50 MPa to 200 MPa, and 1 to 10 cycles of treatment are carried out.

8. Use of the PHA / PVA nanoscale paper-based barrier emulsion according to any one of claims 1 to 4 in the preparation of a paper-based barrier material.

9. A paper-based barrier material, characterized in that, Comprising a paper-based substrate and a barrier coating coated and cured on at least one surface of the paper-based substrate, wherein the barrier coating is derived from the PHA / PVA nanoscale paper-based barrier emulsion according to any one of claims 1 to 4.

10. The paper-based barrier material according to claim 9, wherein The dry weight coating amount of the barrier coating is 1 g / ㎡ to 30 g / ㎡; after the emulsion is coated on the paper-based substrate and dried into a film, the water vapor transmission rate (WVTR) of the formed barrier coating under the conditions of 38°C and 90% relative humidity is ≤ 100 g / (m²·24h); the oxygen transmission rate (OTR) under the conditions of 23°C and 50% relative humidity is < 50 cm³ / (m²·24h·atm).

Citation Information

Patent Citations

  • Environment-friendly cigarette package lined paper

    CN106049188A

  • High-barrier organic-inorganic paper-based composite material and preparation method thereof

    CN115976882A

  • Polyhydroxyalkanoate emulsion capable of forming film at low temperature as well as preparation method and application of polyhydroxyalkanoate emulsion

    CN116874816A

  • Degradable composite barrier coating applied to paper-based material

    CN117626703A

  • Polyhydroxyalkanoate (PHA) dispersions and methods of making same

    CN117769583A

Cited By

  • Pure bio-based PHA aqueous dispersion as well as preparation method and application thereof

    CN120865687A

  • Bamboo pulp paper-PHA double-sided composite soil biodegradable agricultural mulching film as well as preparation method and application thereof

    CN121473170A

  • Bamboo pulp paper-PHA double-sided composite soil biodegradable agricultural mulching film and its preparation method and use

    CN121473170B

  • Paper-based water-based barrier packaging material for pet food as well as preparation method and application thereof

    CN121473171A

  • PHA-containing low-odor low-VOC (volatile organic compound) water-based touch barrier glazing oil composition as well as preparation method and application thereof