By optimizing the material formulation and process parameters, a high-strength nanoscale chip packaging material with a three-layer composite structure was prepared, which solved the limitations of traditional materials in terms of mechanical properties, conductivity and optical properties, and achieved multi-scenario adaptability and reliability of high-end chip packaging.

CN120269890BActive Publication Date: 2026-11-20ZHEJIANG HANJING TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510396152.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-31
Publication Date
2026-11-20
Estimated Expiration
2045-03-31

AI Technical Summary

Technical Problem

Traditional chip packaging materials have limitations in terms of mechanical properties, conductivity, environmental adaptability, and optical properties, making it difficult to meet the needs of high-end applications, especially in high-frequency, high-density, and extreme environments.

Method used

By optimizing the material formulation and utilizing the synergistic effects of acrylonitrile-butadiene-styrene copolymer, polystyrene, conductive carbon black, and various additives, combined with precise process parameter control, a high-strength nanoscale chip packaging material with a three-layer composite structure was prepared, including a top layer, a bottom layer, and an intermediate layer. The mechanical properties, electrical conductivity, and optical effects of the material were improved by utilizing the addition reaction of methylallyl nickel chloride dimer with zirconium aminophthalate MOF and the modification of allyl phenyl selenide.

Benefits of technology

The prepared material possesses excellent mechanical properties, good electrical conductivity, and controllable optical effects, making it suitable for complex and varied chip packaging applications and improving chip packaging reliability and lifespan.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application discloses a kind of high-strength nanoscale chip packaging material preparation methods, it is related to packaging material technical field.The material is composed of surface layer, bottom layer and intermediate formula layer, using specific conductive masterbatch, ABS, PS, conductive carbon black, modified nylon and related auxiliary agent, by batching, feeding, stirring, extrusion, pressure roller, slitting and winding process preparation is formed.Its mechanical properties are superior, with high tensile strength, good elongation, stable gloss, low moisture content.The material of the application can be widely used in chip packaging field, with excellent electrical conductivity, mechanical stability and environmental protection characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of packaging materials technology, and in particular to a method for preparing a high-strength nanoscale chip packaging material. Background Technology

[0002] With the rapid development of electronic information technology, the demand for integrated circuit chips, as the core of the information industry, is increasing daily. Chip packaging technology, as a crucial step in chip manufacturing, plays a vital role in improving chip performance, protecting chip structure, and achieving functional integration. Chip packaging materials must simultaneously meet the requirements of high mechanical strength, good electrical conductivity, excellent heat resistance, and processability. This is especially true in high-frequency, high-density, and extreme environment applications, where the performance requirements for packaging materials are further enhanced.

[0003] Traditional chip packaging materials, such as epoxy resin and polyimide, while exhibiting good performance in some aspects, have limitations in mechanical properties, conductivity, and environmental adaptability. For example, epoxy resin has low tensile strength, is prone to stress cracking, and has poor conductivity, making it unsuitable for high-end applications requiring stable electrical contacts. While polyimide has good heat resistance, its processing performance is poor, its manufacturing process is highly dependent on equipment, and its processes are complex and expensive. Furthermore, traditional packaging materials typically cannot simultaneously optimize both mechanical and conductivity properties, limiting their application in high-performance chip packaging.

[0004] Furthermore, with the increasing operating frequency of electronic devices, the conductivity requirements for chip packaging materials are further enhanced. Traditional materials often exhibit poor dispersion of conductive fillers, leading to an unstable conductive network and consequently affecting the consistency of electrical performance. Simultaneously, the optical properties of packaging materials, such as gloss and surface quality, are increasingly becoming important indicators for evaluating high-end packaging materials. However, existing materials have limited capabilities in controlling optical performance, making it difficult to simultaneously meet the demands of both glossy and matte finish applications.

[0005] Therefore, there is an urgent need to develop a high-performance, easily processable chip packaging material that balances mechanical, electrical, and optical properties. By rationally designing material formulations and optimizing manufacturing processes, product performance can be improved while reducing production costs, providing a better solution for the chip packaging industry and meeting the needs of the modern electronics industry. Summary of the Invention

[0006] To address the aforementioned issues, developing a multifunctional encapsulation material with high mechanical strength, excellent conductivity, and environmental adaptability has become a key research focus. This invention, through optimized material formulation, including the synergistic effects of acrylonitrile-butadiene-styrene copolymer (ABS), polystyrene (PS), conductive carbon black, and various additives, combined with precise process parameter control, has developed a method for preparing a high-strength nanoscale chip encapsulation material. This material exhibits superior mechanical and electrical properties, with controllable surface gloss, meeting the needs of various application scenarios. It can significantly improve the packaging reliability and lifespan of chips, providing a reliable solution for high-end electronic devices.

[0007] To achieve the above objectives, the present invention provides the following technical solution:

[0008] A method for preparing a high-strength nanoscale chip packaging material, comprising:

[0009] Top and bottom layers: made of conductive masterbatch, selected from carbon black conductive masterbatch, graphite conductive masterbatch or a combination thereof; Intermediate layer: composed of 50-70 parts by weight of acrylonitrile-butadiene-styrene copolymer, 20-40 parts by weight of polystyrene, 5-15 parts by weight of conductive carbon black, 3-8 parts by weight of modified nylon, 0.5-2 parts of reinforcing agent, 0.1-0.5 parts of antioxidant, 0.1-0.5 parts of lubricant and 0.3-1 parts of toughening agent;

[0010] The three layers form the overall structure, with the top and bottom layers having a thickness of 0.02-0.05mm and the middle layer having a thickness of 0.1-0.5mm.

[0011] The method for preparing the reinforcing agent includes the following steps:

[0012] By weight, 0.05-0.5 parts of methylallyl nickel chloride dimer (CAS No.: 12145-60-7), 10-20 parts of zirconium aminophthalate MOF (CAS No.: 1260119-00-3), 200-300 parts of DMF and 2-5 parts of trimethylamine were stirred and reacted at 70-80°C for 100 to 150 minutes; then 0.2-0.5 parts of allyl phenyl selenide (CAS No.: 14370-82-2) were added, and the reaction was continued at 70-80°C for 50 to 120 minutes; DMF was removed by distillation to obtain the reinforcing agent.

[0013] The antioxidant is selected from type 1010 antioxidant or type 168 antioxidant.

[0014] The lubricant is selected from at least one of calcium stearate, zinc stearate, or polyethylene wax.

[0015] The toughening agent is selected from at least one of maleic anhydride-grafted polypropylene or hydrogenated styrene-butadiene-styrene copolymer.

[0016] The chip packaging material is prepared by the following steps:

[0017] (1) Ingredients: Weigh each component according to the following proportions: 50-70 parts by weight of acrylonitrile-butadiene-styrene copolymer, 20-40 parts by weight of polystyrene, 5-15 parts by weight of conductive carbon black, 3-8 parts by weight of modified nylon, 0.5-2 parts of reinforcing agent, 0.1-0.5 parts of antioxidant, 0.1-0.5 parts of lubricant and 0.3-1 parts of toughening agent;

[0018] (2) Feeding: Weigh the acrylonitrile-butadiene-styrene copolymer, polystyrene, conductive carbon black, modified nylon, reinforcing agent, antioxidant, lubricant and toughening agent and add them to the high-speed mixer in sequence;

[0019] (3) Stirring: Mix evenly at a stirring speed of 300-500 rpm for 10-15 minutes to ensure the mixture is uniform;

[0020] (4) Extrusion: The mixture is extruded through a twin-screw extruder. The extrusion temperature is controlled at 180-200℃ and the screw speed is 80-120rpm.

[0021] (5) Pressure roller: The extruded material is shaped by the pressure roller equipment, the thickness is adjusted to be within the range of 0.3-0.8mm, and the surface gloss is controlled. The gloss of the matte surface is 19-21 and the gloss of the bright surface is 71-83.

[0022] (6) Slitting: Trimming and cutting to the target size using a slitting device;

[0023] (7) Rewinding: The final product is rolled into a roll and stored in a dry environment.

[0024] Mechanism and technical effects:

[0025] The allyl-amino addition reaction between methylallyl nickel chloride dimer and zirconium aminophthalate MOF, and the similar reaction between allyl phenyl selenide and zirconium aminophthalate MOF, are key steps in the preparation of high-end chip packaging materials.

[0026] 1. Role of allyl nickel chloride dimer: As part of the reaction, the allyl group in the structure of the allyl nickel chloride dimer can undergo an addition reaction with the amino group in zirconium aminophthalate MOF to form a new chemical bond. This reaction helps to enhance the mechanical properties of the material because the newly formed chemical bonds can increase the crosslinking density and rigidity of the material.

[0027] Modification effect of allylphenyl selenide: Allylphenyl selenide is further modified into zirconium aminophthalate MOF through a similar addition reaction, introducing selenium. The introduction of selenium can endow the material with better electrical conductivity and optical properties because selenium is a semiconductor element that can form conductive pathways in the material.

[0028] 2. Influence of particle morphology

[0029] Zirconium aminophthalate (MOF), as a metal-organic framework material, comprises MOF particles with specific morphologies and sizes. After addition reactions, these particles can be uniformly dispersed within the matrix material, thereby improving the material's mechanical properties and stability. Simultaneously, particle morphology also influences the material's electrical conductivity and optical properties. Particles with specific shapes and sizes may be more conducive to electron transport and light scattering or absorption, thus improving the material's electrical conductivity and optical performance.

[0030] 3. Technical Effects

[0031] Excellent mechanical properties: The new chemical bonds introduced through the allyl-amino addition reaction and the uniformly dispersed MOF particles together improve the tensile strength and rigidity of the material.

[0032] Good electrical conductivity and optical properties: The introduction of selenium endows the material with good electrical conductivity, while the specific particle morphology helps to improve the material's optical properties.

[0033] In summary, the allyl-amino addition reaction between methylallyl nickel chloride dimer and zirconium aminophthalate MOF, and the similar reaction between allyl phenyl selenide and zirconium aminophthalate MOF, have led to the successful preparation of materials for high-end chip packaging by modifying molecular structure, considering steric hindrance, and controlling particle morphology. These materials not only possess excellent mechanical properties, good electrical conductivity, and optical effects, but also meet environmental protection requirements, making them suitable for complex and diverse chip packaging applications. Detailed Implementation

[0034] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0035] Example 1:

[0036] Ingredients:

[0037] Weigh out 50g of acrylonitrile-butadiene-styrene copolymer, 40g of polystyrene, 5g of conductive carbon black, 8g of modified nylon, 0.5g of reinforcing agent, 0.5g of type 1010 antioxidant, 0.1g of calcium stearate lubricant, and 1g of maleic anhydride-grafted polypropylene toughening agent.

[0038] Preparation of the reinforcing agent: 0.05 g of allyl nickel chloride dimer (CAS No.: 12145-60-7), 20 g of zirconium aminophthalate MOF (CAS No.: 1260119-00-3), 200 g of DMF and 5 g of trimethylamine were stirred and reacted at 70 °C for 150 minutes; then 0.2 g of allyl phenyl selenide (CAS No.: 14370-82-2) was added, and the reaction was continued at 70 °C for 120 minutes; DMF was removed by distillation to obtain the reinforcing agent.

[0039] Feeding:

[0040] The weighed acrylonitrile-butadiene-styrene copolymer, polystyrene, conductive carbon black, modified nylon, reinforcing agent, antioxidant, lubricant and toughening agent are added sequentially to the high-speed mixer.

[0041] Stir:

[0042] Mix thoroughly at 300 rpm for 15 minutes to ensure the mixture is homogeneous.

[0043] Extrusion:

[0044] The mixture is extruded through a twin-screw extruder, with the extrusion temperature controlled at 180℃ and the screw speed at 120 rpm.

[0045] Pressure roller:

[0046] The extruded material is shaped using a pressure roller device, with the thickness adjusted to 0.3mm, and the surface gloss controlled. The matte finish has a gloss level of 19, and the gloss finish has a gloss level of 71.

[0047] Slicing:

[0048] The edges are trimmed and cut to the target size using a slitting device.

[0049] End of issue:

[0050] The final product is rolled into rolls and stored in a dry environment.

[0051] The top and bottom layers are made of carbon black conductive masterbatch with a thickness of 0.02 mm; the middle layer has a thickness of 0.1 mm.

[0052] Example 2:

[0053] Ingredients:

[0054] Weigh out 60g of acrylonitrile-butadiene-styrene copolymer, 30g of polystyrene, 10g of conductive carbon black, 5g of modified nylon, 1g of reinforcing agent, 0.3g of type 168 antioxidant, 0.3g of zinc stearate lubricant, and 0.6g of hydrogenated styrene-butadiene-styrene copolymer toughening agent.

[0055] Preparation of the reinforcing agent: 0.3 g of allyl nickel chloride dimer (CAS No.: 12145-60-7), 15 g of zirconium aminophthalate MOF (CAS No.: 1260119-00-3), 250 g of DMF and 3 g of trimethylamine were stirred and reacted at 75 °C for 120 minutes; then 0.3 g of allyl phenyl selenide (CAS No.: 14370-82-2) was added, and the mixture was stirred and reacted at 75 °C for another 80 minutes; DMF was removed by distillation to obtain the reinforcing agent.

[0056] Feeding:

[0057] The weighed acrylonitrile-butadiene-styrene copolymer, polystyrene, conductive carbon black, modified nylon, reinforcing agent, antioxidant, lubricant and toughening agent are added sequentially to the high-speed mixer.

[0058] Stir:

[0059] Mix thoroughly at 400 rpm for 12 minutes to ensure the mixture is homogeneous.

[0060] Extrusion:

[0061] The mixture is extruded through a twin-screw extruder, with the extrusion temperature controlled at 190°C and the screw speed at 100 rpm.

[0062] Pressure roller:

[0063] The extruded material is shaped using a pressure roller device, with the thickness adjusted to 0.5mm, and the surface gloss controlled. The matte finish has a gloss level of 20, and the gloss finish has a gloss level of 77.

[0064] Slicing:

[0065] The edges are trimmed and cut to the target size using a slitting device.

[0066] End of issue:

[0067] The final product is rolled into rolls and stored in a dry environment.

[0068] The top and bottom layers are made of graphite conductive masterbatch with a thickness of 0.03 mm; the middle layer has a thickness of 0.3 mm.

[0069] Example 3:

[0070] Ingredients:

[0071] Weigh out 70g of acrylonitrile-butadiene-styrene copolymer, 20g of polystyrene, 15g of conductive carbon black, 3g of modified nylon, 1.5g of reinforcing agent, 0.1g of type 1010 antioxidant, 0.5g of polyethylene wax lubricant, and 0.3g of maleic anhydride grafted polypropylene toughening agent.

[0072] Preparation of the reinforcing agent: 0.5 g of allyl nickel chloride dimer (CAS No.: 12145-60-7), 10 g of zirconium aminophthalate MOF (CAS No.: 1260119-00-3), 300 g of DMF and 2 g of trimethylamine were stirred and reacted at 80 °C for 100 minutes; then 0.5 g of allyl phenyl selenide (CAS No.: 14370-82-2) was added, and the mixture was stirred and reacted at 80 °C for another 50 minutes; DMF was removed by distillation to obtain the reinforcing agent.

[0073] Feeding:

[0074] The weighed acrylonitrile-butadiene-styrene copolymer, polystyrene, conductive carbon black, modified nylon, reinforcing agent, antioxidant, lubricant and toughening agent are added sequentially to the high-speed mixer.

[0075] Stir:

[0076] Mix thoroughly at 500 rpm for 10 minutes to ensure the mixture is homogeneous.

[0077] Extrusion:

[0078] The mixture is extruded through a twin-screw extruder, with the extrusion temperature controlled at 200℃ and the screw speed at 80 rpm.

[0079] Pressure roller:

[0080] The extruded material is shaped using a pressure roller device, with the thickness adjusted to 0.8mm, and the surface gloss controlled. The matte finish has a gloss level of 21, and the gloss finish has a gloss level of 83.

[0081] Slicing:

[0082] The edges are trimmed and cut to the target size using a slitting device.

[0083] End of issue:

[0084] The final product is rolled into rolls and stored in a dry environment.

[0085] The top and bottom layers are made of a combination of carbon black and graphite conductive masterbatch, with a thickness of 0.05 mm; the middle layer has a thickness of 0.5 mm.

[0086] Example 4:

[0087] Ingredients:

[0088] Weigh out 55g of acrylonitrile-butadiene-styrene copolymer, 35g of polystyrene, 8g of conductive carbon black, 6g of modified nylon, 2g of reinforcing agent, 0.4g of type 168 antioxidant, 0.2g of calcium stearate and zinc stearate mixed lubricant (1:1 mixture) and 0.8g of hydrogenated styrene-butadiene-styrene copolymer toughening agent.

[0089] Preparation of the reinforcing agent: 0.2 g of allyl nickel chloride dimer (CAS No.: 12145-60-7), 18 g of zirconium aminophthalate MOF (CAS No.: 1260119-00-3), 220 g of DMF and 4 g of trimethylamine were stirred and reacted at 78 °C for 130 minutes; then 0.4 g of allyl phenyl selenide (CAS No.: 14370-82-2) was added, and the reaction was continued at 78 °C for 100 minutes; DMF was removed by distillation to obtain the reinforcing agent.

[0090] Feeding:

[0091] The weighed acrylonitrile-butadiene-styrene copolymer, polystyrene, conductive carbon black, modified nylon, reinforcing agent, antioxidant, lubricant and toughening agent are added sequentially to the high-speed mixer.

[0092] Stir:

[0093] Mix thoroughly at 350 rpm for 13 minutes to ensure the mixture is homogeneous.

[0094] Extrusion:

[0095] The mixture is extruded through a twin-screw extruder, with the extrusion temperature controlled at 185°C and the screw speed at 110 rpm.

[0096] Pressure roller:

[0097] The extruded material is shaped using a pressure roller device, with the thickness adjusted to 0.4mm, and the surface gloss controlled. The matte finish has a gloss level of 20, and the gloss finish has a gloss level of 75.

[0098] Slicing:

[0099] The edges are trimmed and cut to the target size using a slitting device.

[0100] End of issue:

[0101] The final product is rolled into rolls and stored in a dry environment.

[0102] The top and bottom layers are made of graphite conductive masterbatch with a thickness of 0.04 mm; the middle layer has a thickness of 0.2 mm.

[0103] Comparative Example 1:

[0104] This example serves as a comparative example of Example 1, differing from Example 1 only in that no reinforcing agent is added.

[0105] Comparative Example 2:

[0106] This example serves as a comparative example of Example 1, differing from Example 1 only in that: no methylallyl nickel chloride dimer is added during the preparation of the reinforcing agent.

[0107] Comparative Example 3:

[0108] This example serves as a comparative example of Example 1, differing from Example 1 only in that zirconium aminophthalate is not added during the preparation of the reinforcing agent.

[0109] Test method:

[0110] Tensile strength test: The tensile strength of the material is tested according to GB / T 1040 standard;

[0111] Elongation test: The elongation at break of the material is tested according to GB / T 1040 standard;

[0112] Moisture content test: The moisture content of the material was determined using an infrared moisture meter;

[0113] Density test: The material density was determined according to GB / T 1033 standard.

[0114] Test results:

[0115] Table 1. Test results of the examples and comparative examples.

[0116] Tensile strength (MPa) Elongation at break % Moisture content % <![CDATA[Density g / cm 3 > Example 1 32.2 81 0.18 1.05 Example 2 33.0 85 0.16 1.06 Example 3 33.5 88 0.15 1.05 Example 4 33.8 91 0.13 1.07 Comparative Example 1 28.9 70 0.24 1.03 Comparative Example 2 31.9 77 0.19 1.04 Comparative Example 3 30.5 74 0.21 1.04

[0117] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing a high-strength nanoscale chip packaging material, comprising: Top and bottom layers: made of conductive masterbatch, which is selected from carbon black conductive masterbatch, graphite conductive masterbatch or a combination thereof; Intermediate layer: composed of 50-70 parts by weight of acrylonitrile-butadiene-styrene copolymer, 20-40 parts by weight of polystyrene, 5-15 parts by weight of conductive carbon black, 3-8 parts by weight of modified nylon, 0.5-2 parts of reinforcing agent, 0.1-0.5 parts of antioxidant, 0.1-0.5 parts of lubricant and 0.3-1 parts of toughening agent; The three layers form an integral structure, with the top and bottom layers having a thickness of 0.02-0.05 mm and the middle layer having a thickness of 0.1-0.5 mm. The method for preparing the reinforcing agent includes the following steps: By weight, 0.05-0.5 parts of methylallyl nickel chloride dimer, 10-20 parts of zirconium aminophthalate MOF, 200-300 parts of DMF and 2-5 parts of trimethylamine are stirred and reacted at 70-80°C for 100 to 150 minutes; then 0.2-0.5 parts of allyl phenyl selenide are added, and the reaction is continued at 70-80°C for 50 to 120 minutes; DMF is removed by distillation to obtain the reinforcing agent.

2. The method for preparing a high-strength nanoscale chip packaging material according to claim 1, characterized in that: The antioxidant is selected from type 1010 antioxidant or type 168 antioxidant.

3. The method for preparing a high-strength nanoscale chip packaging material according to claim 1, characterized in that: The lubricant is selected from at least one of calcium stearate, zinc stearate, or polyethylene wax.

4. The method for preparing a high-strength nanoscale chip packaging material according to claim 1, characterized in that: The toughening agent is selected from at least one of maleic anhydride-grafted polypropylene or hydrogenated styrene-butadiene-styrene copolymer.

Citation Information

Patent Citations

  • Additive for modified plastic and preparation method thereof

    CN118772514A

  • Preparation method of transparent electrode and perovskite solar cell

    CN119031804A

  • Conductive polyester-based alloy sheet

    US5989723A