Environment-friendly non-silicon defoaming agent as well as preparation method and application thereof

By preparing an environmentally friendly non-silicon defoaming agent, the synergistic effect of polyetherester A and polyetherester B and the defoaming additives was solved, and the effect of rapid defoaming and long-lasting foam suppression was achieved.

CN120285623APending Publication Date: 2025-07-11JIANGSU SAIOUXINYUE DEFOAMER +1

Patent Information

Application Number
CN202510630237.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2025-07-11

AI Technical Summary

Technical Problem

The existing non-silicon defoaming agents have low defoaming and foam suppression performance in aqueous coatings, making it difficult to effectively control the generation of foam and extend the reaction cycle.

Method used

By mixing polyetherester A and polyetherester B with defoaming additives, emulsifiers, thickeners, hydrophobic particles, organic solvents and deionized water, an environmentally friendly non-silicon defoaming agent is formed. Using the synergistic effect of its amphiphilic structure and defoaming additives, it quickly defoams and lasts for long-term foam suppression.

Benefits of technology

It achieves the effect of rapid defoaming and long-lasting foam suppression, improves the performance of defoaming agent, is suitable for water-based coatings, and reduces the impact of foam on production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of fine chemical engineering preparations, in particular to an environment-friendly non-silicon defoaming agent as well as a preparation method and application thereof. 3.6 to 5.1 parts of a defoaming aid; 0.24 to 0.35 part of a thickening agent; 2-3 parts of a dispersing agent; 2.6 to 3.5 parts of an emulsifier; 18 to 25.3 parts of an organic solvent; 65 to 82 parts of deionized water; wherein the polyether ester A and the polyether ester B with amphiphilic structures in the polyether ester can be quickly spread on the surface of foam, carry hydrophobic components to permeate a liquid membrane and accelerate foam breakage, and the defoaming assistant A and the defoaming assistant B further promote the defoaming and foam inhibition performance of the defoaming agent by reducing competitive adsorption to the defoaming agent and delaying release of active molecules. Compared with the prior art, the method has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fine chemical preparations, and particularly to an environment-friendly non-silicon defoamer and its preparation method and application. Background Art

[0002] With the rapid development of the national economy, higher requirements are put forward for the industrial production capacity of all walks of life in our country. Foam is a major problem that cannot be ignored in industrial production and will bring great harm to industrial production. For example, in the production of beer, alcohol, and major antibiotics in medicine, etc., in various equipment such as fermentation tanks, reaction kettles, and cooking kettles during production, in order to prevent overflow losses caused by the appearance of foam, the feeding coefficient needs to be controlled, which greatly limits the production capacity; for another example, in the sizing process of paper mills, sugar mills' carbonation processes, and textile mills' weaving processes, foam overflow often causes the overflow of precious raw materials, resulting in unnecessary losses; there are also some specific industrial chemical reaction products with foam that will cause gas retention, prolong the reaction cycle, and cause unnecessary increase in power consumption; even worse, foam will pollute the environment and cause accidents. For example, a refinery in a city on the southeast coast of China suffered a major fire and heavy losses due to the overflow of residue oil foam and the failure to use a defoamer to defoam in time. Foam in industry not only causes waste of raw materials, but also poses a great threat to people's lives and property.

[0003] Therefore, in industrial production, in order to avoid the harm caused by foam and improve production efficiency, defoaming aids are usually added to reduce the impact of foam. At present, there are a variety of defoamers suitable for industrial production with different performances, which can be mainly divided into two categories: non-silicon defoamers and silicone defoamers. Common non-silicon defoamers use mineral oil, polyether, amide or fatty alcohol as active substances, and silicone defoamers use polysiloxane as active substances, which have advantages such as good chemical inertness, small surface tension, good thermal stability, and strong foam-breaking ability. However, its foam-inhibiting ability is poor, and a large amount is required to inhibit the generation of foam. Moreover, the compatibility of silicone defoamers with water-phase foaming systems is poor, and it is easy to produce silicon spots, which easily affects the performance of products. Therefore, non-silicon defoamers have developed rapidly.

[0004] In the prior art, for example, the patent technical literature CN104906832A discloses a polyether ester / mineral oil composite defoamer and its preparation method, including 10-20 parts of polyether ester, 19-37 parts of modified mineral oil, 1-10 parts of defoaming aid, and 2-14 parts of emulsifier by weight; the polyether ester is prepared by esterifying polyglycol and polypropylene glycol with a dibasic acid and then blocking the remaining hydroxyl groups with fatty acids. The preparation process is simple and the cost is low, and it can be used in water-based coatings, but the performance of this defoamer in terms of rapid defoaming and long-lasting foam inhibition still needs to be further improved.

[0005] Therefore, according to the above-mentioned related technologies, it is urgent to develop environmentally friendly non-silicon defoaming agents and their preparation methods and applications. Summary of the invention

[0006] In view of this, the purpose of the present invention is to propose an environmentally friendly non-silicon defoamer and a preparation method and application thereof, so as to solve the problem that the defoaming and anti-foaming performance of non-silicon defoamers in water-based coatings in the prior art is not high.

[0007] Based on the above purpose, the present invention provides an environmentally friendly non-silicon defoaming agent and a preparation method and application thereof.

[0008] Environmentally friendly non-silicon defoaming agent, including the following raw materials in parts by weight: Polyether ester 200-285 parts; defoaming agent 3.6-5.1 parts; thickener 0.24-0.35 parts; diffusant 2-3 parts; emulsifier 2.6-3.5 parts; organic solvent 18-25.3 parts; deionized water 65-82 parts; The polyether ester is obtained by mixing polyether ester A and polyether ester B in a mass ratio of 45-60:13-17; The polyether ester A is prepared from modified castor oil and stearic acid; The modified castor oil is prepared from castor oil, ethylene oxide and propylene oxide; The polyether ester B is prepared from pentaerythritol tetraglycidyl ether, methyl propylene glycol and stearic acid; The defoaming aid is obtained by mixing defoaming aid A and defoaming aid B in a mass ratio of 6.5-9:3.4-5.2; The defoaming agent A is prepared from polyether ester A and hydroxyethyl trimethyl ammonium chloride; The defoaming agent B is prepared from dibutyl phthalate and hydrophobic hollow silica microspheres; The thickener is hydrophilic fumed silica; The emulsifier is any one of Span, Tween, AEO-5 and AEO-7; The organic solvent is ethylene glycol; The diffusing agent is liquid paraffin.

[0009] Preferably, the preparation method of the polyether ester A is as follows: Step A1. Add castor oil, zinc-cobalt double metal cyanide, and phosphoric acid with a mass fraction of 85% into a reaction kettle, displace with nitrogen, heat up to 110°C - 140°C for dehydration for 3 - 4 h. Add the ethylene oxide and propylene oxide mixture into a feed tank, displace with nitrogen and set aside. After the reaction kettle is heated up to 140°C, introduce the propylene oxide and ethylene oxide mixture for reaction. The reaction temperature is 135°C - 155°C, and the reaction pressure is 0.05 MPa - 0.1 MPa. After the reaction is completed, carry out curing until there is no obvious pressure drop, remove monomers for 1 h, and cool down to below 90°C to obtain modified castor oil. Step A2. Put the modified castor oil and stearic acid into a reaction kettle, add a catalyst, displace with nitrogen, heat up the reaction kettle to 110°C - 130°C for reaction for 3 h - 5 h, dehydrate and cool down to below 90°C to obtain polyether ester A.

[0010] Preferably, in step A1, the mass ratio of the castor oil, zinc-cobalt double metal cyanide, phosphoric acid with a mass fraction of 85%, ethylene oxide, and propylene oxide is 100 - 240:0.009 - 0.02:0.015 - 0.03:30 - 68:163 - 285; The catalyst in step A2 is obtained by mixing p-toluenesulfonic acid and phosphorous acid in a mass ratio of 1.5 - 2:1; The mass ratio of the modified castor oil, stearic acid, and catalyst is 1800 - 2600:275 - 392:5.5 - 10; The temperature during dehydration is 120°C - 130°C, and the time is 1 h - 2 h.

[0011] Preferably, the preparation method of the polyether ester B is as follows: Step B1. Add pentaerythritol tetraglycidyl ether and methyl propanediol into a reactor, stir evenly at 30 - 40°C under nitrogen protection, then add tetramethylethylenediamine, heat under reflux, and carry out vacuum distillation to obtain a polyether compound; Step B2. Add the polyether compound and stearic acid into the reactor, mix evenly, then add p-toluenesulfonic acid, heat under reflux, and carry out vacuum dehydration to obtain polyether ester B.

[0012] Preferably, in step B1, the dosage ratio of pentaerythritol tetraglycidyl ether, methyl propanediol, and tetramethylethylenediamine is 1 mol:1.5 - 2.2 mol:2 - 2.6 g; The temperature during heating under reflux is 92 - 105°C, and the time is 5.5 - 6.5 h; In step B2, the dosage ratio of the polyether compound, stearic acid, and p-toluenesulfonic acid is 1 mol:1.2 - 1.7 mol:3.5 - 4 g; The temperature during heating under reflux is 120 - 130°C, and the time is 4 - 5.5 h.

[0013] Preferably, the preparation method of the defoaming auxiliary A is as follows: Add polyether ester A and xylene into a reaction kettle, mix evenly, add tetrabutyl titanate, heat up to 110 °C under a nitrogen atmosphere and maintain for 20 - 30 min, cool down to 70 - 80 °C, introduce 2 - hydroxyethyltrimethylammonium chloride, then heat up to 120 - 135 °C, react for 7 - 8.5 h, and perform vacuum distillation to obtain the defoaming auxiliary A; The dosage ratio of the polyether ester A, xylene, tetrabutyl titanate, and 2 - hydroxyethyltrimethylammonium chloride is 1600 - 2200 g: 500 - 700 mL: 8.2 - 14 g: 245 - 318 g.

[0014] Preferably, the preparation method of the defoaming auxiliary B is as follows: Step C1. Add sodium stearate into absolute ethanol, stir evenly at 35 - 45 °C, then add hollow silica microspheres, after heating under reflux, wash with ethanol 3 times and perform vacuum drying to obtain hydrophobic hollow silica microspheres; Step C2. Add dibutyl phthalate into absolute ethanol, stir evenly, then add hydrophobic hollow silica microspheres, stir at 300 - 400 rpm for 6 - 8 h, centrifuge and dry to obtain the defoaming auxiliary B.

[0015] Preferably, the dosage ratio of the sodium stearate, absolute ethanol, and hollow silica microspheres in Step C1 is 2.2 - 3.5 g: 30 - 40 mL: 18 - 24.6 g; The temperature during the heating under reflux is 82 - 95 °C and the time is 7 - 8 h; The temperature during the vacuum drying is 70 - 80 °C and the time is 1 - 2 h; The dosage ratio of the absolute ethanol, dibutyl phthalate, and hydrophobic hollow silica microspheres in Step C2 is 20 - 28 mL: 1.3 - 2 g: 8 - 14.5 g; The temperature during the drying is 45 - 55 °C and the time is 2.5 - 3 h.

[0016] The preparation method of the environment - friendly non - silicon defoaming agent includes the following steps: Add a thickener and an organic solvent into deionized water, after mixing evenly, add an emulsifier, stir at room temperature for 10 - 15 min, then sequentially add a dispersant, a defoaming auxiliary, and a polyether ester, and mix evenly to obtain the environment - friendly non - silicon defoaming agent.

[0017] The application of the environment - friendly non - silicon defoaming agent, the defoaming agent is used in water - based coatings.

[0018] The beneficial effects of the present invention: The present invention provides an environmentally friendly non-silicon defoamer and a preparation method and application thereof. The present invention obtains an environmentally friendly non-silicon defoamer capable of rapid defoaming and long-lasting foam suppression by mixing polyether ester A and polyether ester B, adding a defoaming aid, an emulsifier, a thickener, hydrophobic particles, an organic solvent, a diffusant and deionized water and mixing them uniformly. Among them, polyether ester A and polyether ester B with an amphiphilic structure can spread rapidly on the foam surface, carry hydrophobic components to penetrate the liquid film, and accelerate the foam bursting. The defoaming aid A and the defoaming aid B further promote the defoaming and foam suppression performance of the defoamer by reducing competitive adsorption of the defoamer and delaying the release of active molecules. Compared with the prior art, the present invention has a wide application prospect. DETAILED DESCRIPTION

[0019] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0020] The sources and properties of some of the raw materials used in the present invention are as follows: Zinc-cobalt double metal cyanide was purchased from Shanghai Myrel Chemical Technology Co., Ltd.; propylene oxide was purchased from Shandong Rongnuo Chemical Sales Co., Ltd.; ethylene oxide was purchased from Shandong Rongnuo Chemical Sales Co., Ltd.; castor oil was purchased from Wuhan Kemik Biomedicine Technology Co., Ltd.; stearic acid was purchased from Jiangsu Shuangma Chemical Co., Ltd.; pentaerythritol tetraglycidyl ether was purchased from Harbin Kemeis Technology Co., Ltd.; dibutyl phthalate was purchased from Zhejiang Jianye Chemical Co., Ltd.; and hydrophilic fumed silica was purchased from Lianmai Bio.

[0021] Embodiment 1: A method for preparing an environmentally friendly non-silicon defoaming agent, comprising the following steps: S1. 100g of castor oil, 0.009g of zinc-cobalt double metal cyanide and 0.015g of 85% phosphoric acid were added to the reactor, replaced with nitrogen, heated to 110°C for dehydration for 3h, 30g of ethylene oxide and 163g of propylene oxide were added to the feed tank, replaced with nitrogen for standby use, the reactor was heated to 140°C and then propylene oxide and ethylene oxide were introduced into the mixture for reaction, the reaction temperature was 135°C, the reaction pressure was 0.05MPa, and after the reaction was completed, it was aged until there was no obvious pressure drop, the monomer was removed for 1h, and the temperature was lowered to below 90°C to obtain modified castor oil; S2. 1800 g of modified castor oil and 275 g of stearic acid were put into a reactor, 5.5 g of p-toluenesulfonic acid and phosphorous acid were added in a mass ratio of 1.5:1 as a catalyst, and nitrogen was replaced. The reactor was heated to 110 ° C for 3 h, dehydrated at 120 ° C for 1 h, and cooled to below 90 ° C to obtain polyether ester A; S3. Add 1 mol of pentaerythritol tetraglycidyl ether and 1.5 mol of methylpropanediol into a reactor. Under nitrogen protection, stir evenly at 30 °C, then add 2 g of tetramethylethylenediamine, heat under reflux at 92 °C for 5.5 h, and perform vacuum distillation to obtain a polyether compound; S4. Add 1 mol of the polyether compound and 1.2 mol of stearic acid into the reactor. After mixing evenly, add 3.5 g of p-toluenesulfonic acid, heat under reflux at 120 °C for 4 h, and perform vacuum dehydration to obtain polyether ester B; S5. Add 1600 g of polyether ester A and 500 mL of xylene into a reaction kettle, mix evenly, add 8.2 g of tetrabutyl titanate, heat up to 110 °C under a nitrogen atmosphere and maintain for 20 min, cool down to 70 °C, introduce 245 g of hydroxyethyltrimethylammonium chloride, then heat up to 120 °C, react for 7 h, and perform vacuum distillation to obtain defoaming aid A; S6. Add 2.2 g of sodium stearate into 30 mL of absolute ethanol, stir evenly at 35 °C, then add 18 g of hollow silica microspheres, heat under reflux at 82 °C for 7 h, wash with ethanol 3 times, and vacuum dry at 70 °C for 1 h to obtain hydrophobic hollow silica microspheres; S7. Add 1.3 g of dibutyl phthalate into 20 mL of absolute ethanol, stir evenly, then add 8 g of hydrophobic hollow silica microspheres, stir at 300 rpm for 6 h, centrifuge, and dry at 45 °C for 2.5 h to obtain defoaming aid B; S8. Mix 6.5 g of defoaming aid A and 3.4 g of defoaming aid B to obtain a defoaming aid, then mix 45 g of polyether ester A and 13 g of polyether ester B to obtain a polyether ester. Add 0.24 g of hydrophilic fumed silica Hydrophilic-300 type, 18 g of ethylene glycol into 65 g of deionized water, mix evenly, then add 2.6 g of AEO-5, stir at room temperature for 10 min, and then successively add 2 g of liquid paraffin, 3.6 g of defoaming aid and 200 g of polyether ester, mix evenly to obtain an environment-friendly non-silicon defoamer.

[0022] Example 2: A preparation method of an environment-friendly non-silicon defoamer, comprising the following steps: S1. Add 150 g of castor oil, 0.013 g of zinc-cobalt double metal cyanide and 0.02 g of 85% phosphoric acid by mass into a reaction kettle, perform nitrogen replacement, heat up to 120 °C for dehydration for 3.5 h, add a mixture of 42 g of ethylene oxide and 204 g of propylene oxide into a feed tank, perform nitrogen replacement and reserve for use. After the reaction kettle is heated up to 140 °C, introduce the mixture of propylene oxide and ethylene oxide for reaction, the reaction temperature is 140 °C, the reaction pressure is 0.07 MPa. After the reaction is completed, perform aging until there is no obvious pressure drop, remove monomers for 1 h, and cool down to below 90 °C to obtain modified castor oil; S2. Put 2000 g of modified castor oil and 310 g of stearic acid into a reaction kettle, add 7.2 g of p-toluenesulfonic acid and a catalyst with a mass ratio of phosphorous acid of 1.7:1, conduct nitrogen displacement, heat the reaction kettle to 115 °C and react for 3.5 h, dehydrate at 125 °C for 1.5 h, and cool down to below 90 °C to obtain polyether ester A; S3. Add 1 mol of pentaerythritol tetraglycidyl ether and 1.7 mol of methylpropanediol into a reactor, stir evenly at 35 °C under nitrogen protection, then add 2.2 g of tetramethylethylenediamine, heat and reflux at 96 °C for 6 h, and conduct vacuum distillation to obtain a polyether compound; S4. Add 1 mol of polyether compound and 1.5 mol of stearic acid into the reactor, mix evenly, add 3.6 g of p-toluenesulfonic acid, heat and reflux at 125 °C for 4.5 h, and conduct vacuum dehydration to obtain polyether ester B; S5. Add 1800 g of polyether ester A and 570 mL of xylene into a reaction kettle, mix evenly, add 10 g of tetrabutyl titanate, heat up to 110 °C and maintain for 25 min under a nitrogen atmosphere, cool down to 75 °C, introduce 270 g of hydroxyethyltrimethylammonium chloride, then heat up to 125 °C and react for 7.5 h, and conduct vacuum distillation to obtain defoaming aid A; S8. Add 2.6 g of sodium stearate into 35 mL of absolute ethanol, stir evenly at 40 °C, then add 20.1 g of hollow silica microspheres, heat and reflux at 86 °C for 7.5 h, wash with ethanol 3 times, and vacuum dry at 75 °C for 1.5 h to obtain hydrophobic hollow silica microspheres; S7. Add 1.6 g of dibutyl phthalate into 23 mL of absolute ethanol, stir evenly, then add 10 g of hydrophobic hollow silica microspheres, stir at 350 rpm for 7 h, centrifuge, and dry at 50 °C for 2.5 h to obtain defoaming aid B; S8. Mix 7.3 g of defoaming aid A and 4 g of defoaming aid B to obtain a defoaming aid, then mix 50 g of polyether ester A and 14 g of polyether ester B to obtain a polyether ester, and add 0.27 g of hydrophilic fumed silica Hydrophilic-300 type, 20.9 g of ethylene glycol into 72 g of deionized water, mix evenly, add 2.85 g of AEO-5, stir at room temperature for 12 min, then sequentially add 2.4 g of liquid paraffin, 4.2 g of defoaming aid and 228 g of polyether ester, and mix evenly to obtain an environment-friendly non-silicon defoaming agent.

[0023] Example 3: A preparation method of an environment-friendly non-silicon defoaming agent, comprising the following steps: S1. 200g of castor oil, 0.016g of zinc-cobalt double metal cyanide and 0.025g of 85% phosphoric acid were added to a reactor, replaced with nitrogen, heated to 130°C for dehydration for 3.5h, 55g of ethylene oxide and 255g of propylene oxide mixture were added to a feed tank, replaced with nitrogen for standby use, the reactor was heated to 140°C and then propylene oxide and ethylene oxide mixture were introduced for reaction, the reaction temperature was 150°C, the reaction pressure was 0.08MPa, and after the reaction was completed, it was aged until there was no obvious pressure drop, the monomer was removed for 1h, and the temperature was lowered to below 90°C to obtain modified castor oil; S2. 2400 g of modified castor oil and 355 g of stearic acid were put into a reactor, 8 g of p-toluenesulfonic acid and phosphorous acid were added as a catalyst in a mass ratio of 1.8:1, and nitrogen was replaced. The reactor was heated to 120 ° C for 4.5 h, dehydrated at 125 ° C for 1.5 h, and cooled to below 90 ° C to obtain polyether ester A; S3. 1 mol of pentaerythritol tetraglycidyl ether and 2 mol of methyl propylene glycol were added to the reactor, stirred evenly at 35 ° C under nitrogen protection, and then 2.4 g of tetramethylethylenediamine was added, heated to reflux at 100 ° C for 6 h, and distilled under reduced pressure to obtain a polyether compound; S4. 1 mol of a polyether compound and 1.5 mol of stearic acid were added to the reactor, mixed evenly, and then 3.8 g of p-toluenesulfonic acid was added, heated under reflux at 125 ° C for 5 h, and vacuum-dehydrated to obtain polyether ester B; S5. 2000 g of polyether ester A and 620 mL of xylene were added to the reactor, mixed evenly, 12 g of tetrabutyl titanate was added, the temperature was raised to 110 ° C and maintained for 25 min under a nitrogen atmosphere, the temperature was lowered to 75 ° C, 279 g of hydroxyethyltrimethylammonium chloride was introduced, and then the temperature was raised to 130 ° C, the reaction was carried out for 8 h, and the defoaming agent A was obtained by distillation under reduced pressure; S6. 2.9 g of sodium stearate was added to 35 mL of anhydrous ethanol, stirred at 40 ° C, and then 22.5 g of hollow silica microspheres were added. After heating and reflux at 91 ° C for 7.5 h, the mixture was washed with ethanol three times and vacuum dried at 75 ° C for 1.5 h to obtain hydrophobic hollow silica microspheres; S7. Add 1.7 g of dibutyl phthalate to 25 mL of anhydrous ethanol, stir evenly, then add 12.3 g of hydrophobic hollow silica microspheres, stir at 370 rpm for 7.5 h, centrifuge, and dry at 50 ° C for 2.5 h to obtain a defoaming agent B; S8. Mix 8.2 g of antifoaming aid A and 4.5 g of antifoaming aid B to obtain an antifoaming aid. Then mix 55 g of polyether ester A and 15 g of polyether ester B to obtain a polyether ester. Add 0.3 g of hydrophilic fumed silica type Hydrophilic-300 and 23 g of ethylene glycol to 77 g of deionized water, mix evenly, add 3.2 g of AEO-5, stir at room temperature for 14 min, then add 2.7 g of liquid paraffin, 4.7 g of antifoaming aid and 255 g of polyether ester in sequence, and mix evenly to obtain an environmentally friendly non-silicon antifoaming agent.

[0024] Example 4: A preparation method of an environmentally friendly non-silicon antifoaming agent, comprising the following steps: S1. Add 240 g of castor oil, 0.02 g of zinc-cobalt double metal cyanide and 0.03 g of phosphoric acid with a mass fraction of 85% to a reaction kettle, displace with nitrogen, heat up to 140 °C to dehydrate for 4 h. Add a mixture of 68 g of ethylene oxide and 285 g of propylene oxide to a feed tank, displace with nitrogen and reserve. After the reaction kettle is heated up to 140 °C, introduce the mixture of propylene oxide and ethylene oxide for reaction. The reaction temperature is 155 °C and the reaction pressure is 0.1 MPa. After the reaction is completed, carry out aging until there is no obvious pressure drop, remove monomers for 1 h, and cool down to below 90 °C to obtain modified castor oil. S2. Put 2600 g of modified castor oil and 392 g of stearic acid into a reaction kettle, add 10 g of p-toluenesulfonic acid and a catalyst with a mass ratio of phosphorous acid of 2:1, carry out nitrogen displacement, heat up the reaction kettle to 130 °C for reaction for 5 h, dehydrate at 130 °C for 2 h, and cool down to below 90 °C to obtain polyether ester A. S3. Add 1 mol of pentaerythritol tetraglycidyl ether and 2.2 mol of methylpropanediol to a reactor, stir evenly at 40 °C under nitrogen protection, then add 2.6 g of tetramethylethylenediamine, heat and reflux at 105 °C for 6.5 h, and carry out vacuum distillation to obtain a polyether compound. S4. Add 1 mol of polyether compound and 1.7 mol of stearic acid to the reactor, mix evenly, add 4 g of p-toluenesulfonic acid, heat and reflux at 130 °C for 5.5 h, and carry out vacuum dehydration to obtain polyether ester B. S5. Put 2200 g of polyether ester A and 700 mL of xylene into a reaction kettle, mix evenly, add 14 g of tetrabutyl titanate, heat up to 110 °C and maintain for 30 min under a nitrogen atmosphere, cool down to 80 °C, introduce 318 g of hydroxyethyltrimethylammonium chloride, then heat up to 135 °C, react for 8.5 h, and carry out vacuum distillation to obtain antifoaming aid A. S6. Add 3.5 g of sodium stearate to 40 mL of absolute ethanol, stir evenly at 45 °C, then add 24.6 g of hollow silica microspheres, heat and reflux at 95 °C for 8 h, wash with ethanol 3 times, and vacuum dry at 80 °C for 2 h to obtain hydrophobic hollow silica microspheres. S7. Add 2 g of dibutyl phthalate to 28 mL of absolute ethanol, stir evenly, then add 14.5 g of hydrophobic hollow silica microspheres, stir at 400 rpm for 8 h, centrifuge, and dry at 55 °C for 3 h to obtain defoaming aid B; S8. Mix 9 g of defoaming aid A and 5.2 g of defoaming aid B to obtain a defoaming aid. Then mix 60 g of polyether ester A and 17 g of polyether ester B to obtain a polyether ester. Add 0.35 g of hydrophilic fumed silica Hydrophilic - 300 type and 25.3 g of ethylene glycol to 82 g of deionized water, mix evenly, add 3.5 g of AEO - 5, stir at room temperature for 15 min, then add 3 g of liquid paraffin, 5.1 g of defoaming aid, and 285 g of polyether ester in sequence, and mix evenly to obtain an environmentally friendly non - silicon defoaming agent.

[0025] Comparative Example 1: Compared with Example 1, polyether ester A was not added during the preparation of the non - silicon defoaming agent in this comparative example, and the remaining steps and parameters were the same. This comparative example will not be repeated here, and finally an environmentally friendly non - silicon defoaming agent was obtained.

[0026] Comparative Example 2: Compared with Example 1, polyether ester B was not added during the preparation of the non - silicon defoaming agent in this comparative example, and the remaining steps and parameters were the same. This comparative example will not be repeated here, and finally an environmentally friendly non - silicon defoaming agent was obtained.

[0027] Comparative Example 3: Compared with Example 1, defoaming aid A was not added during the preparation of the non - silicon defoaming agent in this comparative example, and the remaining steps and parameters were the same. This comparative example will not be repeated here, and finally an environmentally friendly non - silicon defoaming agent was obtained.

[0028] Comparative Example 4: Compared with Example 1, defoaming aid B was not added during the preparation of the non - silicon defoaming agent in this comparative example, and the remaining steps and parameters were the same. This comparative example will not be repeated here, and finally an environmentally friendly non - silicon defoaming agent was obtained.

[0029] Comparative Example 5: Compared with Example 1, no defoaming aid was added during the preparation of the non - silicon defoaming agent in this comparative example, and the remaining steps and parameters were the same. This comparative example will not be repeated here, and finally an environmentally friendly non - silicon defoaming agent was obtained.

[0030] Comparative Example 6: Compared with Example 1, hydrophilic fumed silica was not added during the preparation of the non - silicon defoaming agent in this comparative example, and the remaining steps and parameters were the same. This comparative example will not be repeated here, and finally an environmentally friendly non - silicon defoaming agent was obtained.

[0031] Comparative Example 7: This comparative example is the same as Example 1 except that "6.5 g of antifoaming aid A and 3.4 g of antifoaming aid B" is replaced with "6.5 g of antifoaming aid A and 6.5 g of antifoaming aid B". The remaining steps and parameters are the same, so this comparative example will not be repeated here. Finally, an environmentally friendly non-silicon antifoaming agent is obtained.

[0032] Comparative Example 8: This comparative example is the same as Example 1 except that "6.5 g of antifoaming aid A and 3.4 g of antifoaming aid B" is replaced with "3.4 g of antifoaming aid A and 6.5 g of antifoaming aid B". The remaining steps and parameters are the same, so this comparative example will not be repeated here. Finally, an environmentally friendly non-silicon antifoaming agent is obtained.

[0033] Comparative Example 9: This comparative example is the same as Example 1 except that "45 g of polyether ester A and 13 g of polyether ester B" is replaced with "45 g of polyether ester A and 45 g of polyether ester B". The remaining steps and parameters are the same, so this comparative example will not be repeated here. Finally, an environmentally friendly non-silicon antifoaming agent is obtained.

[0034] Comparative Example 10: This comparative example is the same as Example 1 except that "45 g of polyether ester A and 13 g of polyether ester B" is replaced with "13 g of polyether ester A and 45 g of polyether ester B". The remaining steps and parameters are the same, so this comparative example will not be repeated here. Finally, an environmentally friendly non-silicon antifoaming agent is obtained.

[0035] Comparative Example 11: This comparative example is the same as Example 1 except that "antifoaming aid B" is replaced with "dibutyl phthalate". The remaining steps and parameters are the same, so this comparative example will not be repeated here. Finally, an environmentally friendly non-silicon antifoaming agent is obtained.

[0036] Performance test: First defoaming and antifoaming performance test: Add 200 ml of the prepared coating into a 1000 ml cup, and then add 0.3% of the antifoaming agents prepared in Examples 1 - 4 and Comparative Examples 1 - 11 respectively. Use a laboratory high-speed disperser to disperse at a speed of 1000 rpm for 10 min. After stopping, immediately pour it into a 1000 ml graduated cylinder, record the weight and volume of the liquid, and calculate the specific gravity. The larger the specific gravity value, the smaller the gas content, indicating better antifoaming performance of the antifoaming agent; Coating brushing test: Let the coating after high-speed dispersion stand for 15 min, take out a little of the standing liquid and drop it on a clean glass plate, and use a wet film applicator to evenly scrape the emulsion flat. Observe the state (shrinking hole situation) of the emulsion on the glass plate. The higher the grade, the better the compatibility; Second defoaming and antifoaming performance test: Leave the coating that has been tested for defoaming and foam suppression ability for 7 days. Pour it into a 1000 ml graduated cylinder again, record the weight and volume of the liquid, and calculate the specific gravity. A larger specific gravity value indicates a smaller gas content, indicating good foam suppression performance of the defoamer.

[0037] Table 1

[0038] Table 2

[0039] Data analysis: As can be seen from Table 1 and Table 2, the non-silicon defoamer prepared by the present invention has better defoaming and foam suppression performance. This may be because the hydrophobic castor oil long chain in polyether ester A inserts into the foam liquid film, destroying the surface tension balance, promoting the drainage and thinning of the liquid film, while the hydrophilic polyether chain can interact with the liquid film to inhibit foam regeneration. This amphiphilic structure enables polyether ester A to spread rapidly on the foam surface, carry the hydrophobic component to penetrate the liquid film, and accelerate foam rupture; the star-shaped polyether backbone in polyether ester B makes the molecule easier to diffuse in the foam system, shortening the time to reach the interface and achieving the effect of rapid defoaming; and defoaming aid A is prepared from polyether ester A and quaternary ammonium salt. On the one hand, it can neutralize the anionic impurities in the foam liquid film, destroy the electrostatic stable layer of the foam, and accelerate the drainage of the liquid film; on the other hand, it can combine with anionic surfactants through electrostatic interaction, reduce their competitive adsorption on the defoamer, avoid the encapsulation and inactivation of the polyether ester defoamer by the anionic system, and can also form a hydrogen bond network with polyether ester to play a synergistic role and reduce the interfacial energy; the low-density hollow silica microspheres in defoaming aid B make the molecule easy to migrate to the gas-liquid interface. On the one hand, the loaded dibutyl phthalate is more likely to penetrate into the foam liquid film, interfere with the arrangement of surfactant molecules, accelerate the drainage of the liquid film, and this structure can also further improve the stability and defoaming activity of the molecule, achieving the effect of long-lasting defoaming by slowly releasing dibutyl phthalate; on the other hand, it plays a synergistic role with hydrophilic fumed silica, acts on the surfactant together, destroys the local structure of the foam film, accelerates foam rupture, and can also prevent the stratification and sedimentation of the defoamer, improving the stability of the system.

[0040] Those of ordinary skill in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations in different aspects of the present invention as described above, which are not provided in detail for the sake of brevity.

[0041] The present invention aims to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention shall be included within the protection scope of the present invention.

Claims

1. Environmentally friendly non-silicon defoamer, characterized in that, Including the following raw materials by weight: Polyether ester 200-285 parts; defoaming agent 3.6-5.1 parts; thickener 0.24-0.35 parts; diffusant 2-3 parts; emulsifier 2.6-3.5 parts; organic solvent 18-25.3 parts; deionized water 65-82 parts; The polyether ester is obtained by mixing polyether ester A and polyether ester B in a mass ratio of 45-60:13-17; The polyether ester A is prepared from modified castor oil and stearic acid; The modified castor oil is prepared from castor oil, ethylene oxide and propylene oxide; The polyether ester B is prepared from pentaerythritol tetraglycidyl ether, methyl propylene glycol and stearic acid; The defoaming aid is obtained by mixing defoaming aid A and defoaming aid B in a mass ratio of 6.5-9:3.4-5.2; The defoaming agent A is prepared from polyether ester A and hydroxyethyl trimethyl ammonium chloride; The defoaming agent B is prepared from dibutyl phthalate and hydrophobic hollow silica microspheres; The thickener is hydrophilic fumed silica; The emulsifier is any one of Span, Tween, AEO-5 and AEO-7; The organic solvent is ethylene glycol; The diffusing agent is liquid paraffin.

2. The environmentally friendly non-silicon defoamer according to claim 1, characterized in that, The preparation method of the polyether ester A is as follows: Step A1. Castor oil, zinc-cobalt double metal cyanide and 85% by mass phosphoric acid are added to a reactor, replaced with nitrogen, heated to 110°C-140°C for dehydration for 3-4h, ethylene oxide and propylene oxide mixture are added to a feed tank, replaced with nitrogen for standby use, the reactor is heated to 140°C and then propylene oxide and ethylene oxide mixture are introduced for reaction, the reaction temperature is 135°C-155°C, the reaction pressure is 0.05MPa-0.1MPa, and after the reaction is completed, ripening is carried out until there is no obvious pressure drop, the monomer is removed for 1h, and the temperature is lowered to below 90°C to obtain modified castor oil; Step A2. Put modified castor oil and stearic acid into a reactor, add a catalyst, and replace with nitrogen. Heat the reactor to 110°C-130°C for 3h-5h, dehydrate and cool to below 90°C to obtain polyether ester A.

3. The environmentally friendly non-silicon defoamer according to claim 2, wherein The mass ratio of castor oil, zinc-cobalt double metal cyanide, 85% phosphoric acid, ethylene oxide and propylene oxide in step A1 is 100-240: 0.009-0.02: 0.015-0.03: 30-68: 163-285; The catalyst in step A2 is obtained by mixing p-toluenesulfonic acid and phosphorous acid in a mass ratio of 1.5-2:1; The mass ratio of the modified castor oil, stearic acid and catalyst is 1800-2600:275-392:5.5-10; The temperature during the dehydration is 120° C.-130° C. and the time is 1 h-2 h.

4. The environmentally friendly non-silicon defoamer according to claim 1, characterized in that The preparation method of the polyether ester B is as follows: Step B1. Add pentaerythritol tetraglycidyl ether and methyl propylene glycol into a reactor, stir evenly at 30-40° C. under nitrogen protection, then add tetramethylethylenediamine, heat to reflux, and distill under reduced pressure to obtain a polyether compound; Step B2. Add a polyether compound and stearic acid into a reactor. After mixing evenly, add p-toluenesulfonic acid, heat under reflux, and dehydrate under vacuum to obtain polyether ester B.

5. The environmentally friendly non-silicon defoamer according to claim 4, wherein In step B1, the dosage ratio of pentaerythritol tetraglycidyl ether, methylpropanediol, and tetramethylethylenediamine is 1 mol: 1.5 - 2.2 mol: 2 - 2.6 g; The temperature during the heating under reflux is 92 - 105 °C, and the time is 5.5 - 6.5 h; In step B2, the dosage ratio of the polyether compound, stearic acid, and p-toluenesulfonic acid is 1 mol: 1.2 - 1.7 mol: 3.5 - 4 g; The temperature during the heating under reflux is 120 - 130 °C, and the time is 4 - 5.5 h.

6. The environmentally friendly non-silicon defoamer according to claim 1, characterized in that The preparation method of the defoaming auxiliary A is as follows: Add polyether ester A and xylene into a reaction kettle, mix evenly, add tetrabutyl titanate, heat up to 110 °C under a nitrogen atmosphere and maintain for 20 - 30 min, cool down to 70 - 80 °C, introduce 2-hydroxyethyltrimethylammonium chloride, then heat up to 120 - 135 °C, react for 7 - 8.5 h, and carry out vacuum distillation to obtain defoaming auxiliary A; The dosage ratio of the polyether ester A, xylene, tetrabutyl titanate, and 2-hydroxyethyltrimethylammonium chloride is 1600 - 2200 g: 500 - 700 mL: 8.2 - 14 g: 245 - 318 g.

7. The environmentally friendly non-silicon defoamer according to claim 1, characterized in that, The preparation method of the defoaming auxiliary B is as follows: Step C1. Add sodium stearate into absolute ethanol, stir evenly at 35 - 45 °C, then add hollow silica microspheres, heat under reflux, wash with ethanol 3 times, and dry under vacuum to obtain hydrophobic hollow silica microspheres; Step C2. Add dibutyl phthalate into absolute ethanol, stir evenly, then add the hydrophobic hollow silica microspheres, stir at 300 - 400 rpm for 6 - 8 h, centrifuge and dry to obtain defoaming auxiliary B.

8. The environmentally friendly non-silicon defoamer according to claim 7, wherein In step C1, the dosage ratio of sodium stearate, absolute ethanol, and hollow silica microspheres is 2.2 - 3.5 g: 30 - 40 mL: 18 - 24.6 g; The temperature during the heating under reflux is 82 - 95 °C, and the time is 7 - 8 h; The temperature during the vacuum drying is 70 - 80 °C, and the time is 1 - 2 h; In step C2, the dosage ratio of absolute ethanol, dibutyl phthalate, and hydrophobic hollow silica microspheres is 20 - 28 mL: 1.3 - 2 g: 8 - 14.5 g; The temperature during the drying is 45 - 55 °C, and the time is 2.5 - 3 h.

9. The environmentally friendly non-silicon defoamer according to any one of claims 1-8, characterized in that, It includes the following steps: Add a thickener and an organic solvent into deionized water. After mixing evenly, add an emulsifier, stir at room temperature for 10 - 15 min, then sequentially add a dispersant, a defoaming auxiliary, and a polyether ester, and mix evenly to obtain an environment-friendly non-silicon defoaming agent.

10. The environment-friendly non-silicon defoamer according to any one of claims 1-8, characterized in that, The defoaming agent is used in waterborne coatings.

Citation Information

Patent Citations

  • Polyether ester / mineral oil composite defoaming agent and preparation method thereof

    CN104906832A

Cited By

  • Silicon-free defoaming agent for oil and gas fields and preparation method of silicon-free defoaming agent

    CN121338401A

  • Composite defoaming agent for papermaking white water system and preparation method of composite defoaming agent

    CN121606934A

  • Aqueous emulsion type non-silicon defoaming agent and preparation method thereof

    CN121796956A

  • Water emulsion type non-silicon defoaming agent and preparation method thereof

    CN121796956B