A multilayer composite extruded sheet and a method for producing the same

Through multi-layer composite structure design and specific material combination, the shortcomings of traditional extruded polystyrene boards in terms of thermal insulation performance, structural strength and multifunctionality have been solved, achieving improved thermal insulation performance and enhanced structural strength, meeting the high requirements of prefabricated buildings.

CN120287684BActive Publication Date: 2026-11-24HEBEI FENGDE THERMAL INSULATION MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510491159.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-18
Publication Date
2026-11-24
Estimated Expiration
2045-04-18

AI Technical Summary

Technical Problem

Traditional extruded polystyrene (XPS) boards are inadequate in terms of thermal insulation performance, structural strength, and multifunctionality, making it difficult to meet the high requirements of prefabricated and modular buildings.

Method used

The material adopts a multi-layer composite structure design, with functional surface, middle and inner layers composed of specific raw materials. Through a reasonable hierarchical structure and three-layer co-extrusion foaming technology, gradient acoustic impedance and thermal impedance are formed. Combined with graphite-modified polystyrene, nano-silica, zinc oxide-coated montmorillonite and other materials, the material's thermal insulation, fire resistance and sound insulation performance are improved.

Benefits of technology

It achieves improved thermal insulation performance, enhanced structural strength, multi-functionality, meets the high requirements of prefabricated buildings, and has excellent fire resistance and sound insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the field of extruded sheet, and proposes a kind of multilayer composite extruded sheet and preparation method thereof.The multilayer composite extruded sheet includes functional surface layer, intermediate layer and inner layer;The functional surface layer is composed of the following raw materials by weight: polystyrene 45-55 parts, graphite modified polystyrene 25-35 parts, nano-silica 4-6 parts, flame retardant 8-12 parts, antioxidant 1-2 parts and lubricant 2-4 parts;The intermediate layer is composed of the following raw materials by weight: polystyrene 60-70 parts, glass fiber chopped strand 14-16 parts, grafted modified glass fiber 5-7 parts, flame retardant 8-12 parts, coupling agent 2-4 parts, foaming nucleating agent 1.5-2.5 parts.The multilayer composite extruded sheet provided by the present application realizes the balance of thermal insulation and structural strength by designing reasonable hierarchical structure, and meets the demand of multifunction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of extruded polystyrene (XPS) board technology, specifically to a multilayer composite XPS board and its preparation method. Background Technology

[0002] Extruded polystyrene (XPS) board, as a high-performance building insulation material, is widely used in the construction industry due to its lightweight, high compressive strength, water resistance, air impermeability, wear resistance, and thermal insulation properties. Especially in wall insulation and low-temperature storage flooring, XPS board has become a preferred construction material due to its cost-effectiveness. However, with the continuous development of the construction industry, the performance requirements for XPS board are constantly increasing, and traditional XPS board can no longer meet market demands in some aspects.

[0003] Extruded polystyrene (XPS) boards are materials formed through continuous extrusion foaming. The resulting hard film on the surface is uniform and smooth, while the interior is filled with completely closed-cell foam in a continuous and uniform manner, forming a honeycomb structure. This structure endows XPS boards with excellent physical and chemical properties. For example, its high compressive strength allows it to withstand large loads without deformation; its lightweight nature facilitates transportation and construction; and its non-absorbent and airtight properties effectively prevent the penetration of moisture and air, thereby improving the building's insulation and moisture-proof performance.

[0004] Currently, the production technology of extruded polystyrene (XPS) boards is relatively mature, but some problems still exist in practical applications. For example, traditional XPS boards still have room for improvement in terms of thermal insulation performance, structural strength, and multifunctionality. In addition, with the rise of prefabricated and modular buildings, new requirements have been placed on the dimensional accuracy, ease of installation, and environmental performance of XPS boards.

[0005] While traditional extruded polystyrene (XPS) boards offer excellent thermal insulation, they still fall short in terms of structural strength. This is particularly true in buildings requiring heavy loads or operating in challenging environments, where a single layer of XPS board is insufficient. Furthermore, with the development of the construction industry, the functional requirements for XPS boards are increasing. For example, XPS boards need to simultaneously provide thermal insulation, sound insulation, and fire resistance. However, traditional XPS boards have significant limitations in terms of multifunctionality. Therefore, this invention proposes a multi-layer composite XPS board and its preparation method. Summary of the Invention

[0006] This invention proposes a multi-layer composite extruded polystyrene board and its preparation method. By designing a reasonable layered structure, a balance between thermal insulation and structural strength is achieved, meeting the multi-functional requirements of thermal insulation, sound insulation, and fire resistance.

[0007] The technical solution of the present invention is as follows: In a first aspect, the present invention proposes a multilayer composite extruded polystyrene board, comprising a functional surface layer, a middle layer and an inner layer; The functional surface layer is composed of the following raw materials in parts by weight: 45-55 parts polystyrene, 25-35 parts graphite-modified polystyrene, 4-6 parts nano silica, 8-12 parts flame retardant, 1-2 parts antioxidant and 2-4 parts lubricant. The intermediate layer is composed of the following raw materials in parts by weight: 60-70 parts polystyrene, 14-16 parts chopped glass fiber, 5-7 parts grafted modified glass fiber, 8-12 parts flame retardant, 2-4 parts coupling agent, and 1.5-2.5 parts foaming nucleating agent. The inner layer is composed of the following raw materials in parts by weight: 50-60 parts polystyrene, 25-35 parts supercritical CO2 foaming agent, 4-6 parts zinc oxide-coated montmorillonite, 0.4-0.6 parts carbon nanotubes, and 2-3 parts quaternary ammonium salt antistatic agent.

[0008] As a further technical solution, the thickness ratio of the functional surface layer, intermediate layer and inner layer is 14-16:35-45:42-48.

[0009] As a further technical solution, the preparation method of the grafted modified glass fiber includes: ultrasonically dispersing 2-3g of octavinylsilsesquioxane in 200-220mL of ethanol, adding 0.1-0.2g of benzoyl peroxide initiator, and magnetically stirring to dissolve and obtain a grafting solution; immersing silanized glass fiber in the solution, heating to 60-70℃ under nitrogen protection, stirring at 700-900rpm for 5-7h, controlling the ratio of silanized glass fiber to grafting solution to 1:20-24g / mL, after the reaction is completed, ultrasonically washing with ethanol and deionized water 3-5 times in sequence, and vacuum drying at 60-80℃ for 12-14h to obtain grafted modified glass fiber.

[0010] As a further technical solution, the preparation method of the silanized glass fiber includes: heating the glass fiber to 550-600℃ at 3-4℃ / min and holding it at that temperature for 2-3h to obtain pretreated glass fiber; mixing a silane coupling agent, ethanol and water in a volume ratio of 1:18-20:2 and adjusting the pH to 4-5 with acetic acid; then impregnating the pretreated fiber in the mixture, ultrasonically vibrating it at 60-70℃ and 40-50kHz for 30-40min, letting it stand for 22-24h, and vacuum drying it at 60-80℃ for 6-10h to obtain silanized glass fiber.

[0011] As a further technical solution, the preparation method of zinc oxide-coated montmorillonite includes: dissolving zinc acetate dihydrate in ethanol, adding sodium hydroxide to adjust the pH to 9-11, ultrasonically dispersing at 50-60℃ for 5-7 hours to obtain zinc oxide sol, mixing montmorillonite with zinc oxide sol, adding hydrazine hydrate solution, ultrasonically stirring at 70-80℃ for 6-7 hours, then reacting at 165-175℃ for 22-24 hours, and obtaining the final product after filtration, washing, and drying.

[0012] As a further technical solution, the weight ratio of the zinc acetate dihydrate: ethanol: montmorillonite and hydrazine hydrate solution is 10-20: 30-50: 1-3: 1.5-3.5.

[0013] As a further technical solution, the flame retardant in the functional surface layer includes ammonium polyphosphate and pentaerythritol in a weight ratio of 2-3:4-6, the antioxidant is antioxidant 1010, and the lubricant is calcium stearate.

[0014] As a further technical solution, the average length of the short glass fiber filaments in the intermediate layer is 3-5 mm, the flame retardant includes magnesium hydroxide and aluminum hydroxide in a weight ratio of 1:3-4, the silane coupling agent is silane coupling agent KH550, and the foaming nucleating agent is talc; the quaternary ammonium salt antistatic agent in the inner layer is octadecyltrimethylammonium chloride.

[0015] Secondly, this invention proposes a method for preparing a multi-layer composite extruded board, comprising the following steps: mixing functional surface layer, intermediate layer and inner layer raw materials separately, controlling the die temperature at 105-110℃, using three-layer co-extrusion foaming to extrude pre-formed boards, controlling the roller temperature at 80-90℃, pressing the boards through a three-roll calender to achieve a board thickness of 20-100mm, with a calendering speed to extrusion speed ratio of 1:1.2; performing plasma treatment at a power of 4-6kW and a speed of 2.5-3.5m / min, and then curing at a constant temperature of 55-65℃ for 23-25h after slitting to obtain the multi-layer composite extruded board.

[0016] As a further technical solution, the extruder temperatures for the functional surface layer are: Zone 1 185-195℃, Zone 2 195-205℃, and Zone 3 205-215℃; the extruder temperatures for the intermediate layer are: Zone 1 175-185℃, Zone 2 190-200℃, and Zone 3 200-210℃; the extruder temperatures for the inner layer are: Zone 1 170-180℃, Zone 2 180-190℃, and Zone 3 190-200℃; and the injection pressure of the inner layer foaming agent is 12-15MPa.

[0017] The working principle and beneficial effects of this invention are as follows: The multilayer composite extruded polystyrene board in this invention adopts a three-layer structure design. The functional surface layer is mainly responsible for fire resistance, weather resistance, and aging resistance; the middle layer mainly provides mechanical support and thermal insulation performance; and the inner layer forms a uniform cell structure through supercritical foaming technology, further improving thermal insulation performance. This structural design results in a more balanced and superior overall material performance; the functional surface layer (high density), the middle layer (fiber reinforcement), and the inner layer (porous) form an acoustic impedance gradient, attenuating sound wave energy layer by layer.

[0018] In the functional surface layer of this invention, both polystyrene and graphite-modified polystyrene possess excellent thermal insulation properties. The addition of graphite-modified polystyrene further enhances the material's thermal stability and electrical conductivity, contributing to improved overall weather resistance and fire resistance. Nano-silica, as a nanoscale filler, effectively enhances the material's mechanical properties and heat resistance, while also improving its anti-aging properties. The combined use of ammonium polyphosphate and pentaerythritol forms an effective flame-retardant system, reducing the material's combustion rate and temperature, and improving fire resistance. In the intermediate layer, chopped glass fibers and grafted modified glass fibers significantly improve the material's mechanical properties and dimensional stability. Simultaneously, the thermal conductivity of glass fibers contributes to the uniform distribution of heat, enhancing thermal insulation performance.

[0019] In this invention, the surface intumescent flame retardant ammonium polyphosphate and pentaerythritol are combined to generate an intumescent carbon layer (heat insulation and oxygen barrier) at high temperature, and release non-flammable gases to dilute oxygen; the intermediate inorganic flame retardant magnesium hydroxide and aluminum hydroxide are combined to decompose and absorb heat, release water vapor to dilute flammable gases, and effectively improve the flame retardancy of extruded board.

[0020] The inner layer material of this invention uses supercritical CO2 foaming agent to create a uniform microporous closed-cell structure (small pore size and uniform distribution). The thermal conductivity of gas in these closed pores is extremely low, effectively suppressing heat convection and conduction. The zinc oxide-coated montmorillonite nanosheet structure creates a "maze effect" in the matrix, extending the heat transfer path. The intercalation structure of montmorillonite further reduces the thermal conductivity of the material. As a layered silicate, montmorillonite's ability to block heat conduction paths is further enhanced when its surface is uniformly coated with zinc oxide nanoparticles. The layered structure significantly reduces heat conduction efficiency by increasing the tortuosity of the heat flow path. Zinc oxide itself has low thermal conductivity, and when combined with montmorillonite, it forms a multi-level barrier effect. In addition, the grafted modified glass fiber forms a three-dimensional network structure in the middle layer, which reduces the continuity of the polymer matrix and inhibits phonon conduction; the spatial complementarity between the layered barrier of the inner montmorillonite-zinc oxide layer and the fiber network in the middle layer means that heat must bypass the dual barriers of the fiber network and the layered filler, thereby further improving the thermal insulation performance.

[0021] At the microscopic level, zinc oxide forms heterojunctions on the surface of montmorillonite, improving UV absorption efficiency; the organic-inorganic interface of the grafted fibers enhances stress transfer. The intermediate fiber network and the inner montmorillonite sheets together form a hierarchical barrier structure, while the phosphates produced by the decomposition of the surface flame retardant and the intermediate fiber network together construct a continuous fire barrier. The inner foam structure reduces convective heat loss through its closed-cell design. Therefore, grafted modified glass fiber and zinc oxide-coated montmorillonite can achieve synergistic performance enhancement.

[0022] In this invention, flexible organosilicon segments are formed on the surface of the glass fiber grafted with octavinylsilsesquioxane, enhancing the interfacial bonding with the polystyrene matrix and reducing sound wave reflection loss at the interface. Simultaneously, the fiber network dissipates sound energy through friction, and short-cut fibers (3-5 mm) effectively disrupt the propagation of mid-to-high frequency sound waves. Furthermore, the nano-interlayer voids of montmorillonite and the piezoelectric effect of zinc oxide work together: the interlayer voids absorb low-frequency sound waves through viscous damping, and the micro-current generated by zinc oxide under sound wave pressure converts mechanical energy into heat energy. This, together with the intermediate fiber network, forms a broadband sound-absorbing layer.

[0023] In terms of fire resistance and flame retardancy, silanized glass fibers grafted with octavinylsilsesquioxane decompose at high temperatures to generate a Si-OC cross-linked network. This network synergistically interacts with the water vapor generated by the decomposition of magnesium hydroxide / aluminum in the intermediate layer, promoting the formation of a dense char layer. The grafted organosilicon segments improve the thermal stability of the char layer. Meanwhile, zinc oxide transforms into ZnO at high temperatures, forming a physical barrier with the montmorillonite layers to slow the diffusion of combustible gases. The free radicals trapped between the montmorillonite layers and the photocatalytic activity of ZnO synergistically inhibit the combustion chain reaction. Furthermore, in terms of low-temperature weather resistance, the hydroxyl groups on the surface of the glass fibers treated with the silane coupling agent undergo free radical grafting with the vinyl groups of the octavinylsilsesquioxane, forming C-Si-O covalent bonds. The hydrophobicity of the fiber grafted layer reduces frost heave stress caused by moisture penetration. Detailed Implementation

[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. It should be noted that the graphite-modified polystyrene in the present invention is of the type SEPS.

[0025] Example 1 This embodiment provides a multi-layer composite extruded polystyrene board, including a functional surface layer, a middle layer, and an inner layer with a thickness ratio of 3:8:9; The functional surface layer is composed of the following raw materials in parts by weight: 50 parts polystyrene, 30 parts graphite-modified polystyrene, 5 parts nano silica, 10 parts flame retardant, 1.5 parts antioxidant and 3 parts lubricant. The intermediate layer is composed of the following raw materials in parts by weight: 65 parts polystyrene, 15 parts chopped glass fiber, 6 parts grafted modified glass fiber, 10 parts flame retardant, 3 parts coupling agent, and 2 parts foaming nucleating agent. The inner layer is composed of the following raw materials in parts by weight: 55 parts polystyrene, 30 parts supercritical CO2 foaming agent, 5 parts zinc oxide-coated montmorillonite, 0.5 parts carbon nanotubes, and 2.5 parts quaternary ammonium salt antistatic agent; The process involved heating glass fibers to 570℃ at 3.5℃ / min and holding for 2.5h to obtain pretreated glass fibers. A mixture of silane coupling agent KH550, ethanol, and water (volume ratio 1:19:2) was prepared, and the pH was adjusted to 4.5 with acetic acid. The pretreated fibers were then impregnated in the mixture, ultrasonically vibrated at 65℃ and 45kHz for 35min, allowed to stand for 23h, and then vacuum dried at 70℃ for 8h to obtain silanized glass fibers. 2.5g of octavinylsilsesquioxane was ultrasonically dispersed in 210mL of ethanol, and 0.15g of benzoyl peroxide initiator was added and magnetically stirred to dissolve the silanized glass fibers to obtain a grafting solution. The silanized glass fibers were then impregnated in this solution, heated to 65℃ under nitrogen protection, and stirred at 800rpm for 6h. The ratio of silanized glass fibers to grafting solution was controlled at 1:22g / mL. After the reaction, the fibers were ultrasonically cleaned four times with ethanol and deionized water, and then vacuum dried at 70℃ for 13h to obtain grafted modified glass fibers. The preparation method of zinc oxide-coated montmorillonite includes: dissolving zinc acetate dihydrate in ethanol, adding sodium hydroxide to adjust the pH to 10, ultrasonically dispersing at 55°C for 6 hours to obtain zinc oxide sol, mixing montmorillonite with zinc oxide sol, adding hydrazine hydrate solution, ultrasonically stirring at 75°C for 6.5 hours, then reacting at 170°C for 23 hours, and obtaining the product after filtration, washing, and drying; the weight ratio of zinc acetate dihydrate: ethanol: montmorillonite and hydrazine hydrate solution is 15:40:2:2.5. The functional surface layer contains a flame retardant consisting of ammonium polyphosphate and pentaerythritol in a weight ratio of 2.5:5, an antioxidant of antioxidant 1010, and a lubricant of calcium stearate. The intermediate layer contains chopped glass fibers with an average length of 4 mm, flame retardants consisting of magnesium hydroxide and aluminum hydroxide in a weight ratio of 1:3.5, a silane coupling agent of silane coupling agent KH550, and a foaming nucleating agent of talc. The inner layer contains a quaternary ammonium salt antistatic agent of octadecyltrimethylammonium chloride. The preparation method of this multi-layer composite extruded board includes the following steps: mixing functional surface layer, intermediate layer and inner layer raw materials separately, controlling the die temperature at 107℃, using three-layer co-extrusion foaming to extrude the pre-formed board, controlling the roller temperature at 85℃, pressing the board through a three-roll calender to achieve a board thickness of 50mm, with a calendering speed to extrusion speed ratio of 1:1.2; performing plasma treatment at a power of 5kW and a speed of 3m / min, and then curing at a constant temperature of 60℃ for 24 hours after slitting to obtain the multi-layer composite extruded board; wherein, the extruder temperatures for the functional surface layer are: zone 1 190℃, zone 2 200℃, zone 3 210℃; the extruder temperatures for the intermediate layer are: zone 1 180℃, zone 2 195℃, zone 3 205℃; the extruder temperatures for the inner layer are: zone 1 175℃, zone 2 185℃, zone 3 195℃; and the foaming agent injection pressure for the inner layer is 13MPa.

[0026] Example 2 This embodiment provides a multi-layer composite extruded polystyrene board, comprising a functional surface layer, a middle layer, and an inner layer with a thickness ratio of 14:35:42; The functional surface layer is composed of the following raw materials in parts by weight: 45 parts polystyrene, 25 parts graphite-modified polystyrene, 4 parts nano silica, 8 parts flame retardant, 1 part antioxidant and 2 parts lubricant. The intermediate layer is composed of the following raw materials in parts by weight: 60 parts polystyrene, 14 parts chopped glass fiber, 5 parts grafted modified glass fiber, 8 parts flame retardant, 2 parts coupling agent, and 1.5 parts foaming nucleating agent. The inner layer is composed of the following raw materials in parts by weight: 50 parts polystyrene, 25 parts supercritical CO2 foaming agent, 4 parts zinc oxide coated montmorillonite, 0.4 parts carbon nanotubes and 2 parts quaternary ammonium salt antistatic agent; The process involves heating glass fibers to 550℃ at 3℃ / min and holding for 2 hours to obtain pretreated glass fibers. A mixture of silane coupling agent KH550, ethanol, and water (volume ratio 1:18:2) is prepared, and the pH is adjusted to 4 with acetic acid. The pretreated fibers are then impregnated in the mixture, ultrasonically vibrated at 60℃ and 40kHz for 30 minutes, allowed to stand for 22 hours, and then vacuum-dried at 60℃ for 6 hours to obtain silanized glass fibers. 2g of octavinylsilsesquioxane is ultrasonically dispersed in 200mL of ethanol, and 0.1g of benzoyl peroxide initiator is added and magnetically stirred to dissolve the mixture, yielding a grafting solution. The silanized glass fibers are then impregnated in this solution, heated to 60℃ under nitrogen protection, and stirred at 700rpm for 5 hours. The ratio of silanized glass fibers to grafting solution is controlled at 1:20g / mL. After the reaction, the fibers are ultrasonically cleaned three times with ethanol and deionized water, and then vacuum-dried at 60℃ for 12 hours to obtain grafted modified glass fibers. The preparation method of zinc oxide-coated montmorillonite includes: dissolving zinc acetate dihydrate in ethanol, adding sodium hydroxide to adjust the pH to 9, ultrasonically dispersing at 50°C for 5 hours to obtain zinc oxide sol, mixing montmorillonite with zinc oxide sol, adding hydrazine hydrate solution, ultrasonically stirring at 70°C for 6 hours, then reacting at 165°C for 22 hours, and obtaining the final product after filtration, washing, and drying; the weight ratio of zinc acetate dihydrate: ethanol: montmorillonite and hydrazine hydrate solution is 10:30:1:1.5. The functional surface layer contains flame retardants including ammonium polyphosphate and pentaerythritol in a weight ratio of 2:4, antioxidant 1010, and calcium stearate as a lubricant; the intermediate layer contains glass fiber chopped strands with an average length of 3 mm, flame retardants including magnesium hydroxide and aluminum hydroxide in a weight ratio of 1:3, silane coupling agent KH550, and talc as a foaming nucleating agent; and the inner layer contains quaternary ammonium salt antistatic agent octadecyltrimethylammonium chloride. The preparation method of this multi-layer composite extruded board includes the following steps: mixing functional surface layer, intermediate layer and inner layer raw materials separately, controlling the die temperature at 105℃, using three-layer co-extrusion foaming to extrude the pre-formed board, controlling the roller temperature at 80℃, pressing the board through a three-roll calender to achieve a board thickness of 50mm, with a calendering speed to extrusion speed ratio of 1:1.2; performing plasma treatment at a power of 4kW and a speed of 2.5m / min, and then curing at a constant temperature of 55℃ for 23h after slitting to obtain the multi-layer composite extruded board; wherein, the extruder temperatures for the functional surface layer are: zone 1 185℃, zone 2 195℃, zone 3 205℃; the extruder temperatures for the intermediate layer are: zone 1 175℃, zone 2 190℃, zone 3 200℃; the extruder temperatures for the inner layer are: zone 1 170℃, zone 2 180℃, zone 3 190℃; and the foaming agent injection pressure for the inner layer is 12MPa.

[0027] Example 3 This embodiment provides a multi-layer composite extruded board, including a functional surface layer, a middle layer, and an inner layer with a thickness ratio of 16:45:48; The functional surface layer is composed of the following raw materials in parts by weight: 55 parts polystyrene, 35 parts graphite-modified polystyrene, 6 parts nano silica, 12 parts flame retardant, 2 parts antioxidant and 4 parts lubricant. The intermediate layer is composed of the following raw materials in parts by weight: 70 parts polystyrene, 16 parts chopped glass fiber, 7 parts grafted modified glass fiber, 12 parts flame retardant, 4 parts coupling agent, and 2.5 parts foaming nucleating agent. The inner layer is composed of the following raw materials in parts by weight: 60 parts polystyrene, 35 parts supercritical CO2 foaming agent, 6 parts zinc oxide coated montmorillonite, 0.6 parts carbon nanotubes, and 3 parts quaternary ammonium salt antistatic agent. The process involves heating glass fibers to 600℃ at 4℃ / min and holding for 3 hours to obtain pretreated glass fibers. A mixture of silane coupling agent KH550, ethanol, and water (volume ratio 1:20:2) is prepared, and the pH is adjusted to 5 with acetic acid. The pretreated fibers are then impregnated in the mixture, ultrasonically vibrated at 70℃ and 50kHz for 40 minutes, allowed to stand for 24 hours, and vacuum dried at 80℃ for 10 hours to obtain silanized glass fibers. 3g of octavinylsilsesquioxane is ultrasonically dispersed in 220mL of ethanol, and 0.2g of benzoyl peroxide initiator is added and magnetically stirred to dissolve the mixture, yielding a grafting solution. The silanized glass fibers are then impregnated in this solution, heated to 70℃ under nitrogen protection, and stirred at 900rpm for 7 hours. The ratio of silanized glass fibers to grafting solution is controlled at 1:20g / mL. After the reaction, the fibers are ultrasonically cleaned five times with ethanol and deionized water, and vacuum dried at 80℃ for 14 hours to obtain grafted modified glass fibers. The preparation method of zinc oxide-coated montmorillonite includes: dissolving zinc acetate dihydrate in ethanol, adding sodium hydroxide to adjust the pH to 11, ultrasonically dispersing at 60°C for 7 hours to obtain zinc oxide sol, mixing montmorillonite with zinc oxide sol, adding hydrazine hydrate solution, ultrasonically stirring at 80°C for 7 hours, then reacting at 175°C for 24 hours, and obtaining the final product after filtration, washing, and drying; the weight ratio of zinc acetate dihydrate: ethanol: montmorillonite and hydrazine hydrate solution is 20:50:3:3.5. The functional surface layer contains flame retardants including ammonium polyphosphate and pentaerythritol in a weight ratio of 3:6, antioxidant 1010, and calcium stearate as a lubricant; the intermediate layer contains glass fiber chopped strands with an average length of 5 mm, flame retardants including magnesium hydroxide and aluminum hydroxide in a weight ratio of 1:4, silane coupling agent KH550, and talc as a foaming nucleating agent; and the inner layer contains quaternary ammonium salt antistatic agent octadecyltrimethylammonium chloride. The preparation method of this multi-layer composite extruded board includes the following steps: mixing functional surface layer, intermediate layer and inner layer raw materials separately, controlling the die temperature at 110℃, using three-layer co-extrusion foaming to extrude the pre-formed board, controlling the roller temperature at 90℃, pressing the board through a three-roll calender to achieve a board thickness of 50mm, with a calendering speed to extrusion speed ratio of 1:1.2; performing plasma treatment at a power of 6kW and a speed of 3.5m / min, and then curing at a constant temperature of 65℃ for 25h after slitting to obtain the multi-layer composite extruded board; wherein, the extruder temperatures for the functional surface layer are: zone 1 195℃, zone 2 205℃, zone 3 215℃; the extruder temperatures for the intermediate layer are: zone 1 185℃, zone 2 200℃, zone 3 210℃; the extruder temperatures for the inner layer are: zone 1 180℃, zone 2 190℃, zone 3 200℃; and the foaming agent injection pressure for the inner layer is 15MPa.

[0028] Example 4 This embodiment provides a multilayer composite extruded polystyrene board, including a functional surface layer, a middle layer, and an inner layer with a thickness ratio of 14:45:42; The functional surface layer is composed of the following raw materials in parts by weight: 45 parts polystyrene, 35 parts graphite-modified polystyrene, 4 parts nano silica, 12 parts flame retardant, 1 part antioxidant and 4 parts lubricant. The intermediate layer is composed of the following raw materials in parts by weight: 60 parts polystyrene, 16 parts chopped glass fiber, 5 parts grafted modified glass fiber, 12 parts flame retardant, 2 parts coupling agent, and 2.5 parts foaming nucleating agent. The inner layer is composed of the following raw materials in parts by weight: 50 parts polystyrene, 35 parts supercritical CO2 foaming agent, 4 parts zinc oxide coated montmorillonite, 0.6 parts carbon nanotubes and 2 parts quaternary ammonium salt antistatic agent; The process involves heating glass fibers to 550℃ at 4℃ / min and holding for 3 hours to obtain pretreated glass fibers. A mixture of silane coupling agent KH550, ethanol, and water (volume ratio 1:18:2) is prepared, and the pH is adjusted to 5 with acetic acid. The pretreated fibers are then impregnated in the mixture, ultrasonically vibrated at 60℃ and 50kHz for 30 minutes, allowed to stand for 24 hours, and then vacuum-dried at 60℃ for 10 hours to obtain silanized glass fibers. 2g of octavinylsilsesquioxane is ultrasonically dispersed in 220mL of ethanol, and 0.1g of benzoyl peroxide initiator is added and magnetically stirred to dissolve the mixture, yielding a grafting solution. The silanized glass fibers are then impregnated in this solution, heated to 70℃ under nitrogen protection, and stirred at 700rpm for 7 hours. The ratio of silanized glass fibers to grafting solution is controlled at 1:20g / mL. After the reaction, the fibers are ultrasonically cleaned five times with ethanol and deionized water, and then vacuum-dried at 60℃ for 14 hours to obtain grafted modified glass fibers. The preparation method of zinc oxide-coated montmorillonite includes: dissolving zinc acetate dihydrate in ethanol, adding sodium hydroxide to adjust the pH to 9, ultrasonically dispersing at 60°C for 5 hours to obtain zinc oxide sol, mixing montmorillonite with zinc oxide sol, adding hydrazine hydrate solution, ultrasonically stirring at 80°C for 6 hours, then reacting at 175°C for 22 hours, and obtaining the final product after filtration, washing, and drying; the weight ratio of zinc acetate dihydrate: ethanol: montmorillonite and hydrazine hydrate solution is 20:30:1:3.5. The functional surface layer contains a flame retardant consisting of ammonium polyphosphate and pentaerythritol in a weight ratio of 2:6, an antioxidant of antioxidant 1010, and a lubricant of calcium stearate. The intermediate layer contains chopped glass fibers with an average length of 3 mm, flame retardants consisting of magnesium hydroxide and aluminum hydroxide in a weight ratio of 1:3, a silane coupling agent of silane coupling agent KH550, and a foaming nucleating agent of talc. The inner layer contains a quaternary ammonium salt antistatic agent of octadecyltrimethylammonium chloride. The preparation method of this multi-layer composite extruded board includes the following steps: mixing functional surface layer, intermediate layer and inner layer raw materials separately, controlling the die temperature at 110℃, using three-layer co-extrusion foaming to extrude the pre-formed board, controlling the roller temperature at 80℃, pressing the board through a three-roll calender to achieve a board thickness of 50mm, with a calendering speed to extrusion speed ratio of 1:1.2; performing plasma treatment at a power of 6kW and a speed of 2.5m / min, and then curing at a constant temperature of 65℃ for 23h after slitting to obtain the multi-layer composite extruded board; wherein, the extruder temperatures for the functional surface layer are: zone 1 195℃, zone 2 195℃, zone 3 215℃; the extruder temperatures for the intermediate layer are: zone 1 175℃, zone 2 200℃, zone 3 210℃; the extruder temperatures for the inner layer are: zone 1 180℃, zone 2 190℃, zone 3 200℃; and the foaming agent injection pressure for the inner layer is 12MPa.

[0029] Comparative Example 1 The method is based on Example 1, with the difference being that the grafted modified glass fiber is replaced with silanized glass fiber.

[0030] Comparative Example 2 The method is based on Example 1, with the difference being that the grafted modified glass fiber is replaced with chopped glass fiber.

[0031] Comparative Example 3 The method is based on Example 1, but with adjustments. The difference from Example 1 is that grafted modified glass fiber is not added to the intermediate layer material.

[0032] Comparative Example 4 The method is based on Example 1, with the difference being that zinc oxide-coated montmorillonite is replaced with zinc oxide.

[0033] Comparative Example 5 The method is based on Example 1, with the difference being that zinc oxide-coated montmorillonite is replaced with montmorillonite.

[0034] Comparative Example 6 The method is based on Example 1, but with adjustments. The difference from Example 1 is that grafted modified glass fiber is not added to the inner layer material.

[0035] Test Example 1: The multilayer composite extruded polystyrene boards prepared in Examples 1-4 and Comparative Examples 1-6 were subjected to the following tests: 1. Thermal insulation: The thermal conductivity of the extruded board was tested according to the protective hot plate method in GB / T 10294-2008, with an average temperature of 25℃. 2. Sound insulation: The sound insulation of the extruded polystyrene board was tested in the 125-4000Hz frequency band according to GB / T 19889.3-2005 airborne sound insulation laboratory measurement. 3. Flame retardancy: Tested according to GB / T 2406.2-2009; 4. Weather resistance: -20℃ for 12 hours, room temperature for 12 hours, cycle 30 times to evaluate the cracking of the extruded board. The cracking is divided into 5 levels, with level 1 being almost no cracking and level 5 being very serious cracking.

[0036] The results are shown in Table 1 below: Table 1

[0037] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A multi-layer composite extruded polystyrene board, characterized in that, The product comprises a functional surface layer, an intermediate layer, and an inner layer. The functional surface layer is composed of the following raw materials in parts by weight: 45-55 parts polystyrene, 25-35 parts graphite-modified polystyrene, 4-6 parts nano-silica, 8-12 parts flame retardant, 1-2 parts antioxidant, and 2-4 parts lubricant. The intermediate layer is composed of the following raw materials in parts by weight: 60-70 parts polystyrene, 14-16 parts chopped glass fiber, 5-7 parts grafted modified glass fiber, 8-12 parts flame retardant, 2-4 parts coupling agent, and 1.5-2.5 parts foaming nucleating agent. The inner layer is composed of the following raw materials in parts by weight: 50-60 parts polystyrene, 25-35 parts supercritical CO2 foaming agent, 4-6 parts zinc oxide-coated montmorillonite, 0.4-0.6 parts carbon nanotubes, and 2-3 parts quaternary ammonium salt antistatic agent. The preparation method of the grafted modified glass fiber includes: ultrasonically dispersing 2-3g of octavinylsilsesquioxane in 200-220mL of ethanol, adding 0.1-0.2g of benzoyl peroxide initiator, and magnetically stirring to dissolve and obtain a grafting solution; immersing silanized glass fiber in the solution, heating to 60-70℃ under nitrogen protection, stirring at 700-900rpm for 5-7h, controlling the ratio of silanized glass fiber to grafting solution to 1:20-24g / mL, after the reaction is completed, ultrasonically washing with ethanol and deionized water 3-5 times in sequence, and vacuum drying at 60-80℃ for 12-14h to obtain grafted modified glass fiber; The method for preparing the silanized glass fiber includes: heating the glass fiber to 550-600℃ at 3-4℃ / min and holding it at that temperature for 2-3h to obtain pretreated glass fiber; mixing a silane coupling agent, ethanol, and water in a volume ratio of 1:18-20:2 and adjusting the pH to 4-5 with acetic acid; then impregnating the pretreated fiber in the mixture, ultrasonically vibrating it at 60-70℃ and 40-50kHz for 30-40min, allowing it to stand for 22-24h, and vacuum drying it at 60-80℃ for 6-10h to obtain silanized glass fiber. The preparation method of zinc oxide-coated montmorillonite includes: dissolving zinc acetate dihydrate in ethanol, adding sodium hydroxide to adjust the pH to 9-11, ultrasonically dispersing at 50-60℃ for 5-7 hours to obtain zinc oxide sol, mixing montmorillonite with zinc oxide sol, adding hydrazine hydrate solution, ultrasonically stirring at 70-80℃ for 6-7 hours, and then reacting at 165-175℃ for 22-24 hours, followed by filtration, washing, and drying to obtain the final product.

2. The multi-layer composite extruded polystyrene board according to claim 1, characterized in that, The thickness ratio of the functional surface layer, intermediate layer and inner layer is 14-16:35-45:42-48.

3. The multi-layer composite extruded polystyrene board according to claim 1, characterized in that, The weight ratio of the zinc acetate dihydrate: ethanol: montmorillonite and hydrazine hydrate solution is 10-20: 30-50: 1-3: 1.5-3.

5.

4. The multi-layer composite extruded polystyrene board according to claim 1, characterized in that, The flame retardant in the functional surface layer includes ammonium polyphosphate and pentaerythritol in a weight ratio of 2-3:4-6, the antioxidant is antioxidant 1010, and the lubricant is calcium stearate.

5. A multi-layer composite extruded polystyrene board according to claim 1, characterized in that, The average length of the short glass fiber filaments in the intermediate layer is 3-5 mm. The flame retardant includes magnesium hydroxide and aluminum hydroxide in a weight ratio of 1:3-4. The silane coupling agent is silane coupling agent KH550, and the foaming nucleating agent is talc. The quaternary ammonium salt antistatic agent in the inner layer is octadecyltrimethylammonium chloride.

6. A method for preparing a multilayer composite extruded polystyrene board as described in any one of claims 1-5, characterized in that, step include: The functional surface, intermediate, and inner layer materials are mixed separately, and the die temperature is controlled at 105-110℃. The pre-formed board is produced by three-layer co-extrusion foaming, with the roller temperature controlled at 80-90℃. The board is pressed by a three-roll calender to achieve a thickness of 20-100mm, with a calendering speed to extrusion speed ratio of 1:1.

2. Plasma treatment is then performed at a power of 4-6kW and a speed of 2.5-3.5m / min. After slitting, the board is cured at a constant temperature of 55-65℃ for 23-25 ​​hours to obtain the multi-layer composite extruded board.

7. The method for preparing a multilayer composite extruded polystyrene board according to claim 6, characterized in that, The extruder temperatures for the functional surface layer are: Zone 1 185-195℃, Zone 2 195-205℃, and Zone 3 205-215℃; the extruder temperatures for the intermediate layer are: Zone 1 175-185℃, Zone 2 190-200℃, and Zone 3 200-210℃; the extruder temperatures for the inner layer are: Zone 1 170-180℃, Zone 2 180-190℃, and Zone 3 190-200℃; and the injection pressure of the inner layer foaming agent is 12-15MPa.

Citation Information

Patent Citations

  • Low-temperature-resistant hydrolysis-resistant glass fiber reinforced PBT and preparation method thereof

    CN112321995A

  • Surfactant-free synthesis and foaming of liquid blowing agent-containing activated carbon-nano / microparticulate polymer composites

    US20110240904A1