Method for the production of a short fiber and bacterial cellulose-calcium alginate aerogel fiber composite yarn

By preparing a spinning solution by mixing bacterial cellulose with sodium alginate and solidifying it with calcium ions, combined with friction spinning technology, the problems of poor mechanical properties and low torsional stiffness of aerogel fibers were solved, and the preparation of aerogel fiber composite yarn with excellent mechanical properties and torsional resistance was realized.

CN120291253BActive Publication Date: 2026-11-24QINGDAO UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510437818.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-09
Publication Date
2026-11-24
Estimated Expiration
2045-04-09

AI Technical Summary

Technical Problem

Existing aerogel fibers have poor mechanical properties and low torsional stiffness, making them difficult to process into textiles and difficult to spin into yarn.

Method used

A spinning solution was prepared by mixing bacterial cellulose and sodium alginate. The solution was then solidified with calcium ions and combined with friction spinning to produce a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers.

Benefits of technology

The mechanical properties and torsion resistance of aerogel fibers were improved, enabling them to withstand torsion during spinning. This led to the preparation of aerogel fiber composite yarns, which also possess spinnability and flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120291253B_ABST
    Figure CN120291253B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers, comprising the following steps: (1) preparing a spinning solution using bacterial cellulose and sodium alginate; (2) using an injection pump to extrude the spinning solution into a coagulation bath to obtain hydrogel fibers, transferring the hydrogel fibers to a displacement solution to displace the water in the hydrogel fibers, and then freezing and drying them to obtain bacterial cellulose-calcium alginate aerogel fibers; (3) using a friction spinning process to blend the short fibers and bacterial cellulose-calcium alginate aerogel fibers to obtain a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers. The aerogel fibers prepared by this invention using bacterial fibers and sodium alginate have high mechanical properties and torsion resistance. Furthermore, the composite yarn of short fibers coated with bacterial cellulose-calcium alginate aerogel fibers is prepared using a friction spinning process, making the aerogel fibers spinnable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of textile technology, specifically to a method for preparing a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers. Background Technology

[0002] Aerogel fibers have a three-dimensional network porous structure, low density, high porosity and low thermal conductivity. They can be used in fire suits, spacesuits and everyday thermal clothing. They have broad application prospects in thermal insulation and aerospace fields and are known as a new generation of thermal insulation materials.

[0003] Currently, aerogel fibers mainly include silica aerogel fibers, polyimide aerogel fibers, and cellulose aerogel fibers. Among them, silica aerogel fibers have poor mechanical properties, exhibit dust shedding, and poor spinnability; polyimide aerogels possess good mechanical properties, but their preparation process is complex, time-consuming, involves various organic solvents, is environmentally unfriendly, and has low torsional stiffness, making them difficult to process in textiles; cellulose aerogel fibers are typically prepared by dissolving cellulose in organic solvents such as DMSO, NMP, or DMAC to prepare a spinning solution, which is then extruded into a coagulation bath to produce aerogel fibers, but the resulting aerogel fibers have poor mechanical properties. Therefore, the preparation of aerogel fibers that combine high strength and torsional performance remains a technological bottleneck, and given the difficulty in torturing aerogel fibers, weaving them into yarns is even more challenging. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a method for preparing composite yarns of short fibers and bacterial cellulose-calcium alginate aerogel fibers.

[0005] The technical solution adopted in this invention is as follows:

[0006] A method for preparing a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers includes the following steps:

[0007] (1) Prepare a bacterial cellulose suspension and add sodium alginate powder. Stir thoroughly to dissolve the sodium alginate and mix the bacterial cellulose and sodium alginate evenly to prepare a spinning solution.

[0008] (2) The spinning solution was extruded into the coagulation bath by an injection pump to obtain the shaped hydrogel fiber. The hydrogel fiber was transferred to the replacement solution to replace the water in the hydrogel fiber. Then it was frozen and dried to obtain bacterial cellulose-calcium alginate aerogel fiber.

[0009] (3) The short fiber and bacterial cellulose-calcium alginate aerogel fiber are blended by friction spinning process to obtain a composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber.

[0010] Further, in step (1), the mass concentration of the bacterial cellulose suspension is 0.5-5.0%, and the mass ratio of the solid content of bacterial cellulose to sodium alginate is 0.2-5:1.

[0011] Furthermore, the solution used in the coagulation bath in step (2) is a calcium chloride solution, and the replacement solution is an aqueous solution of ethanol, tert-butanol or propanol.

[0012] Furthermore, the mass concentration of the calcium chloride solution is 1-10%, and the volume concentration of the aqueous solutions of ethanol, tert-butanol, or propanol is 5-50%.

[0013] Furthermore, in step (2), the injection rate of the syringe pump is 50-300 mL / h.

[0014] Furthermore, in step (2), the freezing method is liquid nitrogen freezing or refrigerator freezing, and the freezing temperature is -196℃ to -20℃.

[0015] Furthermore, the composite yarn obtained by friction spinning in step (3) is a core-spun yarn with short fibers coated with bacterial cellulose-calcium alginate aerogel fibers.

[0016] Furthermore, the short fibers used in the friction spinning in step (3) are at least one of cotton fiber, viscose fiber, polyester fiber, nylon fiber, and aramid fiber.

[0017] The beneficial effects of this invention are as follows:

[0018] (1) This invention provides a method for preparing composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber. The method uses bacterial cellulose and sodium alginate to prepare spinning solution and uses calcium ions to solidify and form the yarn. Bacterial cellulose can provide a continuous and non-agglomerated cellulose spatial network at a certain concentration. The bacterial cellulose spatial network ensures the stable spatial structure and excellent torsion resistance of the aerogel fiber. The sodium alginate solution is uniformly dispersed on the surface of bacterial cellulose nanofibers and then solidified by calcium chloride to further ensure the structural stability of the aerogel fiber, improve the mechanical properties and torsion resistance of the aerogel fiber, and enable it to withstand a certain torsion during spinning, thereby realizing the preparation of aerogel fiber composite yarn.

[0019] (2) This invention provides a method for preparing a composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber. The short fiber and bacterial cellulose-calcium alginate aerogel fiber are blended by friction spinning process. The unique spinning characteristics of friction spinning cause the aerogel fiber to be subjected to only limited torsion during the spinning process. Using this spinning process, a composite yarn of short fiber coated with bacterial cellulose-calcium alginate aerogel fiber can be prepared, which greatly improves the mechanical properties of aerogel fiber and makes the aerogel fiber spinnable, so that it can be used to prepare textile products.

[0020] (3) This invention provides a method for preparing composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber, using bacterial cellulose and sodium alginate as raw materials, which have the characteristics of wide availability, biodegradability, renewability and environmental friendliness; in addition, sodium alginate also has flame retardancy, which also makes the prepared aerogel fiber have a certain flame retardancy. Attached Figure Description

[0021] To clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 This is a schematic diagram illustrating the cross-linking effect of bacterial cellulose, sodium alginate, and calcium ions in this invention.

[0023] Figure 2 Here is a scanning electron microscope image of the aerogel fibers prepared in Example 1 of this invention;

[0024] Figure 3 This is a scanning electron microscope image of the composite yarn prepared in Example 1 of the present invention. Detailed Implementation

[0025] This invention provides a method for preparing composite yarns of short fibers and bacterial cellulose-calcium alginate aerogel fibers. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0026] This invention provides a method for preparing a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers, comprising the following steps:

[0027] (1) Prepare a bacterial cellulose suspension and add sodium alginate powder. Stir thoroughly to dissolve the sodium alginate and mix the bacterial cellulose and sodium alginate evenly to prepare a spinning solution.

[0028] Specifically, in this step, the mass concentration of the bacterial cellulose suspension is 0.5-5.0%, the solid content mass ratio of bacterial cellulose to sodium alginate is 0.2-5:1, and bacterial cellulose is preferably used.

[0029] (2) The spinning solution was extruded into the coagulation bath by an injection pump to obtain the shaped hydrogel fiber. The hydrogel fiber was transferred to the replacement solution to replace the water in the hydrogel fiber. Then it was frozen and dried to obtain bacterial cellulose-calcium alginate aerogel fiber.

[0030] Specifically, in this step, the coagulation bath uses a calcium chloride solution with a mass concentration of 1-10%; the replacement solution is an aqueous solution of ethanol, tert-butanol, or propanol, with a volume concentration of 5-50%; the injection rate of the syringe pump is 50-300 mL / h; and the freezing method is liquid nitrogen freezing or refrigerator freezing, with a freezing temperature of -196℃ to -20℃.

[0031] (3) The short fiber and bacterial cellulose-calcium alginate aerogel fiber are blended by friction spinning process to obtain a composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber.

[0032] Specifically, in this step, the short fibers used in friction spinning are at least one of cotton fiber, viscose fiber, polyester fiber, nylon fiber, and aramid fiber, with a length of 35 to 150 mm; and the composite yarn prepared by friction spinning is a core-spun yarn in which short fibers are coated with bacterial cellulose-calcium alginate aerogel fibers.

[0033] Through the above technical solution, this invention solves the problem that aerogel fibers cannot be textile processed due to their poor mechanical properties and low torsional stiffness. Specifically, this invention mainly solves this problem through the following aspects:

[0034] In the first aspect, the present invention utilizes the structural characteristics of bacterial cellulose, which has a nano-space network structure. By controlling its concentration, it is uniformly dispersed in an aqueous solution to form a continuous and non-agglomerated cellulose spatial network. The bacterial cellulose spatial network ensures the stable spatial structure and excellent torsion resistance of the aerogel fiber.

[0035] Secondly, this invention involves uniformly mixing bacterial cellulose and sodium alginate, spinning the mixture, and then solidifying it with a calcium chloride solution to obtain hydrogel fibers. These are then freeze-dried to obtain aerogel fibers. During the aerogel fiber formation process, the bacterial cellulose in the spinning solution acts as the "skeleton" of the aerogel fibers, while the sodium alginate solution is uniformly dispersed on the surface of the bacterial cellulose nanofibers. After solidification with calcium chloride to form calcium alginate, it becomes the "cement" of the aerogel fibers, creating a structure similar to "reinforced concrete." This ensures the structural stability of the aerogel fibers and improves their mechanical properties through the "reinforced concrete" connection. Furthermore, referring to… Figure 1 When bacterial cellulose and sodium alginate spinning solution are injected into calcium chloride solution, hydrogen bonds will form between the hydroxyl groups on bacterial cellulose and the hydroxyl and carboxyl groups on sodium alginate. At the same time, hydrogen bonds will also form between and within cellulose molecules. Hydrogen bonds will solidify and form hydrogel fibers through hydrogen bonding and calcium ion cross-linking.

[0036] Thirdly, in order to ensure the structural stability of bacterial cellulose and calcium alginate hydrogel fibers during freeze-drying, after the bacterial cellulose and calcium alginate hydrogel fibers are prepared, a low surface energy displacement solution, such as tert-butanol, is first used to displace the water in the bacterial cellulose and calcium alginate hydrogel fibers. After the displacement is completed, freeze-drying is then carried out.

[0037] Furthermore, in this invention, the above three aspects are combined and work together. If ordinary cellulose is used instead of bacterial cellulose, or if the concentration of bacterial cellulose is too low or too high, it is difficult to form an interconnected and continuous bacterial cellulose network. Even if sodium alginate is added to prepare cellulose-calcium alginate aerogel fibers, the torsional resistance cannot be guaranteed because the cellulose is not continuous in its spatial structure. If only bacterial cellulose is used without adding sodium alginate, calcium alginate cannot be coated on the bacterial cellulose, i.e., a "reinforced concrete" structure cannot be formed, resulting in poor structural stability and mechanical properties of the aerogel fibers, or even failure to form the aerogel fibers. If the hydrogel fibers are directly freeze-dried, the high surface energy of water will destroy the bond between bacterial cellulose and calcium alginate during the freeze-drying sublimation, thereby damaging the aerogel fiber structure and potentially reducing porosity and torsional resistance. This invention achieves structural stability, high mechanical properties, and torsional resistance of aerogel fibers through the combination of the above three aspects.

[0038] Building upon the solutions to the problems of poor mechanical properties and low torsional stiffness of aerogel fibers through the three aspects mentioned above, this invention also utilizes the aerogel fibers for spinning. Conventional spinning methods require twisting the fibers multiple times, involving them to intertwine and entangle with other fibers, resulting in high resistance to bending, compression, and torsion. Even though the aerogel fibers prepared by the method of this invention have relatively good torsion resistance, they still cannot completely avoid the inherent incompressibility and torsion of aerogel fibers. Therefore, this invention employs friction spinning to blend the aforementioned aerogel fibers with other short fibers, using the aerogel fibers as the core yarn and other short fibers covering the aerogel fibers. Due to the unique spinning characteristics of friction spinning, the aerogel fibers only experience limited torsion during the spinning process, and the torsion resistance of the aerogel fibers prepared by this invention can withstand this torsion. The aerogel fibers prepared by this invention, combined with the friction spinning process, can be used to prepare aerogel fiber composite yarns.

[0039] It should be noted that the mechanical properties of the aforementioned aerogel fibers mainly refer to tensile strength.

[0040] Furthermore, this invention does not impose any special restrictions on the source of any raw materials; they can be commercially available.

[0041] Example 1

[0042] This embodiment provides a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers, the preparation process of which is as follows:

[0043] (1) Prepare a 1 wt% bacterial cellulose suspension, then add sodium alginate powder. The solid content mass ratio of sodium alginate to bacterial cellulose is 1:1. Stir thoroughly to dissolve sodium alginate and mix bacterial cellulose and sodium alginate evenly to prepare spinning solution.

[0044] (2) The spinning solution was extruded into a 3wt% calcium chloride solution using an injection pump at an injection speed of 80mL / h to obtain the formed hydrogel fiber. The hydrogel fiber was transferred to a 25% tert-butanol aqueous solution for 12h and then frozen using liquid nitrogen at a freezing temperature of -196℃. Subsequently, it was placed in a freeze dryer for drying to obtain bacterial cellulose-calcium alginate aerogel fiber.

[0045] (3) The viscose short fiber and bacterial cellulose-calcium alginate aerogel fiber are blended by friction spinning process, so that the viscose short fiber covers the bacterial cellulose-calcium alginate aerogel fiber, and a composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber is obtained.

[0046] The bacterial cellulose-calcium alginate aerogel fibers prepared in step (2) of Example 1 above were examined using scanning electron microscopy, such as... Figure 2 As shown, (a) is a scanning electron microscope (SEM) image of the overall cross-section of the aerogel fiber, and (b) is a SEM image of the aerogel on the aerogel fiber. From Figure 2 As can be seen, aerogel fibers have a three-dimensional network porous structure.

[0047] The composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers prepared in step (3) of Example 1 was observed, and the results were as follows: Figure 3 As shown, (a) is a photograph of the composite yarn along its length, and (b) is a photograph of the cross-section of the composite yarn. From Figure 3 As can be seen, the composite yarn has a core-sleeved structure in which short fibers are coated with bacterial cellulose-calcium alginate aerogel fibers.

[0048] Testing revealed that the aerogel fiber prepared in this embodiment has a porosity of 92%, a diameter of 903 μm, a tensile strength of 2.6 N, and a single torsion limit of 21 r; the composite yarn has a porosity of 80%, a diameter of approximately 1.6 mm, a tensile strength of 3.6 N, a single torsion limit of 43 r, and a thermal insulation coefficient of 0.04 W / (m·K).

[0049] Example 2

[0050] This embodiment provides a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers, the preparation process of which is as follows:

[0051] (1) Prepare a 0.5 wt% bacterial cellulose suspension, then add sodium alginate powder. The solid content mass ratio of sodium alginate to bacterial cellulose is 1:5. Stir thoroughly to dissolve sodium alginate and mix bacterial cellulose and sodium alginate evenly to prepare spinning solution.

[0052] (2) The spinning solution was extruded into a 3wt% calcium chloride solution using an injection pump at an injection speed of 200mL / h to obtain the formed hydrogel fiber. The hydrogel fiber was transferred to a 10% ethanol aqueous solution for 12h for replacement, and then frozen using liquid nitrogen at a freezing temperature of -196℃. Subsequently, it was placed in a freeze dryer for drying to obtain bacterial cellulose-calcium alginate aerogel fiber.

[0053] (3) The viscose short fiber and bacterial cellulose-calcium alginate aerogel fiber are blended by friction spinning process, so that the viscose short fiber covers the bacterial cellulose-calcium alginate aerogel fiber, and a composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber is obtained.

[0054] Testing revealed that the aerogel fiber prepared in this embodiment has a porosity of 90%, a composite yarn diameter of approximately 1.6 mm, a tensile strength of 5.8 N, and a thermal insulation coefficient of 0.04 W / (m·K).

[0055] Example 3

[0056] This embodiment provides a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers, the preparation process of which is as follows:

[0057] (1) Prepare a 5wt% bacterial cellulose suspension, then add sodium alginate powder. The solid content mass ratio of sodium alginate to bacterial cellulose is 5:1. Stir thoroughly to dissolve sodium alginate and mix the bacterial cellulose and sodium alginate evenly to prepare the spinning solution.

[0058] (2) The spinning solution was extruded into an 8wt% calcium chloride solution using an injection pump at an injection speed of 80mL / h to obtain the formed hydrogel fiber. The hydrogel fiber was transferred to a 40% tert-butanol aqueous solution for 12h and then frozen using liquid nitrogen at a freezing temperature of -196℃. Subsequently, it was placed in a freeze dryer for drying to obtain bacterial cellulose-calcium alginate aerogel fiber.

[0059] (3) The viscose short fiber and bacterial cellulose-calcium alginate aerogel fiber are blended by friction spinning process, so that the viscose short fiber covers the bacterial cellulose-calcium alginate aerogel fiber, and a composite yarn of short fiber and bacterial cellulose-calcium alginate aerogel fiber is obtained.

[0060] Testing revealed that the aerogel fiber prepared in this embodiment has a porosity of 85%, a composite yarn diameter of approximately 1.5 mm, a tensile strength of 12.3 N, and a thermal insulation coefficient of 0.05 W / (m·K).

[0061] Comparative Example 1

[0062] The difference between this comparative example and Example 1 is that the cellulose in this comparative example is nanocellulose (fibrous nanocellulose) prepared by TEMPO oxidation, and bacterial cellulose is not used.

[0063] In this comparative example, the aerogel fibers broke during the friction spinning process, making it impossible to spin smoothly.

[0064] Testing revealed that the aerogel fiber prepared in this comparative example had a porosity of 91%, a tensile strength of 0.9 N, and a single torsion limit of 8 r.

[0065] Comparative Example 2

[0066] The difference between this comparative example and Example 1 is that the concentration of bacterial cellulose in this comparative example is 0.03 wt%.

[0067] In this comparative example, the aerogel fibers broke during the friction spinning process, making it impossible to spin smoothly.

[0068] Testing revealed that the aerogel fiber prepared in this comparative example had a porosity of 96%, a tensile strength of 0.4 N, and a single torsion limit of 3 r.

[0069] Comparative Example 3

[0070] The difference between this comparative example and Example 1 is that this comparative example only uses bacterial cellulose and does not add sodium alginate.

[0071] The aerogel fibers in this comparative example could not be molded.

[0072] Comparative Example 4

[0073] The difference between this comparative example and Example 1 is that, after obtaining the shaped hydrogel fibers in the coagulation bath, this comparative example is directly freeze-dried.

[0074] Testing revealed that the porous structure of the fibers prepared in this comparative example collapsed during the freeze-drying process. The aerogel fibers prepared in this comparative example had a porosity of only 66% and a thermal insulation coefficient of 0.2 W / (m·K), indicating poor thermal insulation performance.

[0075] Comparative Example 5

[0076] The difference between this comparative example and Example 1 is that this comparative example uses a conventional ring spinning process to blend aerogel fibers and short fibers.

[0077] In this comparative example, when ring spinning was used, the hollow structure of the aerogel fiber was destroyed by twisting, the porosity was less than 10%, and a large number of fibers broke during the twisting process.

[0078] It should be noted that any parts not mentioned in this invention can be achieved by using or referencing existing technologies.

[0079] Of course, the above description is not intended to limit the present invention, and the present invention is not limited to the examples given above. Any changes, modifications, additions or substitutions made by those skilled in the art within the scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for the production of a short fiber and bacterial cellulose-calcium alginate aerogel fiber composite yarn, characterized by, Including the following steps: (1) Prepare a bacterial cellulose suspension and add sodium alginate powder. Stir thoroughly to dissolve the sodium alginate and mix the bacterial cellulose and sodium alginate evenly to prepare a spinning solution. (2) The spinning solution was extruded into the coagulation bath by an injection pump to obtain the formed hydrogel fiber. The hydrogel fiber was transferred to the replacement solution to replace the water in the hydrogel fiber. Then it was frozen and dried to obtain bacterial cellulose-calcium alginate aerogel fiber. (3) The short fibers and bacterial cellulose-calcium alginate aerogel fibers are blended by friction spinning process to obtain composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers. In step (1), the mass concentration of the bacterial cellulose suspension is 0.5-5.0%, and the mass ratio of the solid content of bacterial cellulose to sodium alginate is 0.2-5:

1. The solution used in the coagulation bath in step (2) is calcium chloride solution, and the replacement solution is an aqueous solution of ethanol, tert-butanol or propanol.

2. A process for the preparation of a short fiber and bacterial cellulose- calcium alginate aerogel fiber composite yarn according to claim 1, characterized in that, The mass concentration of calcium chloride solution is 1-10%, and the volume concentration of aqueous solutions of ethanol, tert-butanol, or propanol is 5-50%.

3. A process for the preparation of a short fiber and bacterial cellulose- calcium alginate aerogel fiber composite yarn as claimed in claim 1, wherein, In step (2), the injection rate of the syringe pump is 50~300 mL / h.

4. A process for the preparation of a short fiber and bacterial cellulose- calcium alginate aerogel fiber composite yarn as claimed in claim 1, wherein, In step (2), the freezing method is liquid nitrogen freezing or refrigerator freezing, and the freezing temperature is -196℃ to -20℃.

5. A process for the preparation of a short fiber and bacterial cellulose- calcium alginate aerogel fiber composite yarn as claimed in claim 1, wherein, The composite yarn obtained by friction spinning in step (3) is a core-spun yarn with short fibers coated with bacterial cellulose-calcium alginate aerogel fibers.

6. The method for preparing a composite yarn of short fibers and bacterial cellulose-calcium alginate aerogel fibers according to claim 1, characterized in that, The short fibers used in the friction spinning in step (3) are at least one of cotton fiber, viscose fiber, polyester fiber, nylon fiber, and aramid fiber.

Citation Information

Patent Citations

  • Bacterial cellulose / sodium alginate composite fiber and preparation method thereof

    CN101613893A

  • Moist antibacterial hydrogel dressing for curing diabetic foot ulcer

    CN103041438A